A network polymer organic electrode material based on phenazine derivatives and its preparation method and application

By designing net-p-PZ, a network polymer organic electrode material based on phenazine derivatives, the problems of environmental pollution and low conductivity of traditional lithium-ion battery materials have been solved, achieving higher battery stability and capacity, and improving The cycle life of the battery.

CN115850696BActive Publication Date: 2024-10-01HANGZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211413428.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-10-01
Estimated Expiration
2042-11-11

AI Technical Summary

Technical Problem

The manufacturing and recycling of inorganic electrode materials for traditional lithium-ion batteries releases large amounts of CO2 and has problems with toxic heavy metal pollution. At the same time, the low electronic conductivity and capacity fading issues of organic electrode materials limit their applications.

Method used

A network polymer organic electrode material net-p-PZ is designed based on phenazine derivatives. Through the synthesis process, a two-dimensional network structure is formed, which improves the polymerization degree and packing density of the material and inhibits the material from dissolving in the electrolyte. The dissolution enhances the stability and theoretical capacity of the battery.

Benefits of technology

It improves the stability and theoretical capacity of the battery, solves the problem of disordered accumulation, increases the specific surface area of ​​the material and the migration ability of electrolyte ions, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115850696B_ABST
    Figure CN115850696B_ABST
Patent Text Reader

Abstract

The present invention discloses a network polymer organic electrode material based on phenazine derivatives, and a preparation method and application thereof. The organic electrode material net-p-PZ uses dihydrophenazine and N,N'-diphenyl-5,10-dihydrophenazine as active centers and bridging groups at the same time to form a network polymer that radiates outward copolymerization with N,N'-diphenyl-5,10-dihydrophenazine as the center. The net-p-PZ network polymer has excellent thermal stability, is not easily soluble in electrolyte, and the network structure is conducive to ion transmission and electrolyte infiltration. As an organic positive electrode material, it has relatively excellent electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic electrode materials, and in particular to a network polymer organic electrode material based on phenazine derivatives, and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are the main energy storage devices for portable electronic products and the main power source for electric vehicles and smart grids. However, traditional lithium-ion batteries are composed of inorganic electrode materials, such as LiCoO2, and graphite, and their manufacture and recycling release a large amount of CO2 and require a lot of energy consumption. In addition, toxic heavy metals (such as Co) in inorganic cathodes can cause serious environmental pollution. Therefore, in order to circumvent the negative impact on the environment, it is very important to find green and sustainable materials as alternatives to inorganic electrode materials in rechargeable batteries. Organic electrode materials have become promising candidates for green and sustainable lithium-ion batteries due to their low cost, abundant resources, environmental friendliness, high sustainability, and recyclability of organic compounds. To date, organic electrode materials have been applied to various rechargeable batteries, including non-aqueous lithium-ion, sodium-ion, potassium-ion, dual-ion batteries, multivalent metal batteries, aqueous batteries, all-solid-state batteries, redox flow batteries, and can be used under extreme conditions such as high temperature, low temperature, high pH, ​​low pH, and atmosphere (with / without O2). Despite the great success of organic electrode materials, organic batteries still face two major challenges: (1) low electronic conductivity limits the reaction kinetics of organic batteries; (2) organic electrode materials in electrolytes cause rapid capacity decay.

[0003] A network polymer refers to a macromolecule with a three-dimensional network structure formed by chemical bonds between molecular chains, which is the so-called cross-linked structure. Since the network polymer chains are connected by chemical bonds, it has the characteristics of being insoluble and infusible. Network polymers are generally thermosetting polymers, which will not soften when heated due to strong covalent cross-linking. Thermosetting polymers are usually harder and stronger than thermoplastics, and have better dimensional stability. Using a network conductive polymer as an electrode material can effectively prevent it from dissolving in the electrolyte, which is beneficial to improving the cycle stability and life of the battery.

[0004] Chinese patent CN113979957A discloses a self-crosslinked cross-shaped organic positive electrode material and its preparation method and application, and provides the following phenazine derivatives as positive electrode materials for metal ion batteries, wherein R1 to R12 are the same or different from each other and are independently selected from -H, -CN, -F, -Cl, -Br, -CH3, -Et, -nPr, -iPr, -nBu, -tBu, -OMe, -OEt, -OiPr, -OtBu, -Ph, -Tol and -PhOMe. The molecular material structure is still a one-dimensional chain material, and does not involve the special properties of the molecular structure extending to a two-dimensional structure, so it still has the disadvantage of partially disordered stacking.

[0005] Summary of the invention

[0006] Based on the challenges and design concepts faced by the above organic electrode materials, the first object of the present invention is to provide a network polymer organic electrode material based on phenazine derivatives through reasonable structural design.

[0007] A network polymer organic electrode material net-p-PZ based on phenazine derivatives has the following general structural formula:

[0008]

[0009] Wherein, m is an integer greater than or equal to 1, and n is an integer greater than or equal to 1.

[0010] Since small molecule organic matter is easily dissolved in the organic solvent of the electrolyte and shuttles inside the battery, it will not only cause the battery capacity to decay, but also easily cause a short circuit inside the battery. By polymerizing small molecules to form a network polymer with a larger molecular weight, the dissolution of organic materials in organic solvents can be better inhibited. Therefore, the degree of polymerization m+n of the polymer electrode material net-p-PZ proposed in the present invention is greater than or equal to 2 to ensure that the electrode material is not easily dissolved in the electrolyte.

[0011] The second object of the present invention is to provide a method for preparing the network polymer organic electrode material net-p-PZ based on phenazine derivatives, the specific steps are as follows:

[0012] Step (1), Synthesis of 5,10-dihydrophenazine

[0013] The phenazine is placed in a reaction container, ethanol is added, and oxygen is removed by three freeze-pump-thaw cycles; deionized water is added to the sodium dithionite, and the solution is stirred and ultrasonicated to dissolve the solution; the sodium dithionite solution obtained after the solution is added to the reaction container, refluxed and condensed at 75-85° C. and stirred for 3-4 hours; after cooling to room temperature, the product is filtered and washed with ethanol and deionized water respectively, and dried in a vacuum to obtain a fresh light yellow solid product 5,10-dihydrophenazine;

[0014] Preferably, the mass ratio of phenazine to sodium dithionite is 1:10-12.

[0015] Step (2), Synthesis of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline

[0016] Put p-bromoaniline, tris(dibenzylideneacetone)dipalladium(0), sodium tert-butoxide, and 2-dicyclohexylphosphino-2′,6′-dimethoxybiphenyl into a reaction container, add toluene, and remove oxygen through three freeze-pump-thaw cycles; add 4-bromo-2-fluoro-1-iodobenzene into the reaction flask at room temperature, heat to 50-60° C., stir for 20-30 hours, and then cool to room temperature to obtain a crude product; purify the crude product through column chromatography to obtain the product 4-bromo-N-(4-bromophenyl)-2-fluoroaniline.

[0017] Preferably, the molar ratio of p-bromoaniline, tris(dibenzylideneacetone)dipalladium(0) and 2-dicyclohexylphosphino-2′,6′-dimethoxybiphenyl is 30-50:1:2.

[0018] Preferably, the molar ratio of p-bromoaniline to sodium tert-butoxide is 6:7-9.

[0019] Preferably, the molar ratio of p-bromoaniline to 4-bromo-2-fluoro-1-iodobenzene is 1.5 to 2:1.

[0020] Step (3), Synthesis of 2,7-dibromo-5,10-bis(4-bromophenyl)-5,10-dihydrophenazine (Br4-DPPZ)

[0021] Under an ice bath at 0°C, add the ethylmagnesium bromide solution to the ether solution of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline obtained in step (2); after stirring at 20-35°C for 10-15 minutes, remove the solvent in vacuo to obtain a magnesium amide solid. Add FeCl2, 1,2-dibromoethane and toluene to the prepared magnesium amide solid, heat to 100-110°C, stir for 10-18 hours, and then cool to room temperature. Extract with DCM and remove the solvent by vacuum rotary evaporation to obtain a crude product, which is recrystallized in a mixed solvent of dichloromethane (DCM) and methanol to obtain a pure product, Br4-DPPZ.

[0022] Preferably, the molar ratio of ethylmagnesium bromide to 4-bromo-N-(4-bromophenyl)-2-fluoroaniline is 1:9-10.

[0023] Preferably, the molar ratio of magnesium amide, FeCl2 and 1,2-dibromoethane is 1:1:37-45.

[0024] Step (4), Synthesis of Network Polymer Net-p-PZ

[0025] The 5,10-dihydrophenazine obtained in step (1), Br4-DPPZ obtained in step (3) and sodium tert-butoxide are degassed and deoxygenated in anhydrous xylene to obtain solution A; palladium acetate and 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl are degassed and deoxygenated in anhydrous xylene, and stirred at room temperature for 5 to 10 minutes to obtain solution B;

[0026] Solution B was added to solution A, and after three freeze-pump-thaw cycles to remove oxygen, a mixed system III was obtained. In a nitrogen atmosphere, the mixture was first stirred at 110-120°C for 18-24 hours, then heated to 130-140°C and stirred for 10-12 hours, bromobenzene was added for end-capping reaction for 4-6 hours, and then cooled to room temperature to obtain a crude product;

[0027] The crude product was filtered and washed with a large amount of hot o-xylene, DCM, methanol MeOH and H2O; the crude product was dispersed in DCM by mortar and ultrasound, then filtered and washed with DCM, THF, Et3N, MeOH and H2O; after repeated washing, the crude product was purified under vacuum conditions at 330-360°C for 10-15h to remove small molecular weight products, to obtain a brown-black solid, i.e., the network polymer net-p-PZ.

[0028] Preferably, the molar ratio of 5,10-dihydrophenazine, Br4-DPPZ and sodium tert-butoxide is 1:1:2.5-3.

[0029] Preferably, the molar ratio of 5,10-dihydrophenazine to 2-dicyclohexylphosphino-2',4',6'-triisopropylbiphenyl is 20-30:1.

[0030] Preferably, the molar ratio of palladium acetate to 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl is 1:2 to 2.5.

[0031] The third object of the present invention is to provide a battery positive electrode containing the above-mentioned organic positive electrode material, including positive electrode active material net-p-PZ, a conductive agent, and a binder.

[0032] The active material net-p-PZ, conductive agent and binder are prepared in a certain mass ratio (6-9: 0.5-3: 0.5-3), and the solvent N,N-dimethylpyrrolidone solvent (NMP) is added and mixed evenly, coated on the positive electrode collector and dried. After drying, the electrode sheets are cut into suitable sizes to form the net-p-PZ positive electrode sheets.

[0033] Preferably, the slurry layer thickness of the net-p-PZ positive electrode sheet is 50-100 um.

[0034] The fourth object of the present invention is to provide a metal ion battery using the above-mentioned battery positive electrode, which is composed of a positive electrode, a negative electrode, a current collector, a separator and an electrolyte.

[0035] Preferably, the metal ion battery includes a lithium ion battery and a sodium ion battery.

[0036] The negative electrode includes but is not limited to lithium metal, sodium metal, graphite, etc.

[0037] The electrolyte solution includes an organic solvent and an electrolyte salt.

[0038] Preferably, the organic solvent may be one or a combination of ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), propylene carbonate (PC), ethylene glycol dimethyl ether (DME), fluoroethylene carbonate (FEC), hydrofluoroether (HFE), and fluoroethyl methyl carbonate (FEMC); the electrolyte salt includes but is not limited to lithium hexafluorophosphate, lithium bistrifluoromethanesulfonyl imide, lithium difluorooxalatoborate, and the like.

[0039] The diaphragm can be a Celgard 2500 diaphragm, a glass fiber diaphragm, or the like.

[0040] The beneficial effects of the present invention are as follows:

[0041] From the perspective of molecular structure design, the present invention proposes to use tetrabromodiphenylphenazine with 4 active sites and dihydrophenazine with 2 active sites as monomers to form a two-dimensional network molecular structure through a polymerization reaction method. The two-dimensional network structure is conducive to the formation of graphene-like layered stacking of molecules, which is conducive to the transmission, insertion and removal of anions and cations in electrodes. Thereby improving the stability, stacking density and theoretical capacity of the battery, and solving the problem of disordered stacking.

[0042] The present invention proposes to use dihydrophenazine and N,N'-diphenyl-5,10-dihydrophenazine as both active centers and bridging groups to form a network polymer with N,N'-diphenyl-5,10-dihydrophenazine as the center and radiating outward copolymerization. On the one hand, the theoretical specific capacity of the material is increased by reducing the molecular weight corresponding to a single active center, and on the other hand, the dissolution of the material in the electrolyte is inhibited by the network-like polymer structure, and the gaps formed by the network structure are conducive to increasing the specific surface area of ​​the material, improving the wettability of the electrode material with the electrolyte and the migration of electrolyte ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is the synthetic route of net-p-PZ.

[0044] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline.

[0045] Figure 3 This is the H NMR spectrum of Br4-DPPZ.

[0046] Figure 4 This is the MALDI-TOF mass spectrum of Br4-DPPZ.

[0047] Figure 5 It is the TGA graph of the network polymer net-p-PZ.

[0048] Figure 6 It is the DSC graph of the network polymer net-p-PZ.

[0049] Figure 7 This is the charge and discharge curve of a lithium-ion battery based on a net-p-PZ positive electrode at 1C.

[0050] Figure 8 This is the charge and discharge cycle diagram of a lithium-ion battery based on a net-p-PZ positive electrode at 1C. DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further explained below through specific embodiments.

[0052] The present invention provides a method for preparing a network polymer organic electrode material net-p-PZ based on phenazine derivatives, and the specific implementation scheme is as follows:

[0053] Step (1), Synthesis of 5,10-dihydrophenazine

[0054] 2.48 g of phenazine is placed in a reaction container, ethanol is added, and oxygen is removed by three freeze-pump-thaw cycles; deionized water is added to 24.8-29.76 g of sodium dithionite, and the mixture is stirred and ultrasonically dissolved; the sodium dithionite solution obtained after the dissolution is added to the reaction container, refluxed and condensed at 75-85° C. and stirred for 3-4 hours; after cooling to room temperature, the product is filtered and washed with ethanol and deionized water respectively, and dried in a vacuum to obtain a fresh light yellow solid product 5,10-dihydrophenazine;

[0055] Step (2), synthesis of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline

[0056] 30 mmol of p-bromoaniline, 0.6-1 mmol of tris(dibenzylideneacetone)dipalladium(0), 35-45 mmol of sodium tert-butoxide, and 1,2-2 mmol of 2-dicyclohexylphosphino-2′,6′-dimethoxybiphenyl are placed in a reaction container, toluene is added, and oxygen is removed by three freeze-pump-thaw cycles; at room temperature, 15-20 mmol of 4-bromo-2-fluoro-1-iodobenzene is added to the reaction flask, the temperature is raised to 50-60° C., stirred for 20-30 hours, and then cooled to room temperature to obtain a crude product; the crude product is purified by column chromatography to obtain the product 4-bromo-N-(4-bromophenyl)-2-fluoroaniline.

[0057] Step (3), synthesis of 2,7-dibromo-5,10-bis(4-bromophenyl)-5,10-dihydrophenazine (Br4-DPPZ)

[0058] Under an ice bath at 0°C, add 2.97 mmol of ethylmagnesium bromide solution to 26.73-29.7 mmol of ether solution of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline obtained in step (2); after stirring at 20-35°C for 10-15 minutes, remove the solvent in vacuo to obtain a magnesium amide solid. Add FeCl2, 1,2-dibromoethane and toluene to the prepared magnesium amide solid, heat to 100-110°C, stir for 10-18 hours, and then cool to room temperature. Extract with DCM and remove the solvent by vacuum rotary evaporation to obtain a crude product, which is recrystallized in a mixed solvent of dichloromethane DCM and methanol to obtain a pure product Br4-DPPZ; the molar ratio of the magnesium amide, FeCl2 and 1,2-dibromoethane is 1:1:37-45.

[0059] Step (4), synthesis of network polymer net-p-PZ

[0060] 1 mmol of 5,10-dihydrophenazine obtained in step (1), 1 mmol of Br4-DPPZ obtained in step (3) and 2.5-3 mmol of sodium tert-butoxide are degassed and deoxygenated in anhydrous xylene to obtain solution A; 10 mol% of palladium acetate and 20-25 mol% of 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl are degassed and deoxygenated in anhydrous xylene, and stirred at room temperature for 5-10 minutes to obtain solution B;

[0061] Solution B was added to solution A, and after three freeze-pump-thaw cycles to remove oxygen, a mixed system III was obtained. In a nitrogen atmosphere, the mixture was first stirred at 110-120°C for 18-24 hours, then heated to 130-140°C and stirred for 10-12 hours, bromobenzene was added for end-capping reaction for 4-6 hours, and then cooled to room temperature to obtain a crude product;

[0062] The crude product was filtered and washed with a large amount of hot o-xylene, DCM, methanol MeOH and H2O; the crude product was dispersed in DCM by mortar and ultrasound, then filtered and washed with DCM, THF, Et3N, MeOH and H2O; after repeated washing, the crude product was purified under vacuum conditions at 330-360°C for 10-15h to remove small molecular weight products, to obtain a brown-black solid, i.e., the network polymer net-p-PZ.

[0063] The present invention provides a battery positive electrode containing the above-mentioned organic positive electrode material. During preparation, the active material net-p-PZ, the conductive agent and the binder are added with a mass ratio of 6-9:0.5-3:0.5-3, and the solvent N,N-dimethylpyrrolidone solvent (NMP) is evenly mixed, coated on the positive electrode collector and dried, and after drying, cut into electrode sheets of suitable size to obtain the net-p-PZ positive electrode sheet; the slurry layer thickness of the net-p-PZ positive electrode sheet is 50-100um.

[0064] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0065] Example 1: Synthesis of net-p-PZ cathode material and its application in lithium-ion batteries

[0066] The synthesis of net-p-PZ includes the following steps. The synthesis flow chart is shown in Figure 1 :

[0067] (1) Synthesis of 5,10-dihydrophenazine

[0068] Phenazine (2.48 g, 13.8 mmol) was placed in a 250 mL three-necked flask, and ethanol (30 mL) was added and oxygen was removed by three freeze pump-thaw cycles. Sodium dithionite (24.8 g, 142 mmol) was added to a beaker, and deionized water (100 mL) was added, and it was dissolved by stirring and ultrasonication, and the dissolved sodium dithionite solution was added to the reaction flask. The reaction mixture was refluxed and stirred at 80 ° C for 3.5 hours. After cooling to room temperature, it was filtered and washed with ethanol and deionized water (20 mL x 3) respectively, and the fresh light yellow solid was dried in a vacuum (2.2 g, 90% yield). Due to its instability in air, it was directly used in the next step.

[0069] (2) Synthesis of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline

[0070] Place p-bromoaniline (5.16 g, 30 mmol), tris(dibenzylideneacetone)dipalladium(0) (550 mg, 0.6 mmol), sodium tert-butoxide (3.36 g, 35 mmol), and 2-dicyclohexylphosphino-2′,6′-dimethoxybiphenyl (493 mg, 1.2 mmol) in a 250 mL three-necked flask, add toluene (40 mL), and remove oxygen by three freeze pump-thaw cycles. At room temperature, add 4-bromo-2-fluoro-1-iodobenzene (5.99 g, 20 mmol) to the reaction flask, heat to 50°C, stir for 23 hours, and then cool to 25°C. The crude product is purified by column chromatography on neutral alumina (PE / DCM=20:1-10:1) to obtain a compound, namely 4-bromo-N-(4-bromophenyl)-2-fluoroaniline.

[0071] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline, which can confirm the synthesis of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline.

[0072] (3) Synthesis of 2,7-dibromo-5,10-bis(4-bromophenyl)-5,10-dihydrophenazine (Br4-DPPZ)

[0073] Under 0 ℃ ice bath, ethyl magnesium bromide solution (1mL, 2.97M, 2.97mmol) was added to ether solution (1.0mL) of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline (1.01g, 29.1mmol). After stirring the mixture at 25 ℃ for 10 minutes, the solvent was removed in vacuo to obtain magnesium amide. FeCl2 (20mg, 0.16mmol), 1,2-dibromoethane (1.11g, 5.93mmol) and toluene (10mL) were added to the prepared magnesium amide solid, the temperature was raised to 100 ℃, stirred for 12h, and then cooled to 25 ℃. After extraction with DCM and vacuum rotary evaporation to remove the solvent, the crude product was recrystallized in a mixed solvent of DCM and methanol to obtain the pure product Br4-DPPZ.

[0074] Figure 3 This is the H NMR spectrum of Br4-DPPZ. Figure 4 This is the MALDI-TOF mass spectrum of Br4-DPPZ. Combining the H NMR spectrum and the mass spectrum, it can be confirmed that Br4-DPPZ is synthesized.

[0075] Figure 5 is the TGA graph of the network polymer net-p-PZ, Figure 6 This is the DSC graph of the network polymer net-p-PZ. Thermal analysis shows that the net-p-PZ polymer has no thermal decomposition and phase transition in the range of 0 to 300°C and has excellent thermal stability.

[0076] (4) Synthesis of network polymer net-p-PZ

[0077] Monomer 5,10-dihydrophenazine (182 mg, 1 mmol), Br4-DPPZ (650 mg, 1 mmol) and sodium tert-butoxide (360 mg, 2.5 mmol) were degassed and deoxygenated in anhydrous xylene (25 mL) to obtain solution A; palladium acetate (22 mg, 10 mol%) and 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl (48 mg, 20 mol%) were degassed and deoxygenated in anhydrous xylene (15 mL) and stirred at room temperature for 5 minutes to obtain solution B. Solution B was added to solution A, and after three freeze-pump-thaw cycles to remove oxygen, a mixed system III was obtained. Mixed system III was stirred at 120°C for 24 hours under a nitrogen atmosphere, and then stirred at 140°C for 12 hours, and 0.5 mL of bromobenzene was added to the reaction solution for a capping reaction for 5 hours. After the reaction solution was cooled to room temperature, the mixture was filtered and the solid part (crude product) was washed with a large amount of hot o-xylene, dichloromethane (DCM), methanol (MeOH) and H2O. The solubility of p-PZ is poor, and the product is dispersed in DCM by mortar and ultrasound, and then filtered and washed by DCM, THF, Et3N, MeOH and H2O. After repeating this process five times, the product was purified by a physical vapor deposition (PVD) instrument at 350°C and vacuum for 12h to remove small molecular weight products, and a brown-black solid was obtained, namely the network polymer net-p-PZ.

[0078] net-p-PZ's lithium-ion battery applications include the following:

[0079] The synthesized net-p-PZ material, Super P and polyvinylidene fluoride were mixed in N-methyl-2-pyrrolidone (anhydrous) at a weight ratio of 7:2:1, and the mixture was fully stirred in a centrifugal mixer for 30 minutes until a uniform slurry was formed. The slurry was then cast on aluminum foil with a thickness of 100 μm, dried in a vacuum at 60°C for 12 hours, and sliced ​​into 10 mm discs as the positive electrode of the battery.

[0080] A lithium-ion battery was assembled with a net-p-PZ positive electrode, lithium metal as the negative electrode, a Celgard 2500 separator and a 1M LiTFSI solution with EC / DEC=1 / 1 as the electrolyte, and its electrochemical performance was tested.

[0081] Figure 7 The charge and discharge curve of a lithium-ion battery based on a net-p-PZ positive electrode at 1C. The battery has a higher charge and discharge voltage (3.3~4.3V vs Li + / Li).

[0082] Figure 8It is the charge and discharge cycle diagram of the lithium-ion battery based on the net-p-PZ positive electrode at 1C. The battery shows excellent coulombic efficiency (always close to 100%) and good cycle stability.

[0083] Example 2: Synthesis of net-p-PZ cathode material and its application in lithium-ion batteries

[0084] The net-p-PZ material was synthesized according to the net-p-PZ synthesis method described in Example 1.

[0085] The synthesized net-p-PZ material, Super P and polyvinylidene fluoride were mixed in N-methyl-2-pyrrolidone (anhydrous) at a weight ratio of 7:2:1, and the mixture was fully stirred in a centrifugal mixer for 30 minutes until a uniform slurry was formed. The slurry was then cast on aluminum foil with a thickness of 50 μm, dried in a vacuum at 60°C for 12 hours, and sliced ​​into 10 mm discs, which were net-p-PZ positive electrodes.

[0086] A lithium-ion battery was assembled using a net-p-PZ positive electrode, lithium metal as the negative electrode, a Celgard 2500 separator and a 1M LiTFSI solution with EC / DEC=1 / 1 as the electrolyte.

[0087] Example 3: Synthesis of net-p-PZ cathode material and its application in sodium ion batteries

[0088] The net-p-PZ material was synthesized according to the net-p-PZ synthesis method described in Example 1.

[0089] The synthesized net-p-PZ material, Super P and polyvinylidene fluoride were mixed in N-methyl-2-pyrrolidone (anhydrous) at a weight ratio of 7:2:1, and the mixture was fully stirred in a centrifugal mixer for 30 minutes until a uniform slurry was formed. The slurry was then cast on aluminum foil with a thickness of 50 μm, dried in a vacuum at 60°C for 12 hours, and sliced ​​into 10 mm discs, which were net-p-PZ positive electrodes.

[0090] The net-p-PZ positive electrode, lithium metal as the negative electrode, glass fiber membrane as the separator, and 1M NaClO4 EC / DEC=1 / 1 solution as the electrolyte were assembled into a sodium ion battery.

[0091] Example 4: Synthesis of net-p-PZ cathode material and its application in sodium ion batteries

[0092] The net-p-PZ material was synthesized according to the net-p-PZ synthesis method described in Example 1.

[0093] The synthesized net-p-PZ material, Super P and polyvinylidene fluoride were mixed in N-methyl-2-pyrrolidone (anhydrous) at a weight ratio of 7:2:1, and the mixture was fully stirred in a centrifugal mixer for 30 minutes until a uniform slurry was formed. The slurry was then cast on aluminum foil with a thickness of 100 μm, dried in a vacuum at 60°C for 12 hours, and sliced ​​into 10 mm discs, which were net-p-PZ positive electrodes.

[0094] The net-p-PZ positive electrode, lithium metal as the negative electrode, glass fiber membrane as the separator, and 1M NaClO4 EC / DEC=1 / 1 solution as the electrolyte were assembled into a sodium ion battery.

[0095] It will be apparent to those skilled in the art that various changes may be made to the disclosed embodiments. In addition, the general principles defined in the present invention may be applied to other embodiments and application scenarios without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the disclosed embodiments, but should be given the broadest scope consistent with the scope of the invention patent.

Claims

1. A network polymer organic electrode material net-p-PZ based on phenazine derivatives, characterized in that: The general structure is as follows: Wherein, m is an integer greater than or equal to 1, and n is an integer greater than or equal to 1.

2. A method for preparing the network polymer organic electrode material net-p-PZ based on phenazine derivatives as claimed in claim 1, characterized in that: The steps include: Step (1), Synthesis of 5,10-dihydrophenazine The phenazine is placed in a reaction container, ethanol is added, and oxygen is removed by three freeze-pump-thaw cycles; deionized water is added to the sodium dithionite, and the solution is stirred and ultrasonicated to dissolve the solution; the sodium dithionite solution obtained after the solution is added to the reaction container, refluxed and condensed at 75-85° C. and stirred for 3-4 hours; after cooling to room temperature, the product is filtered and washed with ethanol and deionized water respectively, and dried in a vacuum to obtain a solid product 5,10-dihydrophenazine; Step (2), Synthesis of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline Putting p-bromoaniline, tris(dibenzylideneacetone)dipalladium(0), sodium tert-butoxide, and 2-dicyclohexylphosphino-2′,6′-dimethoxybiphenyl into a reaction container, adding toluene, and removing oxygen through three freeze pump-thaw cycles; adding 4-bromo-2-fluoro-1-iodobenzene into the reaction flask at room temperature, heating to 50-60° C., stirring for 20-30 hours, and then cooling to room temperature to obtain a crude product; purifying the crude product by column chromatography to obtain the product 4-bromo-N-(4-bromophenyl)-2-fluoroaniline; Step (3), Synthesis of 2,7-dibromo-5,10-bis(4-bromophenyl)-5,10-dihydrophenazine Br4-DPPZ Under an ice bath at 0°C, add ethylmagnesium bromide solution to the ether solution of 4-bromo-N-(4-bromophenyl)-2-fluoroaniline obtained in step (2); after stirring at 20-35°C for 10-20 minutes, remove the solvent in vacuo to obtain amide magnesium solid; add FeCl2, 1,2-dibromoethane and toluene to the prepared amide magnesium solid, raise the temperature to 100-110°C, stir for 10-18 hours, and then cool to room temperature; extract with DCM and remove the solvent by vacuum rotary evaporation to obtain a crude product, and recrystallize the crude product in a mixed solvent of dichloromethane (DCM) and methanol to obtain a pure product Br4-DPPZ; Step (4), Synthesis of Network Polymer Net-p-PZ The 5,10-dihydrophenazine obtained in step (1), Br4-DPPZ obtained in step (3) and sodium tert-butoxide are degassed and deoxygenated in anhydrous xylene to obtain solution A; palladium acetate and 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl are degassed and deoxygenated in anhydrous xylene, and stirred at room temperature for 5 to 10 minutes to obtain solution B; Solution B was added to solution A, and after three freeze-pump-thaw cycles to remove oxygen, a mixed system III was obtained. In a nitrogen atmosphere, the mixture was first stirred at 110-120°C for 18-24 hours, then heated to 130-140°C and stirred for 10-12 hours, bromobenzene was added for end-capping reaction for 4-6 hours, and then cooled to room temperature to obtain a crude product; The crude product was filtered and washed with hot o-xylene, DCM, methanol MeOH and H2O; the crude product was dispersed in DCM by mortar and ultrasound, then filtered and washed with DCM, THF, Et3N, MeOH and H2O; after repeated washing, the washed crude product was purified under vacuum conditions at 330-360°C for 10-15h to remove small molecular weight products to obtain a network polymer net-p-PZ.

3. The method according to claim 2, characterized in that In step (1), the mass ratio of phenazine to sodium dithionite is 1:10-12.

4. The method according to claim 2, characterized in that: In step (2), the molar ratio of p-bromoaniline, tris(dibenzylideneacetone)dipalladium(0) and 2-dicyclohexylphosphino-2′,6′-dimethoxybiphenyl is 30-50:1:2; the molar ratio of p-bromoaniline and sodium tert-butoxide is 6:7-9; and the molar ratio of p-bromoaniline and 4-bromo-2-fluoro-1-iodobenzene is 1.5-2:

1.

5. The method according to claim 2, characterized in that: In step (3), the molar ratio of ethylmagnesium bromide to 4-bromo-N-(4-bromophenyl)-2-fluoroaniline is 1:9-10; the molar ratio of magnesium amide, FeCl2 and 1,2-dibromoethane is 1:1:37-45.

6. The method according to claim 2, characterized in that In step (4), the molar ratio of 5,10-dihydrophenazine, Br4-DPPZ and sodium tert-butoxide is 1:1:2.5-3; the molar ratio of 5,10-dihydrophenazine and 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl is 20-30:1; and the molar ratio of palladium acetate and 2-dicyclohexylphosphine-2',4',6'-triisopropylbiphenyl is 1:2-2.

5.

7. A positive electrode of a battery, characterized in that: The battery positive electrode comprises the phenazine derivative-based network polymer organic electrode material according to claim 1, a conductive agent and a binder.

8. A battery positive electrode according to claim 7, characterized in that The mass ratio of the network polymer organic electrode material based on phenazine derivatives, the conductive agent and the binder is 6-9:0.5-3:0.5-3.

9. A metal ion battery, characterized in that A battery positive electrode as claimed in claim 7 or 8 is used.

10. A metal ion battery according to claim 9, characterized in that The metal ion battery is a lithium ion battery or a sodium ion battery.