A densely packed nano-diamond film and preparation method thereof
By combining spin-coating seeding with a hot-wire chemical vapor deposition system, a densely packed nanodiamond film with high carrier mobility and controllable microstructure was prepared, solving the problems of low carrier mobility and poor reproducibility of n-type nanodiamond films.
Patent Information
- Application Number
- CN202211549878.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-05
AI Technical Summary
In the existing technology, n-type nanodiamond films have low carrier mobility, and traditional seeding methods have low repeatability, making it difficult to control the film microstructure.
A spin-coating seeding process was used to suspend nanodiamond powder of different particle sizes onto a single-crystal silicon wafer, and a densely packed nanodiamond film with low amorphous carbon grain boundary content was prepared by a hot-wire chemical vapor deposition system.
It achieves improved carrier mobility, enhanced controllability of thin film microstructure, significantly reduced amorphous carbon grain boundary content, and high growth repeatability.
Smart Images

Figure HDA0003980553620000011 
Figure HDA0003980553620000012 
Figure HDA0003980553620000021
Abstract
Description
(I) Technical field
[0001] The invention relates to a densely packed nano diamond film and a preparation method thereof. (II) Background technology
[0002] The band gap of diamond is 5.5eV, and the thermal conductivity is as high as 22W / (cm·K), which is much higher than the third-generation semiconductor materials SiC and GaN. Therefore, diamond has extremely important application prospects in the field of high-frequency and high-power electronic devices.
[0003] At present, p-type diamond films obtained by doping diamond with boron by chemical vapor deposition or ion implantation have been applied in wastewater treatment, medical treatment and other fields, while n-type doping of diamond is still a difficult problem to be solved in order to realize its application in the semiconductor field. Nanodiamond films have good n-type doping potential due to their unique structure of nanocrystalline grains and amorphous carbon phases; in our authorized patents ZL201210594869.4 and ZL201510219422.2, n-type nanodiamond films with high mobility are obtained by implanting phosphorus ions or oxygen ions into the films; however, the amorphous carbon phase is a disordered structure, and the large amount of amorphous carbon phases in the grain boundaries of nanodiamond films have a significant effect on carrier scattering, which makes the carrier mobility of traditional n-type nanodiamond films still low. In the patents CN 108660429 B and CN108660432B we applied for, a seeding method combining manual grinding and ultrasonic vibration was used to adjust the chemical vapor deposition process to prepare a diamond film with dense packing of nano-grains. Interfaces were formed between the grains in the film, the content of amorphous carbon grain boundaries was significantly reduced, and the n-type conductivity was good. In this patent, seeding determines the nucleation rate of the film, which is extremely important for obtaining a densely packed structure. The seeding method combining manual grinding and ultrasonic vibration used previously has problems such as large human errors, low growth repeatability, and difficulty in controlling the microstructure of the subsequently grown film. Therefore, it is urgent to develop a new seeding method.
[0004] This patent uses single crystal silicon as the substrate and invents a spin coating seeding process to prepare a nano-diamond film with a densely packed structure through a hot wire chemical vapor deposition system. This is of great significance for achieving n-type doping of diamond. (III) Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a densely packed nano-diamond film by a spin coating seeding process, wherein nano-diamond powders of different particle sizes obtained by different preparation methods are suspended and coated on a substrate, and then a nano-diamond film with a low amorphous carbon grain boundary content and a densely packed structure is prepared by a hot wire chemical vapor deposition system.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] The present invention provides a densely packed nano-diamond film, which is prepared by the following method:
[0008] (1) Spin coating liquid preparation: diamond powder with a particle size of 3 nm-1 μm (preferably 3-50 nm), an adhesive and an active agent are uniformly dispersed in an organic solvent to obtain a spin coating liquid; the mass ratio of the diamond powder to the active agent is 100:5-10 (preferably 100:6); the volume of the organic solvent is 0.3-0.5 mL / mg (preferably 0.35-0.4 mL / mg, particularly preferably 0.38 mL / mg) based on the mass of the diamond powder; the volume ratio of the adhesive to the organic solvent is 1:20-40 (preferably 1:38); the active agent is one or a mixture of two or more of cetyltrimethylammonium bromide, polydiallyldimethylammonium chloride, glycidol, and octadecyldimethylbenzyl ammonium chloride;
[0009] (2) Spin coating seed crystals: Spin coating the spin coating solution described in step (1) on the surface of a single crystal silicon wafer, wherein the spin coating comprises 15-20 cycles (preferably 20 cycles), wherein each cycle comprises spin coating at 1000 rpm for 10 seconds and then spin coating at 3000 rpm for 30 seconds; thereby obtaining a silicon wafer having a dense seed crystal layer coated on the surface;
[0010] (3) Heat treatment: placing the silicon wafer coated with a dense seed crystal layer in step (2) in a tube furnace, and heat treating it at 500-800° C. for 8-20 min (preferably 700° C. for 10 min) in an argon protective atmosphere to obtain a heat-treated silicon wafer;
[0011] (4) Using the heat-treated silicon wafer of step (3) as a substrate and performing hot wire chemical vapor deposition with acetone as a carbon source to obtain the densely packed nano-diamond film.
[0012] Furthermore, the diamond powder in step (1) is generally nano-diamond powder, which in the embodiments of the present invention are W3 diamond powder (120000 mesh, particle size of 36nm, obtained by crushing method), N3 diamond powder (particle size of 3-5nm, purity of 98%, obtained by detonation method, containing a certain amount of graphite) or YKJ diamond powder (particle size of 200-500nm, obtained by irregular polycrystalline diamond crushing method).
[0013] Furthermore, in order to facilitate dispersion and prevent agglomeration, the adhesive and the active agent in step (1) are first dispersed in an organic solvent separately and then mixed.
[0014] Furthermore, the adhesive in step (1) is one or a mixture of two or more of polyvinyl alcohol, epoxy resin, and polyvinyl acetate. In one embodiment of the present invention, the adhesive is epoxy resin.
[0015] Furthermore, the active agent in step (1) is cetyltrimethylammonium bromide. The surfactant selected in the present invention satisfies two requirements of the technical solution at the same time: 1. It can be adsorbed on the surface of diamond particles through active agent molecules, and repel the same polarity through the same terminal groups, thereby preventing the agglomeration of nano diamond particles; 2. It has poor thermal stability and can be decomposed and volatilized in the subsequent heat treatment process.
[0016] Furthermore, the organic solvent in step (1) is one or a mixed solvent of dimethyl sulfoxide, acetone, and ethyl lactate, and in one embodiment of the present invention, it is acetone. The organic solvent selected in the present invention simultaneously meets the three requirements of the technical solution: 1. It has good compatibility with the active agent and the binder, 2. It can ensure the activity of the surfactant, and 3. It must be completely removed after the heat treatment.
[0017] Furthermore, the single crystal silicon wafer in step (2) is also pre-treated as follows before spin coating:
[0018] The pieces were cut into 20×20 mm size, ultrasonically cleaned in acetone (10 min), and dried with a nitrogen gun.
[0019] Specifically, the hot wire chemical vapor deposition in step (4) is operated as follows: the acetone is brought into the reaction chamber of the hot wire chemical vapor deposition equipment by hydrogen bubbling with a flow rate of 60-100sccm (preferably 80sccm), and pure hydrogen with a flow rate of 100-300sccm (preferably 200sccm) is also introduced, the growth power is 1800-2400W (preferably 2200W), the growth pressure is controlled to be 1.8-2.0KPa (preferably 1.8KPa), the growth time is 45-60min (preferably 60min), the substrate temperature is maintained at 600-700°C (650°C in one embodiment of the present invention), after the growth is completed, the carbon source is stopped, and the power is reduced to 0 at a rate of 1V / min in a pure hydrogen atmosphere to obtain the densely packed nanodiamond film. The obtained film has a grain size of 10-30nm, the grains are densely packed to form an interface, and the amorphous carbon content is very low.
[0020] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in: 1. The spin coating method is used to pre-treat the substrate, which is simple to operate, highly repeatable and easy to control compared to the grinding method; 2. A process is developed to obtain a densely packed nano-diamond film by suspending and coating the substrate with nano-diamond particles of various sizes and specifications; 3. The hot wire chemical vapor deposition method is used to quickly prepare nano-diamond films over a large area; 4. The nano-crystalline densely packed diamond film prepared by this process has interfaces formed between the grains and very little amorphous carbon grain boundaries. (IV) Description of the drawings
[0021] Figure 1 This is a field emission scanning electron microscope (FESEM) image of a silicon substrate after spin coating the seed crystal when the seed crystal powder in Example 1 is W3 powder (particle size is ˜36 nm, obtained by crushing method);
[0022] Figure 2 This is a field emission scanning electron microscope (FESEM) image corresponding to the prepared densely packed nanodiamond (CPND) film when the seed crystal powder is W3 powder in Example 1;
[0023] Figure 3 This is a low-magnification high-resolution transmission electron microscopy (HRTEM) image of the prepared CPND film when the seed crystal powder is W3 powder in Example 1;
[0024] Figure 4 This is a high-magnification TEM image of the CPND film sample prepared when the seed powder is W3 powder in Example 1, the FT pattern in the inset, and the FT pattern of the corresponding area on the right
[0025] Figure 5 This is a field emission scanning electron microscope (FESEM) image corresponding to the silicon substrate after spin coating the seed crystal when the seed crystal powder is YKJ (particle size is 200-500nm, obtained by crushing method) powder in Example 2;
[0026] Figure 6 This is a field emission scanning electron microscope (FESEM) image corresponding to the prepared CPND film when the seed crystal powder is YKJ powder in Example 2;
[0027] Figure 7 This is a low-magnification high-resolution transmission electron microscopy (HRTEM) image of the prepared CPND film when the seed crystal powder is YKJ powder in Example 2;
[0028] Figure 8 (a) is a high-magnification TEM image of the CPND thin film sample prepared when the seed powder is YKJ powder in Example 2, and the inset is the FT pattern of each corresponding area. (b) is an enlarged image of area a in (a).
[0029] Fig. 9This is a field emission scanning electron microscope (FESEM) image of a silicon substrate after spin coating the seed crystal when the seed crystal powder is N3 powder (particle size is 3-5 nm, prepared by detonation method) in Example 3;
[0030] Fig.10 This is a field emission scanning electron microscope (FESEM) image corresponding to the prepared CPND film when the seed crystal powder is N3 powder in Example 3;
[0031] Fig.11 This is a low-magnification high-resolution transmission electron microscopy (HRTEM) image of the prepared CPND film when the seed crystal powder is N3 powder in Example 3;
[0032] Fig.12 (a) is a high-magnification TEM image of a sample of the CPND film prepared when the seed powder is N3 powder in Example 3, and the inset is the FT pattern of the c area in (a); (b) is an enlarged image of the c area, and the right side is the FT pattern of the corresponding area of (b) (V) Specific implementation methods
[0033] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto:
[0034] Example 1
[0035] 100 mg of W3 diamond powder (120000 mesh, particle size of ~36 nm, obtained by crushing method) was mixed with 1 ml of adhesive: epoxy resin (Shanghai MacLean Biochemical Technology Co., Ltd., product number E871957) + 9 ml of acetone, and 6 mg of cetyltrimethylammonium bromide + 9 ml of acetone as an active agent and dissolved in 20 ml of acetone. The solution was then ultrasonically shaken for 60 min to form a suspension, which was kept as a spin coating liquid for later use. A single crystal silicon wafer was cut into a size of ~20×20 mm with a diamond knife, placed in acetone for ultrasonic cleaning for 10 min, and blown dry with a nitrogen gun after cleaning. The silicon wafer was placed on a spin coater (purchased from Beijing Saidekaisi Electronics Co., Ltd., model KW-4A) and spin-coated with a seed crystal spin coating liquid. The spin coating speed was 1000 rpm (10 s) + 3000 rpm (30 s), and the spin coating was repeated 20 times to coat the surface of the silicon wafer with a dense seed crystal layer.
[0036] The silicon wafer after spin coating seed crystal was placed in a tube furnace and heat treated at 700℃ in an argon protective atmosphere for 10 minutes to remove organic matter on the surface of the silicon wafer; then the silicon wafer was placed in a hot wire chemical vapor deposition device (the hot wire chemical vapor deposition device was purchased from Shanghai Jiaoyou Diamond Coating Company, model JUHFCVD001), acetone was used as the carbon source, and acetone was brought into the reaction chamber by hydrogen bubbling. The flow ratio of hydrogen and acetone was 200:80sccm, the growth power was 2200W, the growth pressure was controlled to be 1.8KPa, the growth time was 60min, the substrate temperature was maintained at about 650℃, and after the growth was completed, the power was slowly reduced to 0 at a rate of 1V / min in a hydrogen atmosphere to complete the film preparation process.
[0037] Field emission scanning electron microscopy (FESEM) was used to observe the surface morphology of the silicon wafer substrate and the deposited film after spin coating; high resolution transmission electron microscopy (HRTEM) was used to observe the microstructure composition of the deposited film samples.
[0038] Figure 1 This is a field emission electron microscope image of a silicon substrate at 5000 times magnification after spin coating of the seed crystal when the seed crystal powder is W3 powder. It can be seen that a continuous and dense seed crystal layer is formed on the surface of the silicon wafer after spin coating of the diamond powder.
[0039] Figure 2 This is a field emission electron microscope photo of the sample after film deposition at 50,000 times magnification. It can be seen that the surface is composed of nano-diamond particles, and the needle-like nano-crystals form a continuous and dense surface morphology.
[0040] Figure 3 This is a high-resolution transmission electron microscope image of the deposited film. It can be seen that the film is a structure in which irregular nano-grains are wrapped by slender and narrow grain boundaries. The diamond grains are tightly packed together, showing the characteristics of dense packing. From the interpolated SAED image, it can be seen that the main manifestations are the (111) and (220) crystal planes of diamond, and there is no diffraction information of the amorphous carbon phase, which shows that the amorphous carbon content in the grain boundaries of the film is extremely low.
[0041] Figure 4 This is a high-magnification HRTEM image of the film. The inset FT is the FT transformation pattern of the magnified area. Diffraction spots with different diamond grains can be seen, revealing that there are multiple grains densely packed together in this area. Figure 4The four regions in the figure were further analyzed, and the FT illustration on the right is the FT pattern of the corresponding region. FT1 is the diffraction pattern of region 1 of a diamond grain in the lower left corner. There are two bright diffraction spots in the pattern, and the directions are basically close to being perpendicular to each other. There is only one pair of diamond diffraction points in FT2, which is one of the two pairs of diffraction points in FT1, but it is obviously brighter than that in FT1, and the diffraction information is stronger. This shows that regions 1 and 2 are stacked with two diamond grains. FT3 is the FT pattern of region 3. It can be seen that there are also diffraction spots of diamond grains in region 2 in FT3, but there are also diffraction spots of another diamond grain, which means that region 3 is the grain boundary region between the grains in region 2 and another diamond grain. There is a larger grain in region 4, and there are three pairs of diffraction spots in FT4, but no obvious information about three grains is observed in region 4. We conducted further analysis on FT4 and found that by measuring the angles between the three diffraction points, the angle θ1=θ2=~35° is exactly the angle between the (111) and (220) crystal planes of diamond. This means that the three pairs of diffraction spots in FT4 are the diffraction information of different crystal planes of the same diamond grain, which also indirectly proves that the degree of crystallization of the diamond grain is good.
[0042] Example 2
[0043] 100 mg of N3 diamond powder (particle size of ~3-5 nm, purity of 98%, obtained by detonation method, containing a certain amount of graphite) was mixed with an adhesive: 1 ml of epoxy resin + 9 ml of acetone, and an activator: 6 mg of cetyltrimethylammonium bromide + 9 ml of acetone, and dissolved in 20 ml of acetone. The solution was then ultrasonically shaken for 60 minutes to form a suspension, which was kept as a spin coating liquid for later use; a single crystal silicon wafer was cut into a size of ~20×20 mm with a diamond knife, placed in acetone for ultrasonic cleaning for 10 minutes, and blown dry with a nitrogen gun after cleaning; the silicon wafer was placed on a spin coater (purchased from Beijing Saidekaisi Electronics Co., Ltd., model KW-4A) and spin-coated with a seed crystal spin coating liquid. The spin coating speed was 1000 rpm (10s) + 3000 rpm (30s), and the spin coating was repeated 20 times to coat the surface of the silicon wafer with a dense seed crystal layer. The silicon wafer after spin coating seed crystal was placed in a tube furnace and heat treated at 700℃ in an argon protective atmosphere for 10 minutes to remove organic matter on the surface of the silicon wafer; then the silicon wafer was placed in a hot wire chemical vapor deposition device (the hot wire chemical vapor deposition device was purchased from Shanghai Jiaoyou Diamond Coating Company, model JUHFCVD001), acetone was used as the carbon source, and acetone was brought into the reaction chamber by hydrogen bubbling. The flow ratio of hydrogen and acetone was 200:80sccm, the growth power was 2200W, the growth pressure was controlled to be 1.8KPa, the growth time was 60min, the substrate temperature was maintained at about 650℃, and after the growth was completed, the power was slowly reduced to 0 at a rate of 1V / min in a hydrogen atmosphere to complete the film preparation process.
[0044] Figure 5 This is a field emission electron microscope image of a silicon substrate at 5000 times magnification after spin coating of the seed crystal powder, when the seed crystal powder is N3 powder. It can be seen that a continuous and dense seed crystal layer is formed on the surface of the silicon wafer after spin coating of the diamond powder. Since the seed crystal powder is finer, the powder agglomerates, resulting in certain ups and downs on the surface.
[0045] Figure 6 This is a field emission electron microscope photo of the sample after film deposition at 50,000 times magnification. It can be seen that the surface is composed of nano-diamond particles, and the surface is composed of needle-like nano-crystals to form a continuous and dense surface morphology.
[0046] Figure 7 This is a high-resolution transmission electron microscope image of the deposited film. It can be seen that the film is a structure in which irregular nano-grains are wrapped by slender and narrow grain boundaries. The diamond grains are tightly packed together, showing the characteristics of dense packing. From the interpolated SAED image, it can be seen that the main manifestations are the (111), (220) and (222) crystal planes of diamond, and there is no diffraction information of the amorphous carbon phase, which shows that the amorphous carbon content in the grain boundaries of the film is extremely low.
[0047] Figure 8(a) is a high-magnification HRTEM image of the film. We further analyzed the c region in the figure. FT-c is the FT image of the c region. It can be seen that there are three pairs of bright diffraction spots in FT-c. By measuring the distance between the diffraction spots, the diffraction information of three different diamond grains can be determined. (b) The enlarged pattern of the c region in the figure. It can be clearly seen that there is an overlap of lattice fringes in Figure (b), proving that this area is a grain boundary area with densely packed diamond grains. FT patterns corresponding to three different regions S1, S2 and S3. In the S1 region, three pairs of diamond diffraction spots, two dark and one bright, can be seen, indicating that the three grains have a certain degree of dense overlap in this area. In the S2 region to the right of S1, FT-S2 shows only two pairs of diffraction spots, which happen to be the darker two pairs in FT-S1, indicating that the boundary of the grain corresponding to the bright diffraction point of S1 is located between the S1 and S2 regions. There is only one pair of diffraction spots in the S3 region at the bottom of the picture, indicating that there is only information about one diamond grain. Therefore, there are three different grains densely packed in the c region. There is a grain junction between S1 and S2, and the S2 region is where two grains are stacked and overlapped. The S3 region below mainly contains the information of another grain. The (111) stripes of the three diamond grains meet in this region, forming a densely packed grain boundary.
[0048] Example 3
[0049] 100 mg of YKJ diamond powder (with a particle size of 200 to 500 nm, obtained by crushing irregular polycrystalline diamond) was mixed with an adhesive: 1 ml of epoxy resin + 9 ml of acetone, and an active agent: 6 mg of 1 hexadecyltrimethylammonium bromide + 9 ml of acetone, and dissolved in 20 ml of acetone. The solution was then ultrasonically shaken for 60 minutes to form a suspension. A single crystal silicon wafer was cut into a size of 20×20 mm with a diamond knife, ultrasonically cleaned in acetone for 10 minutes, and dried with a nitrogen gun after cleaning. The silicon wafer was placed on a spin coater (purchased from Beijing Saidekaisi Electronics Co., Ltd., model KW-4A) and spin-coated with a seed crystal spin coating liquid. The spin coating speed was 1000 rpm (10 s) + 3000 rpm (30 s), and the spin coating was repeated 20 times to coat the surface of the silicon wafer with a dense seed crystal layer. The silicon wafer after spin coating seed crystal was placed in a tube furnace and heat treated at 700℃ in an argon protective atmosphere for 10 minutes to remove organic matter on the surface of the silicon wafer; then the silicon wafer was placed in a hot wire chemical vapor deposition device (the hot wire chemical vapor deposition device was purchased from Shanghai Jiaoyou Diamond Coating Company, model JUHFCVD001), acetone was used as the carbon source, and acetone was brought into the reaction chamber by hydrogen bubbling. The flow ratio of hydrogen and acetone was 200:80sccm, the growth power was 2200W, the growth pressure was controlled to be 1.8KPa, the growth time was 60min, the substrate temperature was maintained at about 650℃, and after the growth was completed, the power was slowly reduced to 0 at a rate of 1V / min in a hydrogen atmosphere to complete the film preparation process.
[0050] Fig. 9 This is a field emission electron microscope image of a silicon substrate at 5000 times magnification after spin coating seed crystal treatment when the seed crystal powder is YKJ powder. It can be seen that the YKJ powder forms a dense seed crystal layer on the surface of the silicon wafer and is well dispersed.
[0051] Fig.10 This is a field emission electron microscope photo of the sample after film deposition at 50,000 times magnification. It can be seen that the surface is nano-diamond particles, and the surface is composed of granular nano-crystals to form a continuous and dense surface morphology, and the particle size is less than 100nm.
[0052] Fig.11 This is a high-resolution transmission electron microscope image of the deposited film. It can be seen that the film is a structure in which irregular nano-grains are wrapped by slender and narrow grain boundaries. The diamond grains are tightly packed together, showing the characteristics of dense packing. From the interpolated SAED image, it can be seen that the main manifestations are the (111) and (220) crystal planes of diamond, and there is no diffraction information of the amorphous carbon phase.
[0053] Fig.12(a) is a high-magnification image of the film, and the illustration FT1 is the Fourier transform (FT) pattern of the corresponding area. We performed a micro-area analysis on area a in the figure, and FT-a is the FT pattern of area a. It can be seen that the pattern shows three groups of diffraction spots corresponding to the diamond (111) crystal plane, one pair of which shows obvious elongation, which means that there are more surface defects in area a; (b) is an enlarged image of area a, and it can be seen that there are obvious diamond lattice stripes in two directions stacked together. In order to further analyze its dense stacking, we performed corresponding Fourier transform analysis on the three areas S1, S2 and S3 in area a, and the corresponding FT patterns are Fig.12 (a) The three illustrations in the lower right corner. Observing the FT-S1 pattern, it can be seen that there is only one set of diffraction spots, whose direction is perpendicular to the lattice stripes in the S1 region, corresponding to the lattice stripe diffraction spots of a diamond grain in the S1 region; at the same time, the diffraction spots of FT-S1 are elongated into a line, which means that there are certain surface defects in the S1 region. When moving to the S3 region, the diffraction spots show a single two spots, with a different direction from the S1 region, corresponding to another diamond grain in the S3 region. In the grain boundary part of S2, it can be seen that the diffraction spots of S1 and S3 appear at the same time, and another pair of less obvious diffraction spots appear. This is because the S1 grains and S3 grains are densely stacked in the S2 region, and their lattice stripes are staggered. Due to their good stacking condition, a periodic repeating structure is formed, so a corresponding group of relatively dim diffraction points appear in the grain boundary region of S2. The surface defect corresponding to the elongation of the diffraction point is due to the interlacing of the lattice fringes and the accumulation of grains in the S2 region, which results in the presence of surface defects with a high density near S2 due to the interlacing. Fig.12 (b) Visually it looks like curling has occurred due to grain collision.
Claims
1. A densely packed nanodiamond film, characterized in that The densely packed nano-diamond film is prepared as follows: (1) Preparation of spin coating liquid: diamond powder with a particle size of 3nm-1μm, adhesive and active agent are uniformly dispersed in an organic solvent to obtain a spin coating liquid; the mass ratio of the diamond powder to the active agent is 100:5-10; the volume of the organic solvent is 0.3-0.5mL / mg based on the mass of the diamond powder; the volume ratio of the adhesive to the organic solvent is 1:20-40; the active agent is one or a mixture of two or more of cetyltrimethylammonium bromide, polydiallyldimethylammonium chloride, glycidol, and octadecyldimethylbenzyl ammonium chloride; (2) Spin coating seed crystals: Spin coating the spin coating solution of step (1) on the surface of a single crystal silicon wafer, wherein the spin coating comprises 15 to 20 cycles, wherein each cycle comprises spin coating at 1000 rpm for 10 seconds and then spin coating at 3000 rpm for 30 seconds; thus obtaining a silicon wafer having a dense seed crystal layer coated on the surface; (3) Heat treatment: placing the silicon wafer coated with a dense seed crystal layer in step (2) in a tube furnace, and heat treating it at 500-800° C. for 8-20 min in an argon protective atmosphere to obtain a heat-treated silicon wafer; (4) Using the heat-treated silicon wafer of step (3) as a substrate and performing hot wire chemical vapor deposition with acetone as a carbon source to obtain the densely packed nano-diamond film.
2. The densely packed nano-diamond film according to claim 1, characterized in that: The diamond powder in step (1) is nano diamond powder.
3. The densely packed nano-diamond film according to claim 2, characterized in that: The nano diamond powder is W3 diamond powder, N3 diamond powder or YKJ diamond powder.
4. The densely packed nano-diamond film according to claim 1, characterized in that: The adhesive in step (1) is one or a mixture of two or more of polyvinyl alcohol, epoxy resin, and polyvinyl acetate.
5. The densely packed nano-diamond film according to claim 3, characterized in that: The adhesive in step (1) is epoxy resin.
6. The densely packed nano-diamond film according to claim 1, characterized in that: The organic solvent in step (1) is one or a mixed solvent of two or more selected from the group consisting of dimethyl sulfoxide, acetone and ethyl lactate.
7. The densely packed nano-diamond film according to claim 1, characterized in that: The organic solvent in step (1) is acetone.
8. The densely packed nano-diamond film according to claim 1, characterized in that: The single crystal silicon wafer in step (2) is also pre-treated as follows before spin coating: The pieces were cut into 20×20 mm size, ultrasonically cleaned in acetone, and dried with a nitrogen gun.
9. The densely packed nano-diamond film according to claim 1, characterized in that The hot wire chemical vapor deposition in step (4) is operated as follows: the acetone is brought into the reaction chamber of the hot wire chemical vapor deposition equipment by hydrogen bubbling with a flow rate of 60-100sccm, and pure hydrogen with a flow rate of 100-300sccm is introduced at the same time, the growth power is 1800-2400W, the growth pressure is controlled to be 1.8-2.0KPa, the growth time is 45-60min, and after the growth is completed, the carbon source is stopped, and the working voltage is reduced to 0 at a rate of 1V / min in a pure hydrogen atmosphere to obtain the densely packed nanodiamond film.
10. The densely packed nano-diamond film according to claim 9, characterized in that: The growth power is 2200 W, the growth pressure is 1.8 KPa, and the growth time is 60 min.