Preparation method of carbon catalyst loaded with platinum-cobalt-chromium alloy for fuel cell
By performing two reduction steps and high-temperature treatment in the aqueous suspension of carbon powder, large platinum-cobalt chromium alloy particles with small size deviations are formed, which solves the problem of degradation of existing catalyst performance and improves the stability of fuel cell catalysts and durability.
Patent Information
- Application Number
- CN202280002956.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-01
- Filing Date
- 2022-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-05-12
AI Technical Summary
Existing supported platinum alloy catalysts are prone to particle agglomeration during use, resulting in reduced performance and difficult to maintain the stability and durability of initial performance.
By adding chloroplatinic acid and L-ascorbic acid to the aqueous suspension of carbon powder, two reduction processes are carried out to form cluster-loaded nano-scale platinum particles, and cobalt hydroxide and chromium hydroxide are added at high temperature to form a relatively small amount of platinum particles. Large platinum-cobalt chromium alloy particles with small size deviations.
It effectively improves the performance stability and durability of the catalyst, and prepares platinum-cobalt chromium alloy particles with large particle size and small size deviation, which are suitable for fuel cells to support catalysts.
Smart Images

Figure CN115868045B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a carbon catalyst loaded with a platinum-cobalt-chromium alloy for a fuel cell. Background Art
[0002] Conventionally, a catalyst in which platinum or a platinum alloy is supported on the surface of a carbon support is used as an electrode catalyst for a fuel cell, or a catalyst in which platinum or a platinum alloy is supported on an inorganic oxide support such as silica is used as an exhaust gas treatment catalyst.
[0003] In the preparation of a platinum alloy-supported catalyst, a method is sometimes adopted in which platinum is first supported on a carbon support or the like, and then a metal to be alloyed is added in the form of a compound, and finally these metals are alloyed.
[0004] Regarding the preparation method of carbon loaded with platinum, Patent Document 1 records that a catalyst with a loading of about 10.5% and a platinum particle size of about 30 angstroms is obtained by the following method: a catalyst carrier composed of carbon black or the like is brought into contact with an acid aqueous solution, and the catalyst carrier that has been hydrophilically treated is fully brought into contact with an aqueous solution of chloroplatinic acid, the pH of the system is made alkaline, the temperature of the system is raised to a temperature at which the reducing agent takes effect, hydrogen peroxide is added as an anti-colloidal agglomerating agent, and a reducing agent having an aldehyde group is slowly added to reduce and load chloroplatinic acid.
[0005] In addition, Patent Document 2 describes the following: a carbon powder as a carrier is added to a solution prepared by dissolving dinitrodiammine platinum in nitric acid, and stirring is continued for 60 minutes to allow it to be fully dispersed. Then, an aqueous solution of L-ascorbic acid is added, and the mixture is heated in a hot water bath at 65° C. for one night (16 hours) while stirring and mixing. After cooling, the mixture is filtered, washed, and dried to obtain a carbon powder loaded with 9% by weight of platinum.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 63-49253,
[0009] Patent document 2: Japanese Patent Application Laid-Open No. 04-298238. Summary of the invention
[0010] Problems to be solved by the invention
[0011] Patent documents 1 and 2 are methods of first contacting a platinum compound with a carbon carrier and then reducing the platinum compound with a reducing agent to load fine platinum particles of a few nanometers on the surface of carbon powder. Although the initial performance is high, the catalyst particles agglomerate during use, causing the performance to change (degrade).
[0012] For fuel cell catalysts, such as phosphoric acid fuel cell cathode catalysts, which are strongly required to have improved performance stability and durability from the initial stage to the end of use, it is a problem to support catalyst particles of larger size and less size variation on carbon powder.
[0013] Means for solving problems
[0014] The present inventors have found that in the case of forming platinum particles in the initial stage of obtaining platinum-cobalt-chromium alloy particles, if L-ascorbic acid in an amount of 2.33 to 3.17 times the molar ratio of chloroplatinic acid to chloroplatinic acid is added to a suspension prepared by suspending carbon powder in water and heated to 80 to 100° C., and then an aqueous solution of chloroplatinic acid is added to the suspension at a rate of 0.001 g / min to 0.03 g / min in terms of platinum per 1 g of carbon powder (first reduction step), the surface of the carbon powder is reduced by 2.33 to 3.17 times the molar ratio of L-ascorbic acid to chloroplatinic acid. The platinum particles are grown into cluster-like particles of nanometer size. Then, in the suspension heated to 80-100°C after the first reduction step, the chloroplatinic acid that has not been reduced but can remain (not limited to, equivalent to 5%-30% of the initial amount in the first reduction step) is further reduced in a second reduction step using L-ascorbic acid to completely reduce the remaining chloroplatinic acid. This can effectively load the entire amount of chloroplatinic acid used initially on the surface of the carbon powder. Moreover, after the subsequent cobalt hydroxide and chromium hydroxide precipitation steps, platinum-cobalt-chromium alloy particles with a relatively large particle size and a small deviation can be loaded on the surface of the carbon powder.
[0015] Therefore, the above-mentioned problems can be solved by the present invention having the following features or aspects.
[0016] Method 1: A method for preparing a carbon catalyst loaded with a platinum-cobalt-chromium alloy for a fuel cell, characterized by comprising:
[0017] The process of preparing an aqueous suspension of carbon powder;
[0018] A step of preparing an aqueous solution of chloroplatinic acid;
[0019] A first reduction step, which is to add L-ascorbic acid to the water suspension of the carbon powder heated to 80-100° C., and then, while maintaining the heating temperature, add the chloroplatinic acid aqueous solution to the obtained water suspension of the carbon powder containing the ascorbic acid at a rate of 0.001 g / min-0.03 g / min per 1 g of the carbon powder in terms of platinum, thereby supporting and growing platinum particles of nanometer size in clusters on the surface of the carbon powder, wherein the ascorbic acid is used in a molar ratio of 2.33-3.17 times that of the chloroplatinic acid used;
[0020] A second reduction step, wherein L-ascorbic acid is added to the suspension heated to 80-100° C. after the first reduction step in an amount that can completely reduce the chloroplatinic acid remaining after the reduction step, thereby reducing the chloroplatinic acid and precipitating platinum on the surface of the platinum particles;
[0021] a precipitation step of filtering the suspension containing the carbon particles loaded with platinum particles obtained in the second reduction step to obtain a filter cake containing the carbon particles loaded with the platinum, washing the filter cake, adding an aqueous solution of a chromium compound and an aqueous solution of a cobalt compound to the resuspended solution after resuspending in water, and then adjusting the pH to 9 to 11 with aqueous ammonia, thereby precipitating cobalt hydroxide and chromium hydroxide on the surface of the platinum particles;
[0022] The following step comprises filtering the suspension obtained in the precipitation step, washing and drying the particles on the surface of the platinum particles on which cobalt hydroxide and chromium hydroxide are precipitated, thereby obtaining a powder in which the platinum particles on which cobalt hydroxide and chromium hydroxide are precipitated are supported in clusters on the surface of the carbon powder; and
[0023] The heat treatment step is to heat treat the carbon powder on which the platinum particles on which cobalt hydroxide and chromium hydroxide are precipitated are supported in the form of clusters in an inert gas or nitrogen atmosphere.
[0024] Method 2: The method for preparing a carbon catalyst loaded with a platinum-cobalt-chromium alloy for a fuel cell of Method 1, characterized in that the amount of platinum in the carbon catalyst loaded with a platinum-cobalt-chromium alloy is adjusted to 11 wt% to 15 wt% on a weight basis.
[0025] Method 3: A method for preparing a carbon catalyst loaded with a platinum-cobalt-chromium alloy for a fuel cell of method 1 or 2, characterized in that in the first and second reduction steps of chloroplatinic acid, the temperature of the suspension is set to 92°C~95°C, and the average particle size of the platinum-cobalt-chromium alloy particles is adjusted to 10~20nm.
[0026] Effects of the Invention
[0027] According to the present invention, a platinum-cobalt-chromium alloy-supported carbon catalyst for a fuel cell, which supports platinum-cobalt-chromium alloy particles having a relatively large particle size and a small size deviation, can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] [ Figure 1 ] is an example of a TEM image of platinum-supported carbon after the second reduction step in the preparation method of the present invention.
[0029] [ Figure 2 ] is an example of a TEM image of a platinum-cobalt-chromium alloy-supported carbon catalyst obtained by the preparation method of the present invention. DETAILED DESCRIPTION
[0030] Unless otherwise specified, the terms used in this specification are understood to have the meanings commonly used in the technical field.
[0031] Chloroplatinic acid refers to hexachloroplatinic (IV) acid (H2PtCl6). In addition, L-ascorbic acid is sometimes simply referred to as "ascorbic acid".
[0032] Mode 1 is characterized in that a first reduction step and a second reduction step are adopted. In addition to adopting a structure having such characteristics, the first reduction step and the second reduction step also include a structure having the following characteristics. Specifically, the first reduction step is to add L-ascorbic acid to a heated solution of 80 to 100°C of a previously prepared water suspension of carbon powder, and then, while maintaining the heating temperature, add the chloroplatinic acid aqueous solution to the obtained water suspension of carbon powder containing the ascorbic acid at an input rate of 0.001 g / min to 0.03 g / min per 1 g of the carbon powder in terms of platinum, thereby supporting and growing platinum particles of nanometer size on the surface of the carbon powder in clusters, and further, it is also characterized in that the ascorbic acid is used in a molar ratio of 2.33 to 3.17 times the chloroplatinic acid used in the treatment. The molar ratio of ascorbic acid to chloroplatinic acid mentioned here uses an amount of ascorbic acid that is excessive in amount than the stoichiometric molar ratio required for the reduction of the former. This is based on the confirmation that the ascorbic acid used according to the stoichiometric amount may not work under the reaction conditions of the first reduction step of the method 1. Although not limited to this, in the method 1, due to the above-mentioned "using 2.33 to 3.17 times the ascorbic acid", about 70% to about 95% of the chloroplatinic acid used is reduced. In this way, the second reduction step is adopted, in which L-ascorbic acid is added to the suspension heated to 80 to 100° C. after the first reduction step in an amount that can completely reduce the chloroplatinic acid remaining after the reduction step. However, assuming that in order to reduce the entire amount of chloroplatinic acid used in the first reduction step, it is confirmed that about 3.33 times the ascorbic acid in terms of molar ratio is required. Therefore, the amount of ascorbic acid that can reduce all the chloroplatinic acid remaining after the first reduction step (calculated to be 5% to 30%) is sufficient. When the amount of ascorbic acid added in the first reduction step is X times the molar ratio of chloroplatinic acid, it is sufficient to add (3.33-X) times or more ascorbic acid to the heated suspension after the first reduction step in terms of molar ratio relative to chloroplatinic acid.
[0033] This is not to limit the scope of the present invention by theory, but can be understood as follows.
[0034] If chloroplatinic acid aqueous solution is added to the heated suspension containing ascorbic acid, then at the beginning of the addition, the reduction reaction of platinum is immediately carried out to form nano-sized platinum particles. On the other hand, from the input of the chloroplatinic acid aqueous solution in the second half to the end of the input, since the amount of L-ascorbic acid is limited to 70% to 95% of the amount of reducible chloroplatinic acid, the chloroplatinic acid is slowly reduced in a state where L-ascorbic acid is less. The slowly reduced chloroplatinic acid plays the role of an adhesive connecting platinum particles to each other when it becomes larger particles and is in a stable state, and plays the role of connecting the platinum particles generated in the early stage to the platinum particles supported on carbon. Thus, in this method, the platinum particles grow into clusters and are supported on a carbon carrier. In this way, in the invention of mode 1, the first reduction step and the second reduction step are adopted.
[0035] Next, the suspension after the second reduction step is filtered to obtain a filter cake containing carbon particles loaded with platinum particles, and the filter cake is washed with water to modulate a resuspension formed by resuspending in water. Furthermore, the suspension is supplied to a precipitation step, which is performed by adding an aqueous chromium compound solution and an aqueous cobalt compound solution, and then adjusting the pH to 9 to 11 with ammonia water, so that cobalt hydroxide and chromium hydroxide are precipitated on the surface of the platinum particles. The suspension obtained in the precipitation step is supplied to the following steps in the same manner as the filter cake containing the above-mentioned carbon particles loaded with platinum particles, that is, filtered, washed, and dried to obtain a powder of platinum particles precipitated with cobalt hydroxide and chromium hydroxide in clusters on the surface of the carbon powder. The powder is further supplied to a heat treatment step in which the powder is heat-treated in an inert gas or nitrogen atmosphere, and a carbon catalyst loaded with platinum cobalt chromium alloy for a target fuel cell can be provided.
[0036] Hereinafter, the present invention will be described in more detail although the description may be repeated.
[0037] The carbon powder used in the first embodiment is not particularly limited, and may be a carbon powder used for supporting platinum in the preparation of an electrode catalyst, for example, carbon black such as furnace black, channel black, acetylene black, and graphitized carbon obtained by graphitizing these carbon blacks. For example, a specific surface area of 50 m 2 / g~300m 2 / g of conductive graphitized carbon is suspended in water to obtain a suspension. The carbon concentration in the suspension can be set to 10g / L to 18g / L.
[0038] The water used here may be pure water after ion exchange.
[0039] The method comprises the step of preparing an aqueous solution of chloroplatinic acid, wherein the concentration thereof can be 130 g / L to 660 g / L in terms of platinum.
[0040] In the first reduction step and the second reduction step, L-ascorbic acid is used as a reducing agent for platinum, but ascorbic acid is a safe and easy-to-handle reducing agent compared to aldehydes, hydrazine, and ethanol commonly used in various reduction systems. In addition, chloroplatinic acid is the most common among platinum compounds and is relatively cheap.
[0041] In addition, in the first reduction step, the chloroplatinic acid aqueous solution is added to the 80-100°C water suspension of carbon powder containing ascorbic acid at a rate of 0.001 g / min to 0.03 g / min per 1 g of carbon powder in terms of platinum. Here, if the temperature of the suspension is lower than 80°C, the reduction reaction of chloroplatinic acid is difficult to proceed, and if it is above 100°C, the evaporation amount of water as a solvent becomes large, and it becomes difficult to optimize the amount of solvent, so the heating temperature is generally set to the range of 80-100°C. In addition, since the heating temperature in the first reduction step affects the speed of the reduction reaction and the growth degree of clustered platinum particles, in order to control the clustered platinum particles with high precision, it is preferred to control the heating temperature within a specified range of ±1.5°C.
[0042] Next, an aqueous solution of chloroplatinic acid is added to the suspension at a rate of 0.001 to 0.03 g / min, preferably 0.002 to 0.01 g / min, more preferably 0.003 to 0.006 g / min in terms of platinum per 1 g of carbon powder in the suspension.
[0043] exist Figure 1 An example of a TEM image of platinum-supporting carbon after the second reduction step prepared by the present preparation method is shown in FIG.
[0044] according to Figure 1 It is believed that most of the platinum is reduced in the first reduction step. After the first reduction step, the platinum particles are supported on the carbon support in clusters as shown in the TEM image. The growth rate of the clustered platinum particles is sometimes the biggest factor in determining the alloy particle size.
[0045] By adding the chloroplatinic acid aqueous solution at a predetermined feeding rate of 0.001 g / min to 0.03 g / min in terms of platinum per 1 g of carbon powder, the growth rate of particles can be stably and uniformly controlled at an industrially practicable level.
[0046] The reason for this is considered to be that, at this stage, by controlling the rate of adding chloroplatinic acid, the reduction reaction rate can be controlled under sufficient mixing and diffusion conditions.
[0047] As shown in Table 1 below, since the average particle size of the alloy changes with respect to the input speed of the chloroplatinic acid aqueous solution, the average particle size of the alloy can be adjusted from 8 to 20 nm to a particularly desired average particle size of the alloy by utilizing this relationship. The average particle size of the alloy is preferably set to 8 to 16 nm, more preferably to 10 to 14 nm.
[0048] In the second reduction step, as described above, an amount of ascorbic acid that can completely reduce the chloroplatinic acid remaining without being reduced in the first reduction step is added to the suspension heated to 80-100° C. after the first reduction step, thereby allowing additional platinum to be precipitated on the platinum particles precipitated in the form of carbon powder in the first reduction step.
[0049] The amount of L-ascorbic acid added to the suspension in the second reduction step is set to an amount that can reduce all the chloroplatinic acid remaining in the first reduction step. For example, when L-ascorbic acid is added in a molar ratio of 2.33 times relative to chloroplatinic acid in the first reduction step, the amount of L-ascorbic acid in the second reduction step is set to (3.33-2.33) = 1.00 times or more.
[0050] For example, when 3.17 times the molar amount of L-ascorbic acid is added to chloroplatinic acid in the first reduction step, the amount of L-ascorbic acid in the second reduction step is set to (3.33-3.17)=0.16 times the molar amount or more.
[0051] By making the amount of the L-ascorbic acid added in the suspension in the second reduction process as described above, for 5~30% unreduced chloroplatinic acid remaining after the first reduction process, in the second reduction process, comprise the chloroplatinic acid that plays the role of adhesive, chloroplatinic acid can be fully reduced, be loaded on platinum carbon.Like this, make it almost completely loaded on carbon, do not produce the unreduced platinum relevant with the loss of platinum, certainly this is important industrially, therefore, wish to add a large amount of superfluous (about 3 times of the amount that chloroplatinic acid can be fully reduced) L-ascorbic acid to reduce.That is, in the second reduction process, in order to completely reduce a small amount of unreduced chloroplatinic acid remaining, can add a large amount of superfluous (about 3 times of the amount that chloroplatinic acid can be fully reduced) L-ascorbic acid, also can add L-ascorbic acid several times.
[0052] As described above, the suspension after the second reduction step is filtered to obtain a filter cake containing carbon particles loaded with platinum particles, and the filter cake is washed with water to prepare a re-suspended liquid resuspended in water. Furthermore, the suspension is supplied to a precipitation step, in which a chromium compound aqueous solution and a cobalt compound aqueous solution are added, and then the pH is adjusted to 9 to 11 with ammonia water, so that cobalt hydroxide and chromium hydroxide are precipitated on the surface of the platinum particles. The suspension obtained in the precipitation step is supplied to the following steps in the same manner as the filter cake containing the above-mentioned carbon particles loaded with platinum particles, that is, filtered, washed, and dried to obtain a powder of platinum particles precipitated with cobalt hydroxide and chromium hydroxide in clusters on the surface of the carbon powder. The powder is further supplied to a heat treatment step in which the powder is heat-treated in an inert gas or nitrogen atmosphere, and a target carbon catalyst loaded with platinum cobalt chromium alloy for a fuel cell can be provided. The precipitation step of precipitating cobalt hydroxide and chromium hydroxide on the surface of the platinum particles can usually be carried out at a temperature of 5°C to 50°C for 0.1 hours to 3 hours.
[0053] The above-mentioned washing method is not particularly limited and can be carried out by various means. Filtration can be carried out using a belt filter, a drum filter, a centrifuge, a vacuum filter, a pressure filter, a filter press, etc.
[0054] Regarding the method for precipitating the load of cobalt hydroxide and chromium hydroxide, the re-suspension of the filter cake containing the carbon particles loaded with platinum obtained in the second reduction step in water is mixed with, for example, an aqueous solution of chromium acetate and an aqueous solution of cobalt acetate, and the pH of the mixed solution thus obtained is adjusted to 9 to 11 with aqueous ammonia, thereby cobalt hydroxide and chromium hydroxide can be precipitated on the surface of the platinum particles. As the cobalt compound and the chromium compound, chromium acetate and cobalt acetate can be used. In addition, compounds such as chromium nitrate and cobalt nitrate can be used instead of acetate.
[0055] In this way, a powder in which nano-sized platinum particles having cobalt hydroxide and chromium hydroxide deposited thereon are supported in clusters on the surface of a carbon powder can be obtained, and such a powder is heat-treated in an inert gas or nitrogen atmosphere.
[0056] The filtration and washing of the suspension of the platinum-cobalt hydroxide-chromium hydroxide-supported carbon powder can be performed by the same means as the filtration and washing of the platinum-supported carbon suspension.
[0057] The drying method used in these steps is not particularly limited, and various dryers can be used for drying. Specifically, there can be mentioned methods of using a hot air dryer, a vacuum dryer, an inert oven, etc. at a temperature of 50° C. to 250° C. for several hours to several tens of hours.
[0058] The dried carbon powder loaded with platinum-cobalt hydroxide-chromium hydroxide is heat-treated in an inert gas or nitrogen atmosphere, for example, at 800°C to 1100°C. Thus, alloy particles of platinum-cobalt-chromium are generated. At this time, the inert gas used is not particularly limited, and helium or argon can be used. Preferably, it can be carried out under gas circulation.
[0059] An example of a TEM image of the platinum-cobalt-chromium alloy-supported carbon catalyst obtained by the above operation is shown in Figure 2 middle. Example
[0060] Hereinafter, examples of the present invention will be described, but the present invention is not limited to these examples.
[0061] (Example 1)
[0062] First, the specific surface area of 1877g was about 80m 2 / g of conductive graphitized carbon was suspended in 150L of pure water, and after heating to 97-100°C while stirring the suspension, 594g of L-ascorbic acid was added, and chloroplatinic acid aqueous solution was added 5 minutes later. At this time, a solution was added at a certain speed using a liquid delivery pump for 40 minutes to dissolve 264g of chloroplatinic acid in 1100g of pure water in terms of platinum content. Therefore, the input rate of chloroplatinic acid aqueous solution is 0.0035g / minute per 1g of carbon powder in terms of platinum. 5 minutes after the input of the chloroplatinic acid aqueous solution was completed, 1306g of L-ascorbic acid was added, and heating was stopped 10 minutes later. In this way, a suspension containing a powder loaded with platinum particles in clusters on a carbon carrier was obtained. Hereinafter, the suspension is referred to as "SPtC1".
[0063] <Precipitation of cobalt hydroxide and chromium hydroxide>
[0064] The suspension SPtC1 was filtered to obtain a filter cake. After being cleaned, it was suspended in 120L of pure water, and after being heated to 25-30°C while stirring, a solution of 174g of cobalt acetate (II) tetrahydrate and 118g of chromium acetate (III) dissolved in 3L of water was added, and mixed for more than 30 minutes. Then, in order to precipitate cobalt hydroxide and chromium hydroxide, a liquid feed pump was used to add 762g of 25% ammonia water in the suspension at a certain speed in 10 minutes. In this way, a suspension containing a carbon powder loaded with clustered platinum particles having cobalt hydroxide and chromium hydroxide precipitated on the surface of the platinum particles was obtained. Hereinafter, the suspension is referred to as "SPtCoCrC1".
[0065] The suspension SPtCoCrC1 was filtered to obtain a filter cake. After washing, it was vacuum dried at 100°C for 48 hours. In this way, a carbon powder loaded with clustered platinum particles with cobalt hydroxide and chromium hydroxide precipitated on the surface of the platinum particles was obtained. Hereinafter, this powder is referred to as "powder P1".
[0066] Next, the powder P1 was pulverized into a fine powder, and then heat treated at 980° C. for 1.5 hours in a nitrogen atmosphere.
[0067] The operations were carried out as described above to prepare a platinum-cobalt-chromium alloy-supported carbon catalyst, which is hereinafter referred to as "Example 1".
[0068] (Example 2)
[0069] The supported catalyst was prepared in the same manner as in Example 1 except that the temperature during the reduction loading of chloroplatinic acid was 92-95°C and the time for adding chloroplatinic acid was 35 minutes. Hereinafter, this is referred to as "Example 2". At this time, the rate of adding chloroplatinic acid was 0.0040 g / min per 1 g of carbon powder.
[0070] (Example 3)
[0071] A supported catalyst was prepared in the same manner as in Example 1 except that the temperature during the reduction loading of chloroplatinic acid was 92-95°C and the time for adding chloroplatinic acid was 31 minutes. Hereinafter, this is referred to as "Example 3". At this time, the rate of adding chloroplatinic acid was 0.0045 g / min per 1 g of carbon powder.
[0072] (Example 4)
[0073] A supported catalyst was prepared in the same manner as in Example 1 except that the temperature during the reduction loading of chloroplatinic acid was 92-95°C and the time for adding chloroplatinic acid was 29 minutes. Hereinafter, this is referred to as "Example 4". At this time, the rate of adding chloroplatinic acid was 0.0049 g / min per 1 g of carbon powder.
[0074] (Comparative Example 1)
[0075] The supported catalyst was prepared in the same manner as described in Example 1, except that the amount of L-ascorbic acid added in the first reduction step was set to 1900 g, which was an amount that could completely reduce the chloroplatinic acid, the time for adding chloroplatinic acid was set to 10 seconds, and the second reduction step was not performed. Hereinafter, it is referred to as "Comparative Example 1". At this time, the rate of adding chloroplatinic acid was 0.8443 g / min per 1 g of carbon powder.
[0076] The average particle size and standard deviation σ of the platinum-cobalt-chromium alloy of the platinum-cobalt-chromium alloy-supported carbon catalysts of Examples 1 to 4 and Comparative Example 1 are shown in Table 1 below.
[0077] Table 1
[0078]
[0079] <Measurement of Average Particle Diameter of Catalyst Particles>
[0080] It was determined by TEM observation of each sample.
[0081] In Comparative Example 1 in Table 1 above, the alloy particle size has a large variation, which is an undesirable catalyst property.
[0082] On the other hand, the average particle diameter of the alloy particles of the catalyst involved in Example 1 to Example 4 of the above-mentioned Table 1 is in the range of 8 to 20 nm, which is more uniform. In addition, by changing the temperature and the dropping time of chloroplatinic acid, it can be adjusted to a particularly desired alloy particle diameter. That is, by these results, it is implied that by preparing catalyst with this preparation method, in platinum-cobalt-chromium alloy catalyst, the alloy catalyst particle diameter can be prepared to the desired catalyst particle diameter from the range of 8 to 20 nm with good reproducibility on an industrial scale.
[0083] <Electrochemical Evaluation>
[0084] In order to evaluate the performance as an electrode catalyst for a fuel cell, the oxygen reduction reaction (ORR) activity of the catalyst of Example 2 was evaluated by a rotating electrode method using a BAS potentiostat / galvanostat.
[0085] The catalyst of Example 2 and the perfluorosulfonic acid dispersion were dispersed in a mixed solvent of 2-propanol and water to prepare a catalyst ink. The prepared catalyst ink was applied on glassy carbon (6 mm in diameter) to a platinum content of 18 μg / cm 2 , and electrodes for measurement were produced.
[0086] The prepared measuring electrode was immersed in nitrogen-saturated 25°C, 0.1mol / L perchloric acid, a reversible hydrogen electrode (RHE) was used as the reference electrode, and a platinum wire was used as the counter electrode. The CV (cyclic voltammogram) was measured in a potential scanning range of 0.05V~1.2V (vs. RHE) and a potential scanning rate of 50mV / sec. The ECSA (electrochemically active surface area) was calculated from the hydrogen desorption wave obtained from the CV. Then, oxygen was introduced into the battery, and in an oxygen-saturated atmosphere, the measuring electrode was rotated at 1600rpm while the polarization curve was measured at a potential of 0.05V~1.2V (vs. RHE) and a potential scanning rate of 10mV / sec. According to the obtained polarization curve, the kinetic current value (Ik) excluding the diffusion effect of oxygen was calculated by the following formula from the oxygen reduction current value (I) of 0.9V and the oxygen reduction current value (Id) of 0.4V as the limiting diffusion current value.
[0087] Ik=Id·I (Id·I)
[0088] The specific activity was calculated by dividing the kinetic current value (Ik) by the ECSA, and the mass activity was calculated by dividing the kinetic current value (Ik) by the weight of platinum on the glassy carbon electrode. The ECSA of the catalyst of Example 2 was 8.4 m 2 / g, the specific activity and mass activity were 5692μA / cm 2 , 478A / g. By increasing the catalyst particle size, the ECSA is smaller, but the specific activity and mass activity are high, and high output can be obtained. Therefore, the catalyst prepared by this preparation method can be used as an electrode catalyst for fuel cells.
[0089] Industrial Applicability
[0090] The catalyst obtained by the method of the present invention, i.e., a carbon catalyst loaded with platinum-cobalt-chromium alloy particles having a relatively large particle size and a small size deviation, has high performance stability and durability during use, and can therefore be used as a carbon catalyst loaded with platinum-cobalt-chromium alloy for fuel cells.
Claims
1. A method for preparing a carbon catalyst loaded with a platinum-cobalt-chromium alloy for a fuel cell, characterized in that: include: The process of preparing an aqueous suspension of carbon powder; A step of preparing an aqueous solution of chloroplatinic acid; A first reduction step, which is a step of adding L-ascorbic acid to an aqueous suspension of the carbon powder heated to 80 to 100° C., and then, while maintaining the heating temperature, adding the aqueous solution of chloroplatinic acid to the obtained aqueous suspension of the carbon powder containing the L-ascorbic acid at a rate of 0.001 g / min to 0.03 g / min in terms of platinum per 1 g of the carbon powder, thereby supporting and growing platinum particles of nanometer size in clusters on the surface of the carbon powder, wherein the L-ascorbic acid is used in a molar ratio of 2.33 to 3.17 times that of the chloroplatinic acid used; A second reduction step, wherein L-ascorbic acid is added to the suspension heated to 80 to 100° C. after the first reduction step in an amount capable of completely reducing the chloroplatinic acid remaining after the reduction step, thereby reducing the chloroplatinic acid and precipitating platinum on the surface of the platinum particles; a precipitation step of filtering the suspension containing the carbon particles loaded with platinum particles obtained in the second reduction step to obtain the carbon particles loaded with the platinum, washing the carbon particles, adding an aqueous solution of a chromium compound and an aqueous solution of a cobalt compound to the resuspended solution resuspended in water, and then adjusting the pH to 9 to 11 with aqueous ammonia, thereby precipitating cobalt hydroxide and chromium hydroxide on the surface of the platinum particles; The following step comprises filtering the suspension obtained in the precipitation step, washing and drying the particles on the surface of the platinum particles on which cobalt hydroxide and chromium hydroxide are precipitated, thereby obtaining a powder in which the platinum particles on which cobalt hydroxide and chromium hydroxide are precipitated are supported in clusters on the surface of the carbon powder; and The heat treatment step is to heat treat the carbon powder on which the platinum particles on which cobalt hydroxide and chromium hydroxide are precipitated are supported in the form of clusters in an inert gas or nitrogen atmosphere.
2. The method for preparing the platinum-cobalt-chromium alloy-supported carbon catalyst for fuel cells according to claim 1, characterized in that: The amount of platinum in the platinum-cobalt-chromium alloy-supported carbon catalyst is adjusted to 11 wt % to 15 wt % on a weight basis.
3. The method for preparing the carbon catalyst loaded with platinum-cobalt-chromium alloy for fuel cells according to claim 1 or 2, characterized in that: In the first and second reduction steps of chloroplatinic acid, the temperature of the suspension is set to 92° C. to 95° C., and the average particle size of the platinum-cobalt-chromium alloy particles is adjusted to 10 to 20 nm.