A method for cleaning non-proportioned indium phosphide polycrystalline material for recycling

Through a combination of alcohol, deionized water, high-temperature flowing inert gas heating, grinding, hydrochloric acid etching and ultrasonic waves, the problem of incomplete cleaning of indium phosphide polycrystalline materials and the formation of oxide layers was solved, and the purity and return of polycrystalline materials were improved. performance, simplifying the process and reducing environmental pollution and costs.

CN115872375BActive Publication Date: 2024-10-25THE 13TH RES INST OF CHINA ELECTRONICS TECH GRP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211703548.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-10-25
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

When cleaning indium phosphide polycrystalline materials with the existing technology, surface unevenness and the formation of oxide layers lead to a reduction in return purity, and the process is complicated, causing environmental pollution and high costs.

Method used

Cleaning with alcohol and deionized water, heating with high-temperature flowing inert gas, polishing, hydrochloric acid corrosion and ultrasonic waves are used to remove the surface oxide layer, forming an exposed indium layer and then vacuum drying to avoid the formation of an oxide layer and improve purity.

Benefits of technology

It effectively improves the purity of indium phosphide polycrystalline materials, simplifies the process, reduces environmental pollution and costs, and is suitable for cleaning polycrystalline materials of diverse shapes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method for cleaning non-proportional indium phosphide polycrystalline material for recycling belongs to the field of semiconductor material technology, including: cleaning the non-proportional indium phosphide polycrystalline material with alcohol, and then cleaning it with deionized water for 3-5 times; heating the polycrystalline material to 800-850°C under flowing inert gas for 20-60 minutes, and then lowering the temperature to room temperature; polishing to remove the indium phosphide on the surface; immersing the polished polycrystalline material in hydrochloric acid for corrosion for 1-2 minutes, and then cleaning it with deionized water for 3-5 times; boiling it with boiling deionized water for 10-30 minutes; and vacuum drying. The present invention adopts a method combining physics and chemistry, which can effectively avoid the formation of an oxide layer of the polycrystalline material and improve the purity of the polycrystalline material; the process is simple, the acid corrosion process has fewer links, the pollution to the environment is less, and the cost is low; according to the characteristics of the diversity of shapes of polycrystalline materials for recycling, it can be effectively cleaned.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor materials, and in particular relates to a method for cleaning non-proportioned indium phosphide polycrystalline material for recycling. Background Art

[0002] InP (indium phosphide) is an important compound semiconductor material after silicon (Si), germanium (Ge), and gallium arsenide (GaAs). It is one of the preferred materials for preparing high-frequency and high-speed devices. InP-based microelectronic devices have the characteristics of high frequency, low noise, high efficiency, and radiation resistance. They are widely used in 5G networks, space solar cells, terahertz communications, millimeter wave communications and detection and other fields.

[0003] Indium phosphide polycrystalline material is the basis for preparing single crystals, and a large amount of indium phosphide polycrystalline material is required in the production process of indium phosphide single crystals.

[0004] The indium phosphide polycrystalline material remaining after preparing indium phosphide single crystals is a usable resource and can be returned to the furnace to prepare indium phosphide single crystals again after cleaning.

[0005] During the single crystal growth process, the remaining indium phosphide polycrystalline material contains indium elements, forming non-proportional indium phosphide polycrystals, and the shape is more diverse than that of the original material. Conventional cleaning methods are not suitable for indium phosphide polycrystals used in the furnace.

[0006] The current cleaning process of indium phosphide polycrystalline materials uses physical methods for cleaning, and then corrodes the surface. Generally, the cleaning is achieved by immersing in a cleaning solution. The cleaning solution is generally a mixture of bromomethanol, hydrofluoric acid solution and hydrochloric acid solution, or ammonia water, hydrogen peroxide, etc. Further improvements are to increase vibration, introduce ultrasonic waves, etc. This method has two problems: 1. The indium phosphide polycrystalline material with an uneven surface is not cleaned thoroughly, and 2. Direct corrosion is easy to form an oxide layer on the surface, introduce impurities, and reduce the purity of the recycled indium phosphide polycrystalline material. Summary of the invention

[0007] The purpose of the invention is to provide a cleaning method according to the characteristics of non-proportioned indium phosphide polycrystalline material for recycling.

[0008] The present invention provides a method for cleaning a non-proportioned indium phosphide polycrystalline material for recycling, comprising the following steps:

[0009] Step 1, wash the non-proportioned indium phosphide polycrystalline material with alcohol, and then wash it with deionized water for 3-5 times;

[0010] Step 2, heating the polycrystalline material to 800-850° C. under flowing inert gas for 20-60 minutes, and then lowering the temperature to room temperature;

[0011] Step 3: Polishing to remove the indium phosphide on the surface;

[0012] Step 4, immerse the polished polycrystalline material in hydrochloric acid for 1-2 minutes, and then wash it with deionized water for 3-5 times;

[0013] Step 5: Boil in boiling deionized water for 10-30 minutes;

[0014] Step 6: Vacuum drying.

[0015] Furthermore, in step 2, the polycrystalline material is stirred.

[0016] Further, in step 4, ultrasonic waves are applied.

[0017] The present invention heats the indium phosphide polycrystalline material at 800-850°C and in a flowing inert gas environment for 20-60 minutes, and then cools it to room temperature. Indium phosphide on the surface of the indium phosphide polycrystalline material decomposes indium and phosphorus gas, and the phosphorus gas enters the inert gas. After the surface indium solidifies, a thin layer of indium phosphide is formed on the surface. The surface thin layer of indium phosphide is polished off until the indium layer is exposed, and then it is immersed in hydrochloric acid for corrosion for 1-2 minutes. After forming a bright indium layer, it is vacuum dried, and then phosphorus is added after returning to the furnace to prepare polycrystals, or crystal growth is performed after phosphorus is added.

[0018] Beneficial effects: The traditional single acid etching method will form an oxide layer on the surface and introduce impurities. The present invention adopts a combination of physical and chemical methods, which can effectively avoid the formation of an oxide layer on the polycrystalline material and improve the purity of the polycrystalline material. At the same time, the process is simple, with fewer acid etching process steps, less pollution to the environment, and low cost. In view of the diverse shapes of polycrystalline materials for recycling, it can be effectively cleaned. DETAILED DESCRIPTION

[0019] The present invention provides a method for cleaning a non-proportioned indium phosphide polycrystalline material for recycling, comprising the following steps:

[0020] Step 1: Clean the non-proportioned indium phosphide polycrystalline material with alcohol, and then wash it with deionized water for 3-5 times to remove impurities and organic matter on the surface.

[0021] Step 2: Heat the polycrystalline material to 800-850°C under flowing inert gas for 20-60 minutes, and then lower the temperature to room temperature. During the heating process, a quartz rod can be used to stir the polycrystalline material, or the cleaning equipment can be turned over and over to fully expose the surface of the indium phosphide polycrystalline material to the atmosphere to accelerate the reaction.

[0022] Step 2 is the key to the present invention. Under the above conditions, indium and phosphorus gas are decomposed on the surface of the indium phosphide polycrystalline material, indium liquefies and adheres to the surface of the indium phosphide polycrystalline material, most of the phosphorus gas enters the inert gas and is discharged with the flowing inert gas, and a small amount remains in the liquid indium; after cooling, indium solidifies on the surface of the polycrystalline material, and due to the small amount of phosphorus remaining in the liquid indium, an indium phosphide surface layer is formed on the outermost surface of the polycrystalline material.

[0023] The polycrystalline material that has been heated has a thin layer of indium phosphide on the surface, indium in the middle, and an indium phosphide matrix inside.

[0024] Step 3: Polish to remove the indium phosphide on the surface and expose the indium layer.

[0025] Step 4: Immerse the polished polycrystalline material in hydrochloric acid for corrosion for 1-2 minutes, and then wash it with deionized water for 3-5 times; during the soaking and washing process, apply ultrasonic waves to clean it more effectively.

[0026] Since the surface of the polycrystalline material treated in the above steps is covered with indium, no oxide layer is formed during the etching process.

[0027] Step 5: Boil in boiling deionized water for 10-30 minutes.

[0028] Step 6: Vacuum drying.

[0029] The method proposed by the present invention is also applicable to non-recycled indium phosphide polycrystals.

[0030] During the single crystal growth process, the remaining indium phosphide polycrystalline material will lose some phosphorus due to the high temperature and will contain some indium elements, forming a non-proportional polycrystalline material.

[0031] After cleaning by the method proposed by the present invention, a layer of indium will be formed on the surface of the polycrystalline material. Therefore, the processing of the proportioned indium phosphide polycrystalline material will reduce the proportion of the original polycrystalline material. The recycled indium phosphide polycrystalline material itself is a non-proportional material, and increasing the surface indium content will not deteriorate the material quality.

[0032] When single crystals are prepared from polycrystalline materials cleaned by this method, phosphorus is added to synthesize and prepare polycrystalline materials after returning to the furnace, or crystal growth is directly carried out after phosphorus is added. Example

[0033] Step 1: Take 2 kg of indium phosphide polycrystalline material, first wash it with 85%-100% alcohol for 10-20 minutes, and then wash it with deionized water for 3-5 times.

[0034] Step 2: Heat the polycrystalline material to 800-850° C. under flowing argon or nitrogen gas at 1 atmosphere pressure for 20-60 minutes, and then reduce the temperature to room temperature.

[0035] During the heating process, a quartz rod is used to flip the polycrystalline material so that the surface of the indium phosphide polycrystalline material is fully exposed to the high-temperature atmosphere. The polycrystalline material that has been heated has a thin layer of indium phosphide on the surface, indium in the middle, and an indium phosphide matrix inside. After heating, the temperature is cooled to room temperature and the polycrystalline ingot is taken out.

[0036] Step 3: Use 100-2000 mesh sandpaper to polish the surface of the indium phosphide polycrystalline material until a bright indium layer is exposed.

[0037] Step 4: Wash the polished polycrystalline material 3-5 times with deionized water, and after drying, immerse the polished polycrystalline material in hydrochloric acid for 1-2 minutes, with a concentration of 0.5-5 mol / L. Then wash it 3-5 times with deionized water; during the soaking and washing process, apply ultrasonic waves for more effective cleaning.

[0038] Step 5: Boil the indium phosphide polycrystalline material with boiling deionized water for 10-30 minutes, and then wash it with deionized water, and repeat this process 2-3 times.

[0039] Step 6: Vacuum drying.

[0040] Comparative Example 1

[0041] Step 1: Take 2 kg of indium phosphide polycrystalline material, first wash it with 85%-100% alcohol for 10-20 minutes, and then wash it with deionized water for 3-5 times.

[0042] Step 2: After drying, immerse the polycrystalline material in hydrochloric acid for 1-2 minutes, with a concentration of 0.5-5 mol / L. Then wash it with deionized water for 3-5 times; during the immersion and washing process, apply ultrasonic waves for more effective cleaning.

[0043] Step 3: Boil the indium phosphide polycrystalline material with boiling deionized water for 10-30 minutes, and then wash it with deionized water, and repeat this process 2-3 times.

[0044] Step 4: Vacuum drying.

[0045] Comparative Example 2

[0046] Step 1: Take 2 kg of indium phosphide polycrystalline material, first wash it with 85%-100% alcohol for 10-20 minutes, and then wash it with deionized water for 3-5 times.

[0047] Step 2: Heat the polycrystalline material to 800-850° C. under flowing argon or nitrogen gas at 1 atmosphere pressure for 20-60 minutes, and then reduce the temperature to room temperature.

[0048] During the heating process, a quartz rod is used to flip the polycrystalline material so that the surface of the indium phosphide polycrystalline material is fully exposed to the high-temperature atmosphere. The polycrystalline material that has been heated has a thin layer of indium phosphide on the surface, indium in the middle, and an indium phosphide matrix inside.

[0049] Step 3: Use 100-2000 mesh sandpaper to polish the surface of the indium phosphide polycrystalline material until a bright indium layer is exposed.

[0050] Step 4: Use deionized water to wash the polished polycrystalline material 3-5 times. After drying, wash it with deionized water for 3-5 times; during the soaking and washing process, apply ultrasonic waves to clean it more effectively.

[0051] Step 5: Boil the indium phosphide polycrystalline material with boiling deionized water for 10-30 minutes, and then wash it with deionized water, and repeat this process 2-3 times.

[0052] Step 6: Vacuum drying.

[0053] Four samples were taken from the polycrystalline materials treated in Example and Comparative Examples 1 and 2, respectively. The total impurity concentration (the number of impurity atoms per unit volume) of the surface area of ​​the polycrystalline materials was as follows:

[0054] Example Comparative Example 1 Comparative Example 2 Sample No. <![CDATA[Total impurity concentration / cm 3 > <![CDATA[Total impurity concentration / cm 3 > <![CDATA[Total impurity concentration / cm 3 > a <![CDATA[2.5×10 15 ]]> <![CDATA[8.5×10 15 ]]> <![CDATA[5.5×10 15 ]]> b <![CDATA[5.3×10 15 ]]> <![CDATA[7.1×10 15 ]]> <![CDATA[6.3×10 15 <!-- 3 -->]]> c <![CDATA[4.1×10 15 ]]> <![CDATA[1.2×10 16 ]]> <![CDATA[6.7×10 15 ]]> d <![CDATA[3.2×10 15 ]]> <![CDATA[2.0×10 16 ]]> <![CDATA[4.9×10 15 ]]>

[0055] Comparative Example 1 adopts the traditional pickling process, and Comparative Example 2 partially adopts the process proposed by the present invention, omitting the etching step in the middle.

[0056] Compared with Comparative Examples 1 and 2, the total impurity concentration in the surface area of ​​the polycrystalline material cleaned by the process of the present invention is greatly reduced.

Claims

1. A method for cleaning non-proportioned indium phosphide polycrystalline material for recycling, characterized in that: The method consists of the following steps: Step 1, wash the non-proportioned indium phosphide polycrystalline material with alcohol, and then wash it with deionized water for 3-5 times; Step 2, heating the polycrystalline material to 800-850° C. under flowing inert gas for 20-60 minutes, then lowering the temperature to room temperature. During the heating process, stirring the polycrystalline material with a quartz rod; Step 3: Polishing to remove the indium phosphide on the surface; Step 4, immerse the polished polycrystalline material in hydrochloric acid for 1-2 minutes, and then wash it with deionized water for 3-5 times; Step 5: Boil in boiling deionized water for 10-30 minutes; Step 6: Vacuum drying.

2. The method for cleaning the non-proportioned indium phosphide polycrystalline material for recycling according to claim 1, characterized in that: In step 4, ultrasonic waves are applied.