A metal complex and its preparation method and application
By developing the metal complex M(Cy)(R1R2R3R4) catalyst, the problem of lack of high-efficiency catalyst technology in China has been solved, and the efficient polymerization of ethylene and α-olefins has been achieved, filling the gap in the production process of high-end polyolefin materials, and is suitable for solutions Polyethylene elastomer was prepared.
Patent Information
- Application Number
- CN202210738538.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-09-29
- Filing Date
- 2022-06-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-06-22
AI Technical Summary
The lack of high-efficiency catalyst technology with independent intellectual property rights in China has led to a gap in the production process of high-end polyolefin materials, and has little understanding of the catalyst characteristics protected by foreign patents, and lacks engineering research on copolymerization of olefin high-temperature solutions.
Develop a metal complex M(Cy)(R1R2R3R4) as a catalyst, prepared by reacting compound I-2 with R-MgX and subsequently reacting with B(R4)3, for catalyzing the polymerization of ethylene and α-olefins, suitable for Polyethylene elastomer was prepared by solution method.
It provides a new and better catalytic system that effectively catalyzes the polymerization of ethylene and other olefins, improves the polymerization efficiency, and is suitable for the preparation of olefin materials by continuous or batch solution methods.
Smart Images

Figure CN115873046B_ABST
Abstract
Description
[0001] The present invention claims priority to a prior application with patent application number 202111152624.1, filed with the State Intellectual Property Office of China on September 29, 2021, entitled “A class of β-diketone-semi-locene metal complexes and preparation methods and applications thereof”. The entire text of the prior application is incorporated herein by reference. Technical Field
[0002] The present invention belongs to the field of metal catalysts, and specifically relates to a metal complex and its preparation method and application Background Art
[0003] Polyolefin elastomers include polymers copolymerized by ethylene and α-olefins, such as ethylene-octene copolymers, ethylene-hexene copolymers, and ethylene-butene copolymers. They are synthetic polymers with a rapidly growing production and application. They can replace a series of general polymers such as EPM, EPDM, EVA, SBC (styrene bulk copolymer), TPU, PVC, LDPE, and EMA, and are widely used in medical packaging materials, automotive parts, wires and cables, daily necessities, and toys. Since they can save processing links such as vulcanization during use, they can save 25% to 40% of energy consumption and improve processing efficiency by 10 to 20 times, which is widely welcomed by the industry. At present, the main manufacturers of polyolefin elastomers are Dow, ExxonMobil, and Mitsui of Japan. Representative products are Engage series polyolefin elastomers produced by Dow and Exact series polyolefin elastomers produced by ExxonMobil. The first company to industrialize polyolefin elastomers was Dow Chemical Company of the United States.
[0004] As we all know, catalysts represent the core of olefin coordination polymerization technology. Since the advent of ethylene propylene rubber elastomers (EPR, EPDM) in the 1960s, major petrochemical companies and research institutions have invested a lot of energy in developing catalyst technology for olefin copolymerization. Early EPDM elastomers were prepared using traditional Z-type catalysts, while the types of catalysts used in the industrial production of ethylene / α-olefin copolymer elastomers have now expanded to single-active-center metallocene catalysts and new post-metallocene catalysts. Since Kaminsky discovered that metallocene Cp2MCl2 (M=Ti, Zr, Hf) can catalyze olefin polymerization in aromatic hydrocarbon solvents with the partial hydrolysis product of trimethylaluminum, methylaluminoxane (MAO), as a co-catalyst, and show high catalytic activity, important research institutions around the world have launched research and development of homogeneous olefin polymerization catalytic systems.
[0005] Exxon (now ExxonMobil) of the United States first applied for a patent for metallocene catalysts (US4871705A). The patent application covers non-bridged dimetallocene and bridged dimetallocene catalysts. This technology introduces a bridging functional group into the metallocene ligand to connect the upper and lower metallocene rings, increasing the rigidity of the catalyst, and by changing the substituent structure on the metallocene ring, the steric hindrance of the active center can be adjusted, thereby achieving better control of olefin polymerization activity, product molecular weight size and distribution control, and stereoselectivity control of alpha olefins, and can produce polymer products with specific properties.
[0006] After non-bridged dimetallocene, bridged dimetallocene and bridged semi-metallocene, non-bridged semi-metallocene catalysts have also been studied in depth. Sumitomo Chemical of Japan has applied them to propylene homopolymerization and ethylene-propylene copolymerization, and the molecular weight of the obtained product is more than 200,000, but the catalytic activity is very low.
[0007] The production process of this type of high-end polyolefin materials has always been a blank spot in the domestic materials industry. Developing a high-end polyolefin production process with independent intellectual property rights is the key to meeting the domestic demand for high-end polyolefins. The key catalyst technology and solution polymerization process technology for preparing ethylene / α-olefin copolymer elastomers by high-temperature solution polymerization are almost all protected by foreign patents. Even for some catalytic systems disclosed by patents that have expired or are about to expire, my country lacks a deep understanding of the characteristics of these catalysts, and there are no engineering research reports on olefin high-temperature solution copolymerization.
[0008] Therefore, it is of great significance to develop effective and more efficient catalysts for the polymerization of ethylene and α-olefins. Summary of the invention
[0009] In order to improve the above technical problems, the present invention provides a complex represented by formula (I):
[0010]
[0011] Wherein, M is selected from titanium (Ti), zirconium (Zr) or hafnium (Hf);
[0012] Cy is selected from the following groups which are unsubstituted or optionally substituted by one, two or more Ra: cyclopentadienyl, indenyl, fluorenyl;
[0013] Each R1, R2 is the same or different and is independently selected from hydrogen, the following groups which are unsubstituted or optionally substituted by one, two or more Rb: C 1-20 Alkyl, C 6-20 Aryl, 5-20 membered heteroaryl;
[0014] Each R3 is the same or different and is independently selected from C which is unsubstituted or optionally substituted with one, two or more Rc1-20 alkyl;
[0015] Each R4 is the same or different and is independently selected from hydrogen, halogen, the following groups which are unsubstituted or optionally substituted by one, two or more Rd: C 1-20 Alkyl, C 1-20 Alkoxy, C 6-20 Aryl, C 6-20 Aryl C 1-20 alkyl;
[0016] Each Ra, Rb, Rc, Rd is the same or different and is independently selected from halogen, C 1-20 alkyl.
[0017] According to an embodiment of the present invention, Cy may be selected from cyclopentadienyl or pentamethylcyclopentadienyl;
[0018] Each R1, R2 may be the same or different and are independently selected from hydrogen, the following groups which are unsubstituted or optionally substituted by one, two or more Rb: C 1-6 Alkyl, C 6-8 Aryl, 5-8 membered heteroaryl;
[0019] Each R3 may be the same or different and is independently selected from C which is unsubstituted or optionally substituted with one, two or more Rc. 1-6 alkyl;
[0020] Each R4 may be the same or different and is independently selected from hydrogen, halogen, the following groups which are unsubstituted or optionally substituted by one, two or more Rd: 1-6 Alkyl, C 1-6 Alkoxy, C 6-8 Aryl, C 6-8 Aryl C 1-6 alkyl;
[0021] Each Ra, Rb, Rc, Rd is the same or different and is independently selected from halogen, C 1-6 alkyl.
[0022] According to an embodiment of the present invention, R1 may be selected from hydrogen, C 1-6 alkyl;
[0023] R2 can be selected from C 1-6 Alkyl, C 6-8 Aryl;
[0024] R3 can be selected from C 1-6 alkyl;
[0025] R4 can be selected from C which is unsubstituted or optionally substituted with one, two or more Rd 6-8 Aryl;
[0026] Each Rd is the same or different and is independently selected from halogen, C 1-6 alkyl.
[0027] According to an embodiment of the present invention, R1 may be selected from hydrogen and methyl; R2 may be selected from methyl and phenyl; R3 may be selected from methyl; and R4 may be selected from pentafluorophenyl.
[0028] According to an embodiment of the present invention, the complex represented by formula (I) is selected from:
[0029]
[0030] The present invention also provides a method for preparing the complex represented by formula (I), comprising the following steps:
[0031]
[0032] 1) Compound I-2 reacts with R-MgX to obtain compound I-1;
[0033] 2) Compound I-1 reacts with B(R4)3 to obtain a complex represented by formula (I);
[0034] Wherein, M, Cy, R1, R2, R3, R4 have the above-mentioned definitions; X, X1, X2 are the same or different and are independently selected from Cl, Br, I; R is selected from C 1-20 Alkyl, for example, methylmagnesium chloride, methylmagnesium bromide;
[0035] According to an embodiment of the present invention, in step 1), the reaction can be carried out in an organic solvent, and the organic solvent can be selected from at least one of tetrahydrofuran, diethyl ether, methyl tert-butyl ether, dioxane, and 2-methyltetrahydrofuran;
[0036] According to an embodiment of the present invention, in step 2), the reaction may be carried out in an organic solvent, and the organic solvent may be selected from toluene;
[0037] According to an embodiment of the present invention, in step 2), after the reaction is completed, a purification step is further included, in which the reaction solution is added to a poor solvent to precipitate to obtain a complex represented by formula (I); the poor solvent can be selected from at least one of diethyl ether, methyl tert-butyl ether, n-hexane, cyclohexane, and petroleum ether.
[0038] The present invention also provides the use of the complex represented by formula (I) as a catalyst, for example, for catalyzing the polymerization of ethylene and α-olefins.
[0039] Preferably, it is used for catalyzing the solution copolymerization of ethylene and α-olefin to prepare polyethylene elastomer.
[0040] According to an embodiment of the present invention, the α-olefin may be 1-butene, 1-hexene, or 1-octene.
[0041] According to an embodiment of the present invention, when catalyzing the polymerization of ethylene and α-olefin, the polymerization temperature can be 100°C-200°C, such as 120°C-180°C, exemplified by 130°C, 140°C, 150°C, 160°C, 170°C.
[0042] According to an embodiment of the present invention, when catalyzing the polymerization of ethylene and α-olefin, the polymerization pressure may be 1-8 MPa, such as 2-6 MPa, exemplified by 3 MPa, 4 MPa, and 5 MPa.
[0043] Beneficial Effects
[0044] The present invention provides a metal complex represented by formula (I), a preparation method and application thereof. The complex prepared by the present invention can effectively catalyze the polymerization of ethylene and other olefins (such as alpha olefins) as a catalyst, and is suitable for preparing olefin materials by continuous or intermittent solution method. A new and better catalytic system is provided for the polymerization of ethylene and other olefins (such as alpha olefins).
[0045] Definition and explanation of terms
[0046] Unless otherwise specified, the numerical ranges recorded in this specification and claims are equivalent to recording at least each specific integer value therein. For example, the numerical range "1-20" is equivalent to recording each integer value in the numerical range "1-10", namely 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, and each integer value in the numerical range "11-20", namely 11, 12, 13, 14, 15, 16, 17, 18, 19, 20.
[0047] It should be understood that herein, when describing one, two or more, "more" should refer to an integer greater than 2, for example, greater than or equal to 3, for example 3, 4, 5, 6, 7, 8, 9 or 10.
[0048] The term "halogen" refers to fluorine, chlorine, bromine and iodine.
[0049] The term "C 1-20 "Alkyl" is understood to mean a straight-chain or branched saturated monovalent hydrocarbon group having 1 to 20 carbon atoms. For example, "C 1-10 "Alkyl" means straight chain and branched chain alkyl groups having 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms. 1-8 "Alkyl" means straight chain and branched chain alkyl groups having 1, 2, 3, 4, 5, 6, 7, or 8 carbon atoms. 1-6The term "alkyl" refers to straight-chain and branched alkyl groups having 1, 2, 3, 4, 5 or 6 carbon atoms. The alkyl group is, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl or 1,2-dimethylbutyl, or the like or isomers thereof.
[0050] The term "C 6-20 "Aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic (such as fused, bridged, spiro) or tricyclic hydrocarbon ring having 6 to 20 carbon atoms, which may be a single aromatic ring or a polyaromatic ring fused together, preferably "C 6-14 The term "C 6-14 The term "aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring ("C 6-14 or a ring having 9 carbon atoms ("C9 aryl"), for example indanyl or indenyl, or a ring having 10 carbon atoms ("C 10 aryl), such as tetrahydronaphthyl, dihydronaphthyl or naphthyl, or a ring having 13 carbon atoms ("C 13 aryl), such as fluorenyl, or a ring having 14 carbon atoms ("C 14 aryl”), such as anthracenyl. When the C 6-20 When the aryl group is substituted, it may be monosubstituted or polysubstituted. Also, there is no limitation on the substitution position, for example, it may be substituted at the ortho position, para position or meta position.
[0051] The term "5-20 membered heteroaryl" is understood to include monovalent monocyclic, bicyclic (e.g. fused, bridged, spiro) or tricyclic aromatic ring systems having 5 to 20 ring atoms and containing 1 to 5 heteroatoms independently selected from N, O and S, for example "5-14 membered heteroaryl". The term "5-14 membered heteroaryl" is understood to include monovalent monocyclic, bicyclic or tricyclic aromatic ring systems having 5, 6, 7, 8, 9, 10, 11, 12, 13 or 14 ring atoms, in particular 5 or 6 or 9 or 10 carbon atoms, and containing 1 to 5, preferably 1 to 3 heteroatoms each independently selected from N, O and S and, in each case, furthermore, may be benzo-fused. "Heteroaryl" also refers to a radical in which a heteroaromatic ring is fused to one or more aryl, alicyclic or heterocyclyl rings, wherein the radical or point of attachment is on the heteroaromatic ring. Non-limiting examples include quinolinyl, isoquinolinyl, indolyl, benzo[b]thienyl, benzimidazolyl, benzothiazolyl.
[0052] The term "spirocyclic" refers to a ring system in which two rings share one ring-forming atom.
[0053] The term "fused ring" refers to a ring system in which two rings share two ring atoms.
[0054] The term "bridged ring" refers to a ring system in which two rings share three or more ring atoms. DETAILED DESCRIPTION
[0055] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0056] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0057] The testing method for the obtained product in the following embodiments includes:
[0058] Density: Solid density is tested according to GB / T 1033.1-2008 standard.
[0059] Melt index: GB / T 3682-2000 standard is used for testing, the test temperature is 190°C, the weights are 2.16kg, 5kg and 21.6kg respectively, among which MFR (190 / 2.16) represents the melt index of the resin when the weight is 2.16kg, and MFR (190 / 5) represents the melt index of the resin when the weight is 5kg.
[0060] Mw molecular weight: tested according to GB / T 36214.4-2018 standard.
[0061] PDI (Polymer Dispersibility Index): Tested using GB / T 36214.4-2018 standard.
[0062] Mass content of 1-octene: measured by NMR ( 1 H NMR) spectrum confirmed.
[0063] Catalyst activity: After the reaction in which the catalyst participates is completed, it is calculated based on the mass of the product obtained and the mass of the catalyst used.
[0064] [Example 1]
[0065] Preparation of catalyst a and its polymerization reaction
[0066]
[0067] Take 3mmol of dibenzoylmethane (dbm), add 30mL of dry ether and stir to dissolve. Add n-butyl lithium (1.2mL, 2.5mol / L) dropwise at 0℃, and a white precipitate will be generated immediately. After reacting at room temperature for 2h, a white emulsion will be formed, which is dibenzoylmethane lithium salt ((C 15 H 11 O2)Li) in ether.
[0068] Stir the lithium salt and 3mmol cyclopentadienyl titanium trichloride (CpTiCl3) evenly, keep reflux at 80℃ for 2h. Cool to room temperature and filter. Concentrate the filtrate to about 5mL under vacuum. Add 5mL of freshly distilled n-hexane, filter, and wash the solid twice with 10mL of hexane to obtain a black-red complex, namely dibenzoylmethane cyclopentadienyl titanium dichloride (CpTi(dbm)Cl2), with a yield (ω) of 86%. The elemental analysis results are: C%: measured value 59.19 (theoretical value 59.01); H%: 3.85 (theoretical value 3.96); Ti%: 11.79 (theoretical value 11.76). 1 HNMR (δ): 4.1 (1H, -CH, singlet); 6.89 (5H, -C5H5, singlet); 7.49-7.55 (10H, -C6H5, multiplet).
[0069] Add 1.15mmol of CpTi(dbm)Cl2 to 30mL of ether, add 0.8mL of methylmagnesium chloride (2M) reagent dropwise, and stir at 25°C for 2h. Remove the ether by rotary evaporation, and wash twice with n-hexane. Remove the n-hexane by rotary evaporation to obtain a red oily product, namely dibenzoylmethane cyclopentadienyl dimethyl titanium (CpTi(dbm)(CH3)2), with a yield of 80%. The results of elemental analysis are: C%: measured value 71.90 (theoretical value 72.14); H%: 5.94 (theoretical value 6.05); Ti%: 13.19 (theoretical value 13.07). 1 HNMR (δ): 0.95 (6H, -CH3, singlet); 4.05 (1H, -CH, singlet); 6.84 (5H, -C5H5, singlet); 7.45-7.51 (10H, -C6H5, multiplet).
[0070] Add 0.5mmol of CpTi(dbm)(CH3)2 to a sample bottle, add 1mL of toluene and stir to dissolve, add tri(pentafluorophenyl)borane (0.6mmol), stir for 0.5h, add 3mL of ether, stir and put in a refrigerator. The precipitated solid was filtered and washed with ether 3 times to obtain catalyst a with a yield of 70%. The elemental analysis results are: C%: measured value 54.91 (theoretical value 54.70); H%: 2.31 (theoretical value 2.52); Ti%: 5.39 (theoretical value 5.45). 1 H NMR (δ): 0.85 (3H, -CH3, singlet); 1.20 (3H, -CH3, singlet) 4.13 (1H; -CH, singlet); 7.02 (5H, -C5H5, singlet); 7.64-7.85 (10H, -C6H5, multiplet).
[0071] Prepare a 0.5 μmol / mL toluene standard solution of catalyst a in a glove box. Take 1 mL of the catalyst solution in the glove box and add it to the catalyst tank. Pump out the nitrogen from the 500 mL jacketed stainless steel high-pressure reactor three times, transfer the catalyst tank out of the glove box and install it on the reactor. Add 250 mL of n-hexane, 100 mL of 1-octene and 2.0 mL of TIBA / Hex solution (triiodobenzoic acid / hexane, 10 μmmol / mL) to the reactor. Raise the temperature to 100°C, adjust the speed to 1000 r / min, and introduce ethylene to a pressure of 5 MPa. After the reaction temperature reaches 125°C, add the catalyst and control the reaction temperature to 140°C. After reacting for 3 minutes, stop introducing ethylene, cool to room temperature, and quench the reaction with ethanol acidified with 5% hydrochloric acid to obtain a polymerization precipitate, wash it three times with ethanol, and dry it in a vacuum. The polymerization results are shown in Table 1. Yield: 37.1 g, density 0.865 g / cm 3, melt index is 15.9g / 10min, Mw molecular weight is 112,000; PDI is 2.3; mass content of 1-octene is 42.23%; catalyst activity: 11.09×10 -7 g / mol Ti.h.
[0072] [Example 2]
[0073] Preparation of catalyst b and its polymerization reaction
[0074]
[0075] The implementation steps are the same as the synthesis of Example 1, but dibenzoylmethane and pentamethylcyclopentadienyltitanium trichloride are used as starting materials to synthesize dibenzoylmethane (pentamethylcyclopentadienyl) dimethyltitanium with a total yield of 48%. The elemental analysis results are: C%: measured value 74.01 (theoretical value 74.31); H%: 7.61 (theoretical value 7.39); Ti%: 10.81 (theoretical value 10.97). 1 H NMR (δ): 0.90 (6H, -CH3, singlet); 2.10 (15H, -CH3, singlet); 3.95 (1H, -CH, singlet); 7.31-7.49 (10H, -C6H5, multiplet).
[0076] Add 0.5mmol of dibenzoylmethane (pentamethylcyclopentadienyl) dimethyltitanium to a sample bottle, add 1mL of toluene and stir to dissolve, add tri(pentafluorophenyl)borane (0.6mmol), stir for 0.5h, add 3mL of ether, stir and put in a refrigerator. The solid was precipitated, filtered, and washed with ether 3 times to obtain catalyst b with a yield of 85%. The results of elemental analysis are: C%: measured value 56.69 (theoretical value 56.99); H%: 3.32 (theoretical value 3.40); Ti%: 5.13 (theoretical value 5.05). 1 H NMR (δ): 0.80 (3H, -CH3, singlet); 1.10 (3H, -CH3, singlet); 2.20 (15H, -CH3, singlet); 4.10 (1H, -CH, singlet); 7.44-7.60 (10H, -C6H5, multiplet).
[0077] Prepare a 0.5 μmol / mL toluene standard solution of catalyst b in a glove box. Take 1 mL of the catalyst solution in the glove box and add it to the catalyst tank. Pump out the nitrogen from the 500 mL jacketed stainless steel high-pressure reactor three times, transfer the catalyst tank out of the glove box and install it on the reactor. Add 250 mL of n-hexane, 100 mL of 1-octene and 2.0 mL of TIBA / Hex solution (10 μmmol / mL) to the reactor. Raise the temperature to 100°C, adjust the speed to 1000 r / min, and introduce ethylene to a pressure of 5 MPa. After the reaction temperature reaches 125°C, add the catalyst and control the reaction temperature to 140°C. After reacting for 3 minutes, stop introducing ethylene, cool to room temperature, and quench the reaction with ethanol acidified with 5% hydrochloric acid to obtain a polymerization precipitate, wash it three times with ethanol, and dry it in a vacuum. The polymerization results are shown in Table 1. Yield: 45.1 g, density 0.862 g / cm 3 , melt index is 15.9g / 10min, Mw molecular weight is 98,000; PDI is 2.3; mass content of 1-octene is 44.1%; catalyst activity: 13.49×10 -7 g / mol Ti.h.
[0078] [Example 3]
[0079] Preparation of catalyst c and its polymerization reaction
[0080]
[0081] The implementation steps are the same as the synthesis of Example 1, but acetylacetone and pentamethylcyclopentadienyl titanium trichloride are used as starting materials to obtain diacetylacetonato (pentamethylcyclopentadienyl) dimethyl titanium, with a total yield of 60%. The elemental analysis results are: C%: measured value 65.52 (theoretical value 65.39); H%: 9.07 (theoretical value 9.04); Ti%: 15.24 (theoretical value 15.33). 1 H NMR (δ): 0.89 (6H, -CH3, singlet); 2.10 (15H, -CH3, singlet); 2.23 (6H, -CH3, singlet); 3.95 (1H, -CH, singlet).
[0082] Add 0.5mmol of diacetylacetonato (pentamethylcyclopentadienyl) dimethyltitanium to a sample bottle, add 1mL of toluene and stir to dissolve, add tri(pentafluorophenyl)borane (0.6mmol) after stirring for 0.5h, add 3mL of ether after stirring for 0.5h, and put it in a refrigerator after stirring. The solid was precipitated, filtered, and washed with ether 3 times to obtain catalyst c with a yield of 83%. The results of elemental analysis are: C%: measured value 50.92 (theoretical value 51.00); H%: 3.37 (theoretical value 3.42); Ti%: 5.84 (theoretical value 5.81). 1HNMR (δ): 0.84 (3H, -CH3, singlet); 1.05 (3H, -CH3, singlet); 2.30 (15H, -CH3, singlet); 2.43 (6H, -CH3, singlet); 4.11 (1H, -CH, singlet).
[0083] Prepare a 0.5 μmol / mL toluene standard solution of catalyst c in a glove box. Take 1 mL of the catalyst solution in the glove box and add it to the catalyst tank. Pump out the nitrogen from the 500 mL jacketed stainless steel high-pressure reactor three times, transfer the catalyst tank out of the glove box and install it on the reactor. Add 250 mL of n-hexane, 100 mL of 1-octene and 2.0 mL of TIBA / Hex solution (10 μmmol / mL) to the reactor. Raise the temperature to 100°C, adjust the speed to 1000 r / min, and introduce ethylene to a pressure of 5 MPa. After the reaction temperature reaches 125°C, add the catalyst and control the reaction temperature to 140°C. After reacting for 3 minutes, stop introducing ethylene, cool to room temperature, and quench the reaction with ethanol acidified with 5% hydrochloric acid to obtain a polymerization precipitate, wash it three times with ethanol, and dry it in a vacuum. The polymerization results are shown in Table 1. Yield: 38.0 g, density 0.871 g / cm 3 , melt index is 15.1g / 10min, Mw molecular weight is 105,000; PDI is 2.7; mass content of 1-octene is 35.1%; catalyst activity: 5.36×10 -7 g / mol Ti.h.
[0084] [Example 4]
[0085] Preparation of catalyst d and its polymerization reaction
[0086]
[0087] The implementation steps are the same as the synthesis of Example 1, but using 3-methyl-1,1'-dibenzoylmethane and pentamethylcyclopentadienyltitanium trichloride as starting materials, 3-methyl-1,1'-dibenzoylmethane (pentamethylcyclopentadienyl) dimethyltitanium is obtained, with a total yield of 50%. The elemental analysis results are: C%: measured value 74.71 (theoretical value 74.66); H%: 7.57 (theoretical value 7.61); Ti%: 10.57 (theoretical value 10.63). 1 H NMR (δ): 0.90 (6H, -CH3, singlet); 2.11 (15H, -CH3, singlet); 2.34 (3H, -CH3, singlet); 7.25-7.40 (10H, C6H5, multiplet).
[0088] Add 0.5mmol of 3-methyl-1,1′-dibenzoylmethane (pentamethylcyclopentadienyl) dimethyltitanium to a sample bottle, add 1mL of toluene and stir to dissolve, add tri(pentafluorophenyl)borane (0.6mmol) after stirring for 0.5h, add 3mL of ether after stirring for 0.5h, and put it in a refrigerator after stirring. The solid was precipitated, filtered, and washed with ether 3 times to obtain catalyst d with a yield of 83%. The results of elemental analysis are: C%: measured value 57.71 (theoretical value 57.41); H%: 3.57 (theoretical value 3.56); Ti%: 5.17 (theoretical value 4.97). 1 H NMR (δ): 0.80 (3H, -CH3, singlet); 1.05 (3H, -CH3, singlet); 2.31 (15H, -CH3, singlet); 2.44 (3H, -CH3, singlet); 7.35-7.51 (10H, C6H5, multiplet).
[0089] Prepare a 0.5 μmol / mL toluene standard solution of catalyst d in a glove box. Take 1 mL of the catalyst solution in the glove box and add it to the catalyst tank. Pump out the nitrogen from the 500 mL jacketed stainless steel high-pressure reactor three times, transfer the catalyst tank out of the glove box and install it on the reactor. Add 250 mL of n-hexane, 80 mL of 1-octene and 2.0 mL of TIBA / Hex solution (10 μmmol / mL) to the reactor. Raise the temperature to 100°C, adjust the speed to 1000 r / min, and introduce ethylene to a pressure of 5 MPa. After the reaction temperature reaches 125°C, add the catalyst and control the reaction temperature to 140°C. After reacting for 3 minutes, stop introducing ethylene, cool to room temperature, and quench the reaction with ethanol acidified with 5% hydrochloric acid to obtain a polymerization precipitate, wash it three times with ethanol, and dry it in a vacuum. The polymerization results are shown in Table 1. Yield: 48.0 g, density 0.885 g / cm 3 , melt index is 16.1g / 10min, Mw molecular weight is 89,000; PDI is 2.5; mass content of 1-octene is 43.35%; catalyst activity: 14.66×10 -7 g / mol Ti.h.
[0090] [Example 5] The same as Example 2, except that octene-1 was replaced by an equal mole of hexene-1. The polymerization results are shown in Table 1.
[0091] [Example 6] The same as Example 2, except that octene-1 was replaced by an equal mole of butene-1 and butene-1 was added continuously. The polymerization results are shown in Table 1.
[0092] [Example 7] The same as Example 2, except that the polymerization temperature was controlled at 160° C. The polymerization results are shown in Table 1.
[0093] [Example 8] The same as Example 2, except that the polymerization temperature was controlled at 180° C. The polymerization results are shown in Table 1.
[0094] [Example 9] The same as Example 2, except that the polymerization temperature was controlled at 200° C. The polymerization results are shown in Table 1.
[0095] [Comparative Example 1] is the same as Example 1, except that the catalyst is replaced with CpTi(dbm)Cl2, the co-catalyst is replaced with methylaluminoxane (MAO), and the Al / Ti ratio is 2000.
[0096] [Comparative Example 2] is the same as Example 3, except that the catalyst is replaced with diacetylacetonate (pentamethylcyclopentadienyl) titanium dichloride, the co-catalyst is replaced with methylaluminoxane (MAO), and the Al / Ti ratio is 2000.
[0097] Table 1. Aggregation results
[0098]
[0099] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A complex represented by formula (I): in, M is selected from titanium, zirconium or hafnium; Cy is selected from the following groups which are unsubstituted or optionally substituted with one, two or more Ra: cyclopentadienyl; R1 is selected from hydrogen, unsubstituted or optionally substituted by one, two or more Rb: 1-6 alkyl; Each R2 is the same or different and is independently selected from hydrogen, the following groups which are unsubstituted or optionally substituted by one, two or more Rb: C 1-6 Alkyl, C 6-8 Aryl; Each R3 is the same or different and is independently selected from C which is unsubstituted or optionally substituted with one, two or more Rc 1-6 alkyl; Each R4 is the same or different and is independently selected from hydrogen, halogen, the following groups which are unsubstituted or optionally substituted by one, two or more Rd: C 6-8 Aryl; Each Ra, Rb, Rc, Rd is the same or different and is independently selected from halogen, C 1-6 alkyl.
2. The complex according to claim 1, characterized in that R1 is selected from hydrogen, C 1-6 alkyl; R2 is selected from C 1-6 Alkyl, C 6-8 Aryl; R3 is selected from C 1-6 alkyl; R4 is selected from C which is unsubstituted or optionally substituted with one, two or more Rd 6-8 Aryl; Each Rd is the same or different and is independently selected from halogen, C 1-6 alkyl.
3. The complex according to claim 1, characterized in that R1 is selected from hydrogen and methyl; R2 is selected from methyl and phenyl; R3 is selected from methyl; R4 is selected from pentafluorophenyl.
4. The complex according to claim 1, characterized in that The complex shown in formula (I) is selected from:
5. A method for preparing the complex according to any one of claims 1 to 4, comprising the following steps: 1) Compound I-2 reacts with R-MgX to obtain compound I-1; 2) Compound I-1 reacts with B(R4)3 to obtain a complex represented by formula (I); Wherein, M, Cy, R1, R2, R3, and R4 have the definitions described in any one of claims 1 to 4; X, X1, and X2 are the same or different and are independently selected from Cl, Br, and I; and R-MgX is selected from methylmagnesium chloride and methylmagnesium bromide.
6. The preparation method according to claim 5, characterized in that: In step 1), the reaction is carried out in an organic solvent, and the organic solvent is selected from at least one of tetrahydrofuran, diethyl ether, methyl tert-butyl ether, dioxane, and 2-methyltetrahydrofuran.
7. The preparation method according to claim 5, characterized in that: In step 2), the reaction is carried out in an organic solvent, and the organic solvent is selected from toluene.
8. The preparation method according to claim 5, characterized in that: In step 2), after the reaction is completed, a purification step is further included, in which the reaction solution is added to a poor solvent to precipitate to obtain a complex shown in formula (I); the poor solvent is selected from at least one of diethyl ether, methyl tert-butyl ether, n-hexane, cyclohexane, and petroleum ether.
9. Use of the complex according to any one of claims 1 to 4 as a catalyst.
10. The use according to claim 9, characterized in that: The catalyst is used for catalyzing the polymerization of ethylene and α-olefins.
11. The use according to claim 9, characterized in that: The catalyst is used for catalyzing the solution copolymerization of ethylene and alpha-olefin to prepare polyethylene elastomer.
12. The use according to claim 10 or 11, characterized in that: The α-olefin is selected from 1-butene, 1-hexene and 1-octene.
13. The use according to claim 10, characterized in that: When the catalyst is used to catalyze the polymerization of ethylene and α-olefin, the polymerization temperature is 100°C-200°C.
14. The use according to claim 10, characterized in that: When the catalyst is used to catalyze the polymerization of ethylene and α-olefin, the polymerization temperature is 120°C to 180°C.
15. The use according to claim 10, characterized in that When the catalyst is used to catalyze the polymerization of ethylene and α-olefin, the polymerization pressure is 1-8 MPa.
16. The use according to claim 10, characterized in that: When the catalyst is used to catalyze the polymerization of ethylene and α-olefin, the polymerization pressure is 2-6 MPa.