A deformation control technology for thin-walled dense flow channel components by laser selective melting

By designing rounded corners and graded support structures in nozzle manufacturing, the problem of large stress deformation of thin-walled close-packed runner structures during laser selective melting and forming is solved, achieving high precision and stability of parts and avoiding warpage and cracking. .

CN115889810BActive Publication Date: 2024-10-01CAPITAL AEROSPACE MACHINERY
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211339082.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-10-01
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

In the existing nozzle manufacturing process, the thin-walled close-packed flow channel structure has technical difficulties such as large stress and deformation during the laser selective melting forming process, resulting in warping and cracking of parts.

Method used

The design process is used to fillet the corners to reduce the stress on the part-substrate joint surface, and the structural deformation is controlled through a hierarchical array of axially symmetric conforming internal support structures, including processing the transition connection zone on the substrate and processing the support structure in the inner cavity of the nozzle, and adjusting the thickness of the transition connection zone and process fillets, and a multi-level support structure designed to reduce stress.

Benefits of technology

It effectively reduces the stress on the contact surface between the part and the substrate, avoids warping and cracking of the nozzle, and achieves high-precision manufacturing and structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115889810B_ABST
    Figure CN115889810B_ABST
Patent Text Reader

Abstract

The present application relates to the field of laser selective melting and specifically discloses a laser selective melting method, including: processing a transition connection area on a substrate through a laser selective melting process; processing a nozzle on the transition connection area through a laser selective melting process, wherein the thickness of the transition connection area corresponds to the axial height of the nozzle; after the nozzle is processed, the transition connection area is removed from the nozzle. The method also includes: in the process of processing the nozzle through the laser selective melting process, processing a support structure in the inner cavity of the nozzle, wherein the support structure is connected to the inner wall of the nozzle; after the nozzle is processed, the support structure is removed from the nozzle. In order to solve the technical problem of large deformation, this patent proposes to control structural deformation by designing process fillets to reduce the stress on the part-substrate interface and using a graded array axisymmetric conformal internal support structure to achieve high-precision manufacturing of parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of laser selective melting forming, and in particular to a deformation control technology for laser selective melting forming of thin-walled closely spaced flow channel components. Background Art

[0002] The nozzle is the guarantee of the specific impulse performance of the rocket engine and one of the key parts that affect the success or failure of the engine. The nozzle is mainly used to expand the high-temperature and high-pressure gas generated in the combustion chamber and then eject it at high speed to generate thrust during engine operation. The inner wall of the nozzle is subjected to high temperature (up to 3000°C), vibration and high-speed (up to several times) gas thermal erosion, and the working conditions are extremely harsh. In order to ensure the stable operation of the nozzle under high temperature conditions, most of the existing rocket engine nozzles adopt a regenerative cooling structure, and the fuel is passed into the interlayer to cool the nozzle. The specific structural forms mainly include spiral variable cross-section tube bundle type and wall plate groove two types of dense flow channel structure. In order to ensure the cooling efficiency, the wall thickness of the inner wall of the nozzle structure is generally less than 1mm. The shape of the nozzle is mostly a bell-shaped or conical structure, and the large end diameter and height are generally above 500mm. The existing manufacturing process generally adopts preformed thin-walled square tube welding or groove-wall plate welding. However, the segmented manufacturing and welding of large-scale thin-walled curved structures such as nozzles has technical limitations such as variable-section bends, long manufacturing cycles for groove inner walls, large welding deformation, and low manufacturing efficiency. Selective Laser Melting (SLM) belongs to the field of additive manufacturing. It uses high-energy lasers to melt loose powder layers, and forms three-dimensional parts with a certain density by layer-by-layer powder laying and layer-by-layer melting and accumulation. Compared with traditional mechanical processing technology, SLM technology can realize the manufacturing of complex thin-walled precision components such as variable cross-sections and complex internal flow channels, and has the advantages of high forming accuracy, good internal quality, excellent mechanical properties, and easy integrated manufacturing. SLM can realize the overall manufacturing of large-scale thin-walled dense flow channel structures such as nozzles, and the segmented manufacturing and welding methods have technical limitations. However, there are also technical difficulties in the SLM forming of such large-scale dense flow channel thin-walled components with large stress deformation. Summary of the invention

[0003] This application provides a deformation control technology for laser selective melting of thin-walled closely packed flow channel components. In order to solve the technical problem of large deformation, this patent proposes to use two methods to control structural deformation: designing process fillets to reduce the stress on the part-substrate interface and using a graded array axisymmetric conformal internal support structure to achieve high-precision manufacturing of parts.

[0004] In a first aspect, a laser selective melting forming method is provided, comprising:

[0005] Through the laser selective melting forming process, the transition connection area is processed on the substrate;

[0006] The nozzle is processed on the transitional connection area by a laser selective melting forming process, and the thickness of the transitional connection area corresponds to the axial height of the nozzle;

[0007] After the nozzle is processed, the transition zone is removed from the nozzle.

[0008] Compared with the prior art, the solution provided by this application includes at least the following beneficial technical effects:

[0009] The nozzle structure is a large-size thin-walled structure for the laser selective melting forming process. It has the characteristics of a large projected area on the forming substrate but a small actual contact area. The shape of the contact surface between the part and the substrate changes suddenly, which will generate increased stress during the forming process, causing the part to warp and crack. Therefore, by adding a transition connection area at the lower end of the part and designing the thickness of the transition connection area, a smooth transition between the substrate and the nozzle is achieved, the stress of the contact surface is reduced, and the nozzle warping and cracking are avoided.

[0010] In combination with the first aspect, in certain implementations of the first aspect, the thickness of the transition zone and the axial height of the nozzle satisfy any of the following:

[0011] The axial height of the nozzle is less than 400 mm, and the thickness of the transition zone is 5 to 15 mm;

[0012] The axial height of the nozzle is 400-800 mm, and the thickness of the transition zone is 15-30 mm;

[0013] The axial height of the nozzle is greater than 800 mm, and the thickness of the transition connection zone is 30 to 50 mm.

[0014] Adjusting the thickness of the transition zone according to the nozzle height helps reduce the stress on the contact surface and avoid nozzle warping and cracking.

[0015] In combination with the first aspect, in some implementations of the first aspect, the method further includes:

[0016] A process fillet is machined on the transition zone by a laser selective melting process. The process fillet is a fillet between the transition zone and the nozzle, and the radius of the process fillet corresponds to the axial height of the nozzle.

[0017] By designing the process fillet of the transition connection area connected to the nozzle, a smooth transition between the substrate and the nozzle is achieved, the stress on the contact surface is reduced, and the warping and cracking of the nozzle is avoided.

[0018] In combination with the first aspect, in certain implementations of the first aspect, the radius of the process fillet and the axial height of the nozzle satisfy any of the following:

[0019] The axial height of the nozzle is less than 400 mm, and the thickness of the transition zone is 3 to 7 mm;

[0020] The axial height of the nozzle is 400-800 mm, and the thickness of the transition zone is 7-15 mm;

[0021] The axial height of the nozzle is greater than 800 mm, and the thickness of the transition connection zone is 15 to 25 mm.

[0022] Adjusting the process radius according to the nozzle height helps reduce the stress on the contact surface and avoid nozzle warping and cracking.

[0023] In combination with the first aspect, in some implementations of the first aspect, the method further includes:

[0024] In the process of processing the nozzle by laser selective melting forming process, a support structure is processed in the inner cavity of the nozzle, and the support structure is connected to the inner wall of the nozzle;

[0025] After the nozzle is processed, the support structure is removed from the nozzle.

[0026] For bell-shaped or conical nozzle structures, due to their high height, they will be affected by forming thermal stress and solidification shrinkage stress during laser selective melting, which will cause concave deformation in the middle of the part. Through the additive manufacturing process, a support structure is machined into the inner cavity of the nozzle during the nozzle processing. The support structure can be an axisymmetric graded array conformal internal support. In view of the concave deformation, the support structure can add an axisymmetric graded array conformal internal support inside during the part process design stage to control the deformation of the component.

[0027] In combination with the first aspect, in certain implementations of the first aspect, a three-level support structure is provided in the nozzle, and the three-level support structure satisfies:

[0028] The first-level support structure is arranged at a position where the nozzle radius is less than 0.1 to 0.2D mm;

[0029] The second-level support structure is arranged at a position where the nozzle radius is 0.15D to 0.5D mm;

[0030] The third-level support structure is arranged at a position where the radius of the nozzle is 0.5D to D mm, wherein D is the difference between the radius of the large end and the radius of the small end of the nozzle.

[0031] Designing and arranging multi-level support structures according to the nozzle radius is conducive to achieving reasonable control of component deformation.

[0032] In combination with the first aspect, in certain implementations of the first aspect, a length ratio of the first-level support structure, the second-level support structure, and the third-level support structure is 4:2:1.

[0033] Designing and arranging multi-level support structures according to the nozzle height is conducive to achieving reasonable control of component deformation.

[0034] In combination with the first aspect, in certain implementations of the first aspect, a diameter ratio of the first-level support structure, the second-level support structure, and the third-level support structure is 1:2:4.

[0035] Reasonable design of the dimensions of the multi-level support structure is conducive to achieving reasonable control of component deformation.

[0036] In combination with the first aspect, in some implementations of the first aspect, the number ratio of the first-level support structure, the second-level support structure, and the third-level support structure is 1:2:4.

[0037] Reasonable design of the number of multi-level support structures is conducive to achieving reasonable control of component deformation.

[0038] In combination with the first aspect, in certain implementations of the first aspect, the angle between two adjacent first-level support structures is 45°, the angle between two adjacent second-level support structures is 30°, and the angle between two adjacent third-level support structures is 15°.

[0039] Reasonable design of the arrangement of multi-level support structures is conducive to the reasonable control of component deformation. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A schematic structural diagram of a nozzle.

[0041] Figure 2 It is a schematic structural diagram of a nozzle flow channel.

[0042] Figure 3 A schematic diagram of a component obtained by a laser selective melting forming method provided in an embodiment of the present application.

[0043] Figure 4 A structural schematic diagram of a support structure provided in an embodiment of the present application.

[0044] Figure 5 A structural schematic diagram of a support structure provided in an embodiment of the present application.

[0045] Figure 6 A structural schematic diagram of a support structure provided in an embodiment of the present application. DETAILED DESCRIPTION

[0046] The present application is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0047] Figure 1 is a schematic structural diagram of a nozzle provided in an embodiment of the present application. The nozzle may have two open ends, and the two open ends may be a small end and a large end respectively. The distance between the small end and the large end is the axial height of the nozzle. The material of the nozzle may be titanium alloy, high temperature alloy, stainless steel, etc. Figure 2 As shown, the nozzle may be provided with a flow channel structure. The characteristic form of the flow channel structure may be a spiral flow channel, a straight flow channel, etc., and the flow channel wall thickness is greater than or equal to 0.6 mm.

[0048] The present application embodiment is directed to Figure 1 or Figure 2 The nozzle shown controls deformation during laser selective melting through substrate and process fillet design.

[0049] The nozzle structure is a large-size thin-walled structure for the laser selective melting forming process. It has the characteristics of a large projected area on the forming substrate but a small actual contact area. The shape of the contact surface between the part and the substrate changes suddenly, which will generate increased stress during the forming process, causing the part to warp and crack. Therefore, through the additive manufacturing process, a transition connection zone is processed on the substrate. The transition connection zone is the transition zone between the substrate and the nozzle, and the transition connection zone is connected between the substrate and the nozzle. By adding a transition connection zone at the lower end of the part and designing the thickness of the transition connection zone, as well as the process fillet of the transition connection zone connected to the nozzle, a smooth transition between the substrate and the nozzle is achieved, reducing the stress on the contact surface and avoiding warping and cracking of the nozzle. Specifically, Figure 2 The thickness of the transition zone and the specific parameters of the process fillet may be related to the axial height of the nozzle. For details, please refer to Table 1.

[0050] The transition zone can be a cubic structure, and the projection area of ​​the nozzle can be located within the projection area of ​​the transition zone along the center line of the nozzle. After the nozzle is processed, the transition zone can be removed from the nozzle.

[0051] Table 1 Thickness of transition zone and specific parameters of process fillet

[0052] Component model X Y Z Axis height of component <400mm 400-800mm 800-1000 Thickness of transition zone 10mm 20mm 40mm Process rounded corners 5mm 10mm 20mm

[0053] For bell-shaped or conical nozzle structures, due to their high height, they will be affected by the forming thermal stress and solidification shrinkage stress during laser selective melting, which will cause concave deformation in the middle of the part. Through the additive manufacturing process, during the nozzle processing, a support structure is processed in the inner cavity of the nozzle. The support structure can be an axisymmetric graded array conformal internal support. The embodiment of the present application is directed to Figure 1 or Figure 2The nozzle shown in FIG. 1 also controls the deformation of the nozzle's large-scale thin-walled dense flow channel structure by laser selective melting through the design of a graded array axisymmetric conformal internal support structure. Figure 4 and Figure 5 The support structure can be used to control the deformation of the component by adding an axisymmetric graded array conformal internal support in the part process design stage to target the concave deformation.

[0054] The support structure can be connected to the inner wall of the nozzle. The central symmetry axis of the support structure coincides with the component axis. The support structure can be symmetrically arranged relative to the central axis of the nozzle and vertically arranged relative to the central axis of the nozzle.

[0055] Combination Figure 1 The number of levels of graded array support is determined according to the size of the small end and the large end of the component. Determine the value of D in the range of large end radius-small end radius. Specifically, when the D value is less than 100mm, the support grade number is 1, close to the small end of the component, and the support structure diameter is 1mm; when D is 100-300mm, the support grade number is 2, located in the transition section of the component, and the support structure diameter is 2mm: when D is 300-600mm, the support grade number is 3, close to the large end of the component, and the support structure diameter is 4mm.

[0056] The dimensional characteristics of the conformal internal supports of the axisymmetric graded array are as follows: the one close to the middle axis is defined as level 1, and the ratio of the widths of each level is 1:2:4; the ratio of the lengths of the support structures (the ratio of the distances from the support structure to the large end opening along the center line of the nozzle) is 4:2:1. Level 1 supports are symmetrically distributed along the central axis, with a support quantity a, close to the small end of the component; level 2 supports are symmetrically distributed along the central axis, with a support quantity 2a, located in the transition section of the component; level 3 supports are symmetrically distributed along the central axis, with a support quantity 4a, close to the large end of the component.

[0057] Table 2 Internal support structure design table

[0058]

[0059] Level 1, 2 and 3 supports are divided into three directions, with angles of θ being 15, 30 and 45 degrees. That is, level 1 supports can be set at 45° intervals, and level 1 supports at 45° intervals. Level 2 supports can be set at 30° intervals, and level 2 supports at 30° intervals. Level 3 supports can be set at 15° intervals, and level 3 supports at 15° intervals. See Table 3 above for details. The height of the inner support fits the inside of the nozzle. Figure 6 .

[0060] Table 3 Internal support structure angle transformation design table

[0061]

[0062] This application is further described in detail in conjunction with the following contents.

[0063] Example 1

[0064] Nozzle A: The axial height of the component is 600 mm; the designed connection thickness with the substrate is 20 mm, and the process fillet is 10 mm; as shown in Table 4.

[0065] Table 4 Substrate and process fillet

[0066]

[0067]

[0068] D = large end radius - small end radius = 600 mm. The graded array support design is shown in Table 5.

[0069] Table 5 Specific design table of internal support structure

[0070]

[0071] Example 2

[0072] Nozzle B: The axial height of the component is 900 mm; the designed connection thickness with the substrate is 40 mm, and the process radius is 20 mm; as shown in Table 6.

[0073] Table 6 Substrate and process fillet

[0074] Component model B Axis height of component 900mm Thickness of substrate connection 40mm Process rounded corners 20mm

[0075] D = large end radius - small end radius = 900 mm. The graded array support design is shown in Table 7.

[0076] Table 7 Specific design table of internal support structure

[0077]

[0078]

[0079] Although the present invention is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the claims of the present invention.

Claims

1. A laser selective melting forming method, characterized in that: include: Through the laser selective melting forming process, the transition connection area is processed on the substrate; The nozzle is processed on the transition connection area by a laser selective melting forming process, the thickness of the transition connection area corresponds to the axial height of the nozzle, and the nozzle has two open ends, which are a small end and a large end respectively, and the distance between the small end and the large end is the axial height of the nozzle; After the nozzle is processed, removing the transition zone from the nozzle; In the process of processing the nozzle by the laser selective melting forming process, a support structure is processed in the inner cavity of the nozzle, the support structure is connected to the inner wall of the nozzle, and the height of the support structure is in conformity with the shape of the interior of the nozzle; After the nozzle is processed, removing the support structure from the nozzle; A three-level support structure is provided in the nozzle, and the three-level support structure meets the following requirements: The first-level support structure is arranged at a position where the nozzle radius is less than 0.1Dmm; The second-level support structure is arranged at a position where the nozzle radius is 0.15D~0.5Dmm; The third-level support structure is arranged at a position where the radius of the nozzle is 0.5D~Dmm, wherein D is the difference between the radius of the large end and the radius of the small end of the nozzle; The length ratio of the first-level support structure, the second-level support structure and the third-level support structure is 4:2:1, the length of the support structure is the distance from the support structure to the large end opening along the center line of the nozzle, the diameter ratio of the first-level support structure, the second-level support structure and the third-level support structure is 1:2:4, the number ratio of the first-level support structure, the second-level support structure and the third-level support structure is 1:2:4, the angle between two adjacent first-level support structures is 45°, the angle between two adjacent second-level support structures is 30°, and the angle between two adjacent third-level support structures is 15°; The thickness of the transition zone and the axial height of the nozzle satisfy any of the following: The axial height of the nozzle is less than 400 mm, and the thickness of the transition zone is 5 to 15 mm; The axial height of the nozzle is 400-800 mm, and the thickness of the transition zone is 15-30 mm; The axial height of the nozzle is greater than 800 mm, and the thickness of the transition connection zone is 30-50 mm.

2. The method according to claim 1, characterized in that The method further comprises: A process fillet is machined on the transition zone by a laser selective melting process. The process fillet is a fillet between the transition zone and the nozzle. The radius of the process fillet corresponds to the axial height of the nozzle. The radius of the process fillet and the axial height of the nozzle satisfy any of the following conditions: The axial height of the nozzle is less than 400 mm, and the radius of the process fillet is 3 to 7 mm; The axial height of the nozzle is 400-800 mm, and the radius of the process fillet is 7-15 mm; The axial height of the nozzle is greater than 800 mm, and the radius of the process fillet is 15-25 mm.

Citation Information

Patent Citations

  • Shape follow-up support deformation control method for selective laser melting forming of thin-walled part

    CN108372298A

  • Method for forming inclined Y-shaped crossed rib structure through wire and arc additive manufacturing

    CN109317781A

  • Residual stress control method used in thin-wall special-shaped metal member material additive manufacturing process

    CN111318701A

  • High-precision selective laser melting forming method for cooling body part

    CN112570730A

  • Method for producing hollow, large dimensional turbomachine components

    CN112955267A