Catalyst composition, catalyst for preparing polyester, and preparation method and application thereof

By using catalyst compositions containing titanium, magnesium, zinc, hydroxyl and carboxyl compounds in the titanium catalytic system, the problems of uncontrollable catalytic activity and poor selectivity are solved, and efficient and low-cost catalyst preparation is achieved, with high molecular weight and hue phase of the product Excellent, with significant industrial application potential.

CN115894885BActive Publication Date: 2024-11-19POLYCARBONATE OXYGEN NEW MATERIAL TECH (WUXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210304879.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-23
Publication Date
2024-11-19
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

In industrial production, the existing titanium catalytic system has problems such as uncontrollable catalytic activity, poor selectivity, high equipment requirements and large waste liquid volume in the production of industrial products, resulting in low molecular weight, hue difference and wide molecular weight distribution.

Method used

Using a catalyst composition, including titanium, magnesium, zinc, hydroxyl and carboxyl compounds, a catalyst is prepared through specific reaction steps and conditions to ensure that the catalytic reaction activity is controllable and selective, the resin is bright in color and has a high molecular weight. The molecular weight distribution is narrow.

Benefits of technology

It realizes simple configuration of catalysts and efficient preparation under mild conditions, controllable catalytic reaction activity and excellent selectivity, high molecular weight and excellent hue, and has huge industrial application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003561046520000071
    Figure BDA0003561046520000071
  • Figure BDA0003561046520000081
    Figure BDA0003561046520000081
Patent Text Reader

Abstract

The present invention relates to a catalyst composition and a catalyst for preparing polyester prepared by using the catalyst composition as a raw material. The catalyst composition of the present invention comprises at least one titanium-containing compound, at least one magnesium-containing compound, at least one zinc-containing compound, at least one hydroxyl-containing compound and at least one carboxyl-containing compound. The catalyst of the present invention has controllable catalytic reaction activity and excellent selectivity. Not only is the obtained resin white and bright in color, high in molecular weight and narrow in molecular weight distribution, but also the catalyst configuration process is simple, the configuration conditions are mild, the raw material cost is low, and it has huge industrial application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst preparation and application, in particular to a catalyst composition, a catalyst for preparing polyester, and a preparation method and application thereof. Technical Background

[0002] Polyester catalytic systems are divided into antimony, titanium, and germanium systems. Antimony catalytic systems are gradually being abandoned due to their ecotoxicity, while germanium catalytic systems are difficult to industrialize due to their high cost. Titanium catalytic systems are green, environmentally friendly, and inexpensive, and have the potential for industrial application. Currently, the titanium catalytic systems used for the industrial production of aliphatic-aromatic copolyesters have the following problems: 1. Uncontrollable catalytic activity (low catalytic activity cannot meet polymerization production requirements, which is manifested as a low product molecular weight; high catalytic activity leads to local overreaction, which is manifested as a wide product molecular weight distribution); 2. Poor catalytic selectivity, many side reactions, and poor product quality (manifested as poor resin hue, red or yellow, i.e., high a and b values).

[0003] Patent CN103333328A discloses a method for preparing a silicon-titanium composite catalyst. This catalyst can shorten the reaction cycle and produce resins with good hue and high molecular weight. However, the catalyst preparation process requires high temperature and high vacuum conditions, which places high demands on equipment and generates waste gas and waste liquid. Currently, there are few reports of titanium-based catalysts with controllable catalytic activity and excellent selectivity for industrial application. Summary of the Invention

[0004] To address the challenges of existing titanium catalyst systems, such as stringent preparation conditions and high levels of waste gas and liquid, the present invention provides a catalyst composition and a catalyst for preparing polyester using this catalyst composition as raw material. This catalyst features a simple preparation process, mild preparation conditions, and low raw material costs. Furthermore, the catalyst exhibits controllable catalytic activity and excellent selectivity. The resulting resin exhibits bright white color, high molecular weight, and a narrow molecular weight distribution, demonstrating significant potential for industrial application.

[0005] In a first aspect, the present invention provides a catalyst composition comprising at least one titanium-containing compound, at least one magnesium-containing compound, at least one zinc-containing compound, at least one hydroxyl-containing compound, and at least one carboxyl-containing compound.

[0006] According to some embodiments of the present invention, the titanium-containing compound is selected from the general formula (I) Ti(OR 1 ) m X 4-m One or more of the compounds and titanium oxides shown, wherein R 1 C2-C 10 wherein X is a halogen, such as chlorine, bromine or iodine; and m is an integer from 0 to 4, such as 0, 1, 2, 3 or 4.1 C2-C 10 In some embodiments, R 1 is a C2-C6 hydrocarbon group. 1 is a C2-C6 alkyl group, for example, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl or hexyl.

[0007] According to some embodiments of the present invention, the titanium-containing compound is selected from one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, tetraethyl titanate, tetraisopropyl titanate, tetrabutyl titanate and titanium dioxide.

[0008] According to some embodiments of the present invention, the magnesium-containing compound is selected from the general formula (II) Mg(OR 2 )2X 2-n The compound shown and the general formula (III) Mg(OOR 3 ) One or more compounds shown in 2, wherein R 2 C2-C 10 wherein X is a halogen, such as chlorine, bromine or iodine; n is an integer from 0 to 2, such as 0, 1 or 2; R 3 C2-C 20 In some embodiments, R 2 C2-C 10 In some embodiments, R 2 is a C2-C6 hydrocarbon group. 2 is a C2-C6 alkyl group, such as ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl or hexyl. 3 C2-C 10 In some embodiments, R 3 is a C2-C6 hydrocarbon group. 3 is a C2-C6 alkyl group, for example, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl or hexyl.

[0009] According to some embodiments of the present invention, the magnesium-containing compound is selected from one or more of magnesium dichloride, magnesium dibromide, magnesium diiodide, diethoxymagnesium, dipropoxymagnesium, diisopropoxymagnesium, dibutoxymagnesium, diisobutoxymagnesium, magnesium acetate, magnesium propionate and magnesium butyrate.

[0010] According to some embodiments of the present invention, the zinc-containing compound is selected from the general formula (IV) Zn(OOR 4 ) 2 and one or more of the compounds and zinc halides, the general formula (IV) Zn (OOR4 )2, R 4 C2-C 10 In some embodiments, R 4 C2-C 10 In some embodiments, R 4 is a C2-C6 hydrocarbon group. 4 is a C2-C6 alkyl group, for example, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl or hexyl.

[0011] According to some embodiments of the present invention, the zinc-containing compound is selected from one or more of zinc dichloride, zinc dibromide, zinc diiodide, zinc acetate, zinc propionate and zinc butyrate.

[0012] According to some embodiments of the present invention, the hydroxyl-containing compound is selected from one or more of a monohydric alcohol and a polyhydric alcohol. 10 In some embodiments, the polyol is a 2-6 hydration alcohol, such as C2-C 10 diols, C3-C 15 triols, C4-C 20 Tetrahydric alcohol, C5-C 20 Pentahydric alcohol or C6-C 20 of hexavalent alcohol.

[0013] According to some embodiments of the present invention, the hydroxyl-containing compound is selected from one or more of methanol, ethanol, isopropanol, n-butanol, ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, pentaerythritol and sorbitol.

[0014] According to some embodiments of the present invention, the carboxyl-containing compound is selected from one or more of monocarboxylic acids and polycarboxylic acids. 20 Monocarboxylic acids, such as C1-C 10 Monocarboxylic acids, C1-C6 monocarboxylic acids, C 12 -C 20 Monocarboxylic acid or C 15 -C 20 In some embodiments, the polycarboxylic acid is C2-C 20 dicarboxylic acids or C3-C 20 In some embodiments, the polycarboxylic acid is C2-C 10 In some embodiments, the polycarboxylic acid is a C2-C6 dicarboxylic acid.

[0015] According to some embodiments of the present invention, the carboxyl-containing compound is selected from at least one of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, stearic acid, oxalic acid, malonic acid, succinic acid, glutaric acid and adipic acid.

[0016] In a second aspect, the present invention provides a catalyst for preparing polyester, which is prepared by raw materials including the catalyst composition described in the first aspect or includes the reaction product of the components in the catalyst composition described in the first aspect.

[0017] In some embodiments, the concentration of titanium in the catalyst is 1 to 10 wt%, such as 1.5 wt%, 2.0 wt%, 2.5 wt%, 3.0 wt%, 3.5 wt%, 4.0 wt%, 4.5 wt%, 5.0 wt%, 5.5 wt%, 6.0 wt%, 6.5 wt%, 7.0 wt%, 7.5 wt%, 8.0 wt%, 8.5 wt%, 9.0 wt%, 9.5 wt%, or any value therebetween. In some embodiments, the concentration of titanium in the catalyst is 3 to 10 wt%.

[0018] In a third aspect, the present invention provides a method for preparing the catalyst for preparing polyester according to the second aspect, comprising:

[0019] Step A: reacting a portion of the hydroxyl group-containing compound with the carboxyl group-containing compound to obtain a first solution;

[0020] Step B: adding the remaining portion of the hydroxyl-containing compound, the magnesium-containing compound, the zinc-containing compound, and the titanium-containing compound to the first solution of step A, and reacting to obtain a second solution.

[0021] According to some embodiments of the present invention, the method further comprises step C: allowing the second solution to stand and mature for 5-24 hours.

[0022] According to some embodiments of the present invention, in step A, the reaction temperature is 60-200°C, for example, 70°C, 90°C, 100°C, 110°C, 130°C, 150°C, 170°C, 190°C, or any value therebetween. In some embodiments, in step A, the reaction time is 0.5-5 hours, for example, 1 hour, 2 hours, 3 hours, or 4 hours. In some embodiments, in step B, the reaction temperature is 40-100°C, for example, 50°C, 60°C, 70°C, 80°C, 90°C, or any value therebetween. In some embodiments, in step B, the reaction time is 0.5-5 hours, for example, 1 hour, 2 hours, 3 hours, or 4 hours. In some embodiments, in step C, the aging temperature is 20-60°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, or any value therebetween. In some embodiments, in step C, the aging time is 5-24 hours, for example, 7 hours, 9 hours, 10 hours, 13 hours, 15 hours, 17 hours, 19 hours, 20 hours or 22 hours.

[0023] According to some embodiments of the present invention, the amount of the magnesium-containing compound is 0.01-10 moles, for example, 0.05 moles, 0.1 moles, 0.3 moles, 0.5 moles, 0.7 moles, 0.9 moles, 1.5 moles, 2.0 moles, 3.0 moles, 4.0 moles, 5.0 moles, 6.0 moles, 7.0 moles, 8.0 moles, 9.0 moles, or any value therebetween, calculated per mole of the titanium-containing compound. In some embodiments, the amount of the magnesium-containing compound is 0.2-1 mole, calculated per mole of the titanium-containing compound.

[0024] In some embodiments, the zinc-containing compound is present in an amount of 0.01-10 moles, such as 0.05 moles, 0.1 moles, 0.3 moles, 0.5 moles, 0.7 moles, 0.9 moles, 1.5 moles, 2.0 moles, 3.0 moles, 4.0 moles, 5.0 moles, 6.0 moles, 7.0 moles, 8.0 moles, 9.0 moles, or any value therebetween, per mole of the titanium-containing compound. In some embodiments, the zinc-containing compound is present in an amount of 0.1-1 mole, per mole of the titanium-containing compound.

[0025] In some embodiments, the hydroxyl-containing compound is present in an amount of 1 to 20 moles, such as 1.5 moles, 2.0 moles, 2.5 moles, 3.0 moles, 3.5 moles, 4.0 moles, 4.5 moles, 6.0 moles, 7.0 moles, 8.0 moles, 10.0 moles, 12.0 moles, 14.0 moles, 16.0 moles, 18.0 moles, or any value therebetween, calculated per mole of the titanium-containing compound. In some embodiments, the hydroxyl-containing compound is present in an amount of 1 to 5 moles, calculated per mole of the titanium-containing compound.

[0026] In some embodiments, the carboxyl-containing compound is present in an amount of 0.01-0.5 moles, such as 0.05 moles, 0.07 moles, 0.09 moles, 0.15 moles, 0.20 moles, 0.25 moles, 0.30 moles, 0.35 moles, 0.40 moles, 0.45 moles, or any value therebetween, calculated per mole of the titanium-containing compound. In some embodiments, the carboxyl-containing compound is present in an amount of 0.1-0.5 moles, calculated per mole of the titanium-containing compound.

[0027] In some embodiments, the concentration of titanium in the second solution is 1 to 10 wt %, for example, 1.5 wt %, 2.0 wt %, 2.5 wt %, 3.0 wt %, 3.5 wt %, 4.0 wt %, 4.5 wt %, 5.0 wt %, 5.5 wt %, 6.0 wt %, 6.5 wt %, 7.0 wt %, 7.5 wt %, 8.0 wt %, 8.5 wt %, 9.0 wt %, 9.5 wt %, or any value therebetween. In some embodiments, the concentration of titanium in the second solution is 3 to 10 wt %.

[0028] In a fourth aspect, the present invention provides use of the catalyst composition described in the first aspect, the catalyst described in the second aspect, or the catalyst prepared by the preparation method described in the third aspect in the preparation of polyester.

[0029] According to some embodiments of the present invention, the polyester is selected from aliphatic-aromatic copolyesters. In some embodiments, the monomer raw materials for preparing the copolyester include aliphatic dibasic acid, aromatic dibasic acid and aliphatic diol. In some embodiments, the aliphatic dibasic acid is selected from C2-C 16 In some embodiments, the aromatic dibasic acid is selected from terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid and one or more of its anhydrides and acyl halides. In some embodiments, the aliphatic diol is selected from C2-C 10 One or more diols.

[0030] The present invention combines magnesium-containing compounds, zinc-containing compounds, and titanium-containing compounds, and disperses the resulting product from the reaction of a hydroxyl-containing compound with a carboxyl-containing compound to ensure catalyst activity and selectivity. The catalyst boasts a simple preparation process, mild preparation conditions, and low raw material costs, and has significant potential for industrial application. DETAILED DESCRIPTION

[0031] The present invention will be further described below with reference to specific examples, but the scope of the present invention is not limited thereto.

[0032] The polymer hue is tested using the CIE 1976 L*a*b* color system. The specific test is carried out in accordance with 5.5.2 of GB / T 14190-2008.

[0033] The molecular weight and molecular weight distribution of the polymer were determined by gel permeation chromatography using chloroform as solvent, Waters-e2695 instrument, and polystyrene as standard.

[0034] Example 1

[0035] 54.9 g of 1,4-butanediol and 3.4 g of acetic acid were added to the reactor in sequence, and heated at 90°C for 0.5 h to obtain a transparent solution A1; then 10.1 g of butanol, 5.2 g of ethanol, 5.2 g of magnesium bromide, 7.9 g of zinc bromide, and 26.9 g of titanium tetrachloride were added in sequence, stirred evenly, and heated at 60°C for 2 h to obtain a transparent solution B1. After standing and aging at 50°C for 12 h, a catalyst solution C1 was obtained.

[0036] Example 2

[0037] 36.0 g of ethylene glycol and 8.2 g of adipic acid were added to the reactor, and the mixture was heated at 110°C for 1 h to obtain a transparent solution A2; then 10.1 g of propanol, 5.2 g of ethanol, 9.3 g of magnesium butoxide, 4.8 g of zinc chloride, and 11.6 g of titanium dioxide were added in sequence, stirred evenly, and heated at 90°C for 3 h to obtain a solution B2; after standing and aging at 40°C for 20 h, a catalyst solution C2 was obtained.

[0038] Example 3

[0039] 32.7 g of 1,3-propylene glycol and 16.0 g of stearic acid were added to the reactor, and the mixture was heated at 180°C for 2 h to obtain a transparent solution A3. Then, 10.2 g of sorbitol, 7.8 g of magnesium acetate, 11.2 g of zinc iodide, and 41.1 g of tetraisopropyl titanate were added in sequence, stirred evenly, and heated at 80°C for 4 h to obtain a transparent solution B3. After standing and aging at 25°C for 24 h, a catalyst solution C3 was obtained.

[0040] Example 4

[0041] 31.6 g of 1,5-pentanediol and 7.2 g of succinic acid were added to the reactor, and the mixture was heated at 135°C for 1 h to obtain a transparent solution A4; then 10.1 g of pentaerythritol, 5.2 g of ethanol, 7.8 g of magnesium acetate, 7.9 g of zinc acetate, and 49.2 g of tetrabutyl titanate were added in sequence, stirred evenly, and heated at 70°C for 3 h to obtain a transparent solution B4; after standing and aging at 30°C for 20 h, a catalyst solution C4 was obtained.

[0042] Example 5

[0043] 54.9 g of 1,4-butanediol, 10.1 g of butanol, 5.2 g of ethanol, and 3.4 g of acetic acid were added to the reactor in sequence, and heated at 90°C for 0.5 h to obtain a transparent solution A1-5; then 5.2 g of magnesium bromide, 7.9 g of zinc bromide, and 26.9 g of titanium tetrachloride were added in sequence, stirred evenly, and heated at 60°C for 2 h to obtain a transparent solution B1-5. After standing and aging at 50°C for 12 h, a catalyst solution C1-5 was obtained.

[0044] Comparative Example 1

[0045] 68.1 g of 1,4-butanediol and 3.4 g of acetic acid were added to the reactor in sequence, and heated at 90°C for 0.5 h to obtain a transparent solution A5. Then, 10.1 g of butanol, 5.2 g of ethanol, and 26.9 g of titanium tetrachloride were added in sequence, stirred evenly, and heated at 60°C for 2 h to obtain a transparent solution B5. After standing and aging at 50°C for 12 h, a catalyst solution C5 was obtained.

[0046] Comparative Example 2

[0047] 62.8 g of 1,4-butanediol and 3.4 g of acetic acid were added to the reactor in sequence, and heated at 90°C for 0.5 h to obtain a transparent solution A6. Then, 10.1 g of butanol, 5.2 g of ethanol, 26.9 g of titanium tetrachloride, and 5.2 g of magnesium bromide were added in sequence, stirred evenly, and heated at 60°C for 2 h to obtain a transparent solution B6. After standing and aging at 50°C for 12 h, a catalyst solution C6 was obtained.

[0048] Comparative Example 3

[0049] 60.1 g of 1,4-butanediol and 3.4 g of acetic acid were added to the reactor in sequence, and heated at 90°C for 0.5 h to obtain a transparent solution A7; then 10.1 g of butanol, 5.2 g of ethanol, 26.9 g of titanium tetrachloride, and 7.9 g of zinc bromide were added in sequence, stirred evenly, and heated at 60°C for 2 h to obtain a transparent solution B7. After standing and aging at 50°C for 12 h, a catalyst solution C7 was obtained.

[0050] Comparative Example 4

[0051] 58.3 g of 1,4-butanediol was added to the reactor in sequence. After heating at 90°C for 0.5 h, 10.1 g of butanol, 5.2 g of ethanol, 26.9 g of titanium tetrachloride, 5.2 g of magnesium bromide and 7.9 g of zinc bromide were added in sequence. The mixture was stirred and heated at 60°C for 2 h to obtain a transparent solution B7. After standing and aging at 50°C for 12 h, a catalyst solution C8 was obtained.

[0052] Comparative Example 5

[0053] In the existing industrial polyester titanium catalyst preparation process, 41.1 g of tetraisopropyl titanate and 113.7 g of 1,4-butanediol were added to the reactor in sequence, heated and stirred at 60°C for 2 hours to disperse evenly, and then allowed to stand and mature at 50°C for 12 hours to obtain catalyst solution C9.

[0054] Preparation Example

[0055] The catalysts of the above examples and comparative examples were used to catalyze the preparation of biodegradable fatty-aromatic copolyesters. The specific preparation method was as follows: 6.30 kg of terephthalic acid, 6.00 kg of adipic acid, 11.40 kg of 1,4-butanediol, and 33.20 g of catalyst were added to the reactor in sequence, and an esterification reaction was carried out at a temperature of 230° C. until no more water was produced in the system, and the esterification reaction was completed. Then, a pre-polycondensation reaction was carried out at a temperature of 240° C. and a pressure of 4 kPa for 2 hours, and then a final polycondensation reaction was carried out at a pressure of ≤100 Pa. When the torque of the polymerization stirrer was appropriate, the polycondensation reaction was completed to obtain 16.6 kg of a polyester intermediate, which was fully mixed with 83 g of butyl ether and 132.8 g of ethyl zinc, and a chain growth reaction was carried out at 40° C. to obtain a polyester product after 4 hours.

[0056] The specific resin performance parameters are shown in Table 1 below:

[0057] Table 1

[0058]

[0059]

[0060] Note: The higher the a and b values, the worse the resin hue.

[0061] In summary, the catalyst of the present invention has controllable catalytic activity and excellent selectivity in the preparation of biodegradable polyester, which is specifically manifested in that the prepared aliphatic-aromatic copolyester has excellent hue (a value ≤ 3 and b value ≤ 8) and high molecular weight, i.e., a mass average molecular weight of 9.1-15.0×10 4 , molecular weight distribution 1.8-2.2.

[0062] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation of the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein. On the contrary, the present invention can be extended to all other methods and applications with the same function.

Claims

1. Use of a catalyst in the preparation of polyester, wherein the catalyst is prepared from a raw material of a catalyst composition comprising at least one titanium-containing compound, at least one magnesium-containing compound, at least one zinc-containing compound, at least one hydroxyl-containing compound and at least one carboxyl-containing compound, or comprises a reaction product of the components in the catalyst composition; in, The polymer hue of the polyester has an a value of ≤3, a b value of ≤8, and a mass average molecular weight of 9.1-15.0×10 4 , the molecular weight distribution is 1.8-2.2, and the polymer hue is the polymer hue tested by CIE1976 L*a*b* color system; The titanium-containing compound is selected from one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, tetraethyl titanate, tetraisopropyl titanate, tetrabutyl titanate and titanium dioxide; The magnesium-containing compound is selected from one or more of magnesium dichloride, magnesium dibromide, magnesium diiodide, diethoxymagnesium, dipropoxymagnesium, diisopropoxymagnesium, dibutoxymagnesium, diisobutoxymagnesium, magnesium acetate, magnesium propionate and magnesium butyrate; The magnesium-containing compound is selected from one or more of magnesium dichloride, magnesium dibromide, magnesium diiodide, diethoxymagnesium, dipropoxymagnesium, diisopropoxymagnesium, dibutoxymagnesium, diisobutoxymagnesium, magnesium acetate, magnesium propionate and magnesium butyrate; The magnesium-containing compound is selected from one or more of magnesium dichloride, magnesium dibromide, magnesium diiodide, diethoxymagnesium, dipropoxymagnesium, diisopropoxymagnesium, dibutoxymagnesium, diisobutoxymagnesium, magnesium acetate, magnesium propionate and magnesium butyrate; The magnesium-containing compound is selected from one or more of magnesium dichloride, magnesium dibromide, magnesium diiodide, diethoxymagnesium, dipropoxymagnesium, diisopropoxymagnesium, dibutoxymagnesium, diisobutoxymagnesium, magnesium acetate, magnesium propionate and magnesium butyrate; The catalyst is prepared by a preparation method comprising the following steps: Step A: reacting a portion of the hydroxyl group-containing compound with the carboxyl group-containing compound to obtain a first solution; Step B: adding the remaining part of the hydroxyl-containing compound, the magnesium-containing compound, the zinc-containing compound, and the titanium-containing compound to the first solution of step A to react to obtain a second solution; The preparation method of the polyester is as follows: terephthalic acid, adipic acid, 1,4-butanediol and a catalyst are sequentially added into a reactor, an esterification reaction is carried out at a temperature of 230° C., the esterification reaction is terminated when no more water is produced in the system, and then a pre-polycondensation reaction is carried out at a temperature of 240° C. and a pressure of 4KPa for 2 hours, and then a final polycondensation reaction is carried out at a pressure of ≤100Pa, and when the torque of the polymerization stirrer is appropriate, the polycondensation reaction is terminated to obtain a polyester intermediate, which is mixed with butyl ether and ethyl zinc, and a chain growth reaction is carried out at 40° C. to obtain a polyester product after 4 hours.

2. The use according to claim 1, It is characterized in that The preparation method further comprises step C: allowing the second solution to stand and mature for 5-24 hours.

3. The use according to claim 1, It is characterized in that In step A, the reaction temperature is 60-200° C. and the reaction time is 0.5-5 h. In step B, the reaction temperature is 40-100° C. and the reaction time is 0.5-5 h.

4. The use according to claim 1, It is characterized in that Calculated per mole of titanium-containing compound, the magnesium-containing compound is 0.01-10 moles, the zinc-containing compound is 0.01-10 moles, the hydroxyl-containing compound is 1-20 moles, the carboxyl-containing compound is 0.01-0.5 moles, and the concentration of titanium element in the second solution is 1-10wt%.

5. The use according to claim 4, It is characterized in that The magnesium-containing compound is 0.2-1 mole, the zinc-containing compound is 0.1-1 mole, the hydroxyl-containing compound is 1-5 mole, the carboxyl-containing compound is 0.1-0.5 mole, and the concentration of titanium element in the second solution is 3-10wt%.