Catalyst for nickel-metal hydride battery as well as preparation method and application of catalyst
By loading nickel and precious metals on the carbon-based material support, an efficient and stable nickel-hydrogen battery catalyst is prepared, which solves the problems of high catalyst cost and insufficient stability, improves the catalytic activity and stability of the battery, and is suitable for large-scale production.
Patent Information
- Application Number
- CN202410988436.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-22
AI Technical Summary
The catalysts in high-voltage nickel-hydrogen batteries are expensive and have insufficient stability and catalytic activity, which affects battery performance and life.
Nickel and precious metals are supported on the carbon-based material support, which are located in the outer layer of nickel in whole or part and are calcined in a reducing atmosphere to prepare a catalyst with high HER/HOR bifunctional catalytic activity and stability.
The amount of precious metal platinum is reduced, the stability and catalytic activity of the catalyst is improved, the preparation process is simplified, and it is suitable for large-scale production and application.
Smart Images

Figure CN119008976A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of nickel-hydrogen battery catalysts, and in particular to a catalyst for nickel-hydrogen batteries and a preparation method and application thereof. Background Art
[0002] Due to its high energy density, long cycle life and good environmental performance, the application of high-voltage nickel-hydrogen batteries in the field of energy storage and conversion is constantly expanding, and its market demand is also showing a rapid growth trend. With the advancement of technology, the performance of high-voltage nickel-hydrogen batteries is also constantly improving, and its charging speed, energy density and safety have been significantly improved.
[0003] However, the development of high-voltage nickel-hydrogen batteries also faces some challenges, one of which is the catalyst problem. Catalysts play a vital role in high-voltage nickel-hydrogen batteries, which directly affect the performance and life of the battery. In related technologies, the bifunctional catalysts of hydrogen evolution reaction (HER) and hydrogen oxidation reaction (HOR) actually used in high-voltage nickel-hydrogen batteries are mainly platinum-based materials, which achieve high efficiency and long life through a large number of platinum active sites. Limited by the use of platinum, its cost is very expensive. The stability or catalytic activity of other non-platinum materials is obviously insufficient. Summary of the invention
[0004] In view of this, in order to at least partially solve at least one of the above-mentioned technical problems, the present disclosure provides a catalyst for nickel-hydrogen batteries and a preparation method and application thereof.
[0005] According to an embodiment of one aspect of the present disclosure, a method for preparing a catalyst for a nickel-hydrogen battery is provided, comprising: pre-sintering a mixture of a nickel source and a carbon-based material to obtain a nickel-loaded carbon-based material; loading a precious metal compound onto the nickel-loaded carbon-based material to obtain a catalyst precursor; and calcining the catalyst precursor in a reducing atmosphere to obtain the nickel-hydrogen battery catalyst; wherein the precious metal compound comprises a platinum compound.
[0006] According to an embodiment of the present disclosure, the pre-sintering is performed in a protective atmosphere or a reducing atmosphere.
[0007] According to an embodiment of the present disclosure, the pre-sintering temperature is 400-600° C. and the time is 1-3 hours.
[0008] According to an embodiment of the present disclosure, the calcination temperature is 300-500° C. and the calcination time is 0.5-2 h.
[0009] According to an embodiment of the present disclosure, the reducing gas in the reducing atmosphere includes one or more of hydrogen, carbon monoxide or ammonia.
[0010] According to an embodiment of the present disclosure, the above-mentioned loading of the precious metal compound onto the above-mentioned nickel-loaded carbon-based material to obtain the catalyst precursor includes: adding the above-mentioned nickel-loaded carbon-based material to a solution containing the precious metal compound, so that the above-mentioned precious metal compound is loaded onto the above-mentioned nickel-loaded carbon-based material to obtain the above-mentioned catalyst precursor.
[0011] According to an embodiment of the present disclosure, the concentration of the platinum compound in the solution containing the precious metal compound is 0.001-0.020 mol / L.
[0012] According to an embodiment of the present disclosure, before pre-sintering the mixture of the nickel source and the carbon-based material, the method further includes: pre-treating the carbon-based material with an acidic solution; and preparing the mixture of the nickel source and the carbon-based material by dry or wet mixing.
[0013] According to an embodiment of another aspect of the present disclosure, a catalyst for a nickel-hydrogen battery is provided, wherein the catalyst comprises a carbon-based material, nickel and a precious metal, wherein the nickel and the precious metal are loaded on the carbon-based material, and the precious metal is wholly or partially located in an outer layer of the nickel; wherein the precious metal comprises platinum.
[0014] According to an embodiment of the present disclosure, the above-mentioned precious metal also includes at least one of ruthenium, iridium and palladium.
[0015] According to an embodiment of the present disclosure, the weight ratio of the nickel to the carbon-based material is (2-10):100.
[0016] According to an embodiment of the present disclosure, the molar ratio of the above-mentioned precious metal to the above-mentioned nickel is (0.2~4):10.
[0017] According to an embodiment of the present disclosure, the above-mentioned carbon-based material includes one or more of carbon nanotubes, activated carbon, graphene, carbon nanofibers, carbon black, and carbon felt.
[0018] According to another aspect of the embodiments of the present disclosure, a nickel-hydrogen battery is provided, wherein the nickel-hydrogen battery comprises the nickel-hydrogen battery catalyst prepared by the preparation method or the nickel-hydrogen battery catalyst.
[0019] According to the embodiment of the present disclosure, the mixture of the nickel source and the carbon-based material is first pre-sintered, and the nickel is loaded on the carbon-based material to obtain the carbon-based material loaded with nickel; the noble metal compound is then loaded on the carbon-based material loaded with nickel to obtain a catalyst precursor, so that the noble metal compound including the platinum compound is completely or partially located in the outer layer of the nickel, ensuring the catalytic effect of the noble metal; finally, calcination is performed in a reducing atmosphere group to increase the surface activity of the nickel and the noble metal, and the prepared nickel-hydrogen battery catalyst has high HER / HOR bifunctional catalytic activity and stability. In addition, the preparation method provided in the embodiment of the present disclosure is simplified in process, which is conducive to large-scale production and application.
[0020] According to the embodiments of the present disclosure, carbon-based materials are used as carriers, and nickel and precious metals are used as active components, wherein the precious metals including platinum are wholly or partially located on the outer layer of nickel, thereby reducing the amount of precious metal platinum while ensuring catalytic activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:
[0022] Figure 1 A transmission electron microscope photograph of the catalyst for nickel-hydrogen batteries prepared in Example 2 is shown;
[0023] Figure 2 HER test diagrams of the catalysts for nickel-hydrogen batteries prepared in Examples 1 to 2 and Comparative Examples 1 to 6 are shown;
[0024] Figure 3 The HOR test graphs of the catalysts for nickel-hydrogen batteries prepared in Examples 1-2 and Comparative Examples 1-6 are shown. DETAILED DESCRIPTION
[0025] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the embodiments of the present disclosure. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.
[0026] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The term "comprising" used herein indicates the existence of features, steps, operations, but does not exclude the existence or addition of one or more other features.
[0027] In the case of using expressions such as "at least one of A, B, and C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, and C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.). In the case of using expressions such as "at least one of A, B, or C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, or C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.).
[0028] With the rapid development of electric vehicles and energy storage systems, there is an urgent need for efficient, stable and environmentally friendly battery technology. With its high energy density, long cycle life and good environmental performance, high-voltage nickel-hydrogen batteries are increasingly being used in the field of energy storage and conversion, and their market demand is also showing a rapid growth trend. With the advancement of technology, the performance of high-voltage nickel-hydrogen batteries is also constantly improving, and their charging speed, energy density and safety have been significantly improved.
[0029] However, the development of high-voltage nickel-hydrogen batteries also faces some challenges, one of which is the catalyst problem. Catalysts play a vital role in high-voltage nickel-hydrogen batteries, which directly affect the performance and life of the battery. In related technologies, the bifunctional catalysts for hydrogen evolution reaction and hydrogen oxidation reaction actually used in high-voltage nickel-hydrogen batteries are mainly platinum-based materials, which achieve high efficiency and long life through a large number of platinum active sites. Limited by the use of platinum, its cost is very expensive. The stability or catalytic activity of other non-platinum materials is obviously insufficient.
[0030] In view of the high cost and the inability to balance performance and stability of HER / HOR catalysts, which are the core technology of nickel-hydrogen batteries, the present invention provides a method for preparing a low-cost, low-platinum, efficient and stable HER / HOR bifunctional catalyst.
[0031] In the process of realizing the concept of the present disclosure, it was found that by sequentially loading nickel and precious metals on a carbon-based material carrier so that all or part of the precious metals are located in the outer layer of the nickel, the amount of precious metal platinum can be reduced while ensuring catalytic activity and stability.
[0032] Specifically, according to an embodiment of one aspect of the present disclosure, a method for preparing a catalyst for a nickel-hydrogen battery is provided, comprising: pre-sintering a mixture of a nickel source and a carbon-based material to obtain a nickel-loaded carbon-based material; loading a precious metal compound onto the nickel-loaded carbon-based material to obtain a catalyst precursor; calcining the catalyst precursor in a reducing atmosphere to obtain a nickel-hydrogen battery catalyst; wherein the precious metal compound includes a platinum compound.
[0033] According to the embodiment of the present disclosure, the mixture of the nickel source and the carbon-based material is first pre-sintered, and the nickel is loaded on the carbon-based material to obtain the carbon-based material loaded with nickel; the noble metal compound is then loaded on the carbon-based material loaded with nickel to obtain a catalyst precursor, so that the noble metal compound including the platinum compound is completely or partially located in the outer layer of the nickel, ensuring the catalytic effect of the noble metal; finally, calcination is performed in a reducing atmosphere group to increase the surface activity of the nickel and the noble metal, and the prepared nickel-hydrogen battery catalyst has high HER / HOR bifunctional catalytic activity and stability. In addition, the preparation method provided in the embodiment of the present disclosure is simplified in process, which is conducive to large-scale production and application.
[0034] According to the embodiments of the present disclosure, in the related art, the catalysts often have insufficient catalytic activity in the HER and HOR reactions, resulting in a slow reaction rate, which affects the overall performance of the battery. The embodiments of the present disclosure can change the crystal structure of the catalyst by introducing precious metals as doping metals, thereby affecting the stability of the catalyst; in addition, the electronic state and degree of ionization of the metal atoms in the catalyst are changed, thereby promoting the improvement of reaction activity and selectivity. The preparation method provided by the present disclosure can optimize the electronic structure and surface properties of the catalyst for nickel-hydrogen batteries, improve the adsorption and dissociation ability of hydrogen, thereby enhancing the catalytic activity of the catalyst and improving the energy conversion efficiency of the battery.
[0035] According to the embodiments of the present disclosure, in the related art, the catalyst often suffers from performance degradation or deactivation under long-term operation or high-load conditions. The preparation method provided by the present disclosure enables the precious metal compound including the platinum compound to be completely or partially located in the outer layer of the nickel, and enhances the stability of the catalyst by regulating the composition and structure of the catalyst, so that it can still maintain excellent catalytic performance under long-term operation or harsh environment.
[0036] According to the embodiments of the present disclosure, in the related art, HER / HOR catalysts usually rely on precious metals (such as platinum particles) as active ingredients, which not only increases the manufacturing cost of the catalyst, but also limits its large-scale application. The preparation method provided in the embodiments of the present disclosure introduces nickel elements and adopts a new structure control process to fully utilize precious metal atoms such as platinum on the surface, effectively reducing the use of precious metals, thereby reducing the cost of the catalyst.
[0037] According to an embodiment of the present disclosure, before pre-sintering the mixture of the nickel source and the carbon-based material, the method further includes: pre-treating the carbon-based material with an acidic solution.
[0038] According to an embodiment of the present disclosure, the carbon-based material may be treated in an acidic solution having a concentration of 1 to 3 mol / L and a temperature of 60 to 100° C. for 1 to 6 hours. Preferably, the carbon-based material may be treated in an acidic solution having a concentration of 2 to 3 mol / L and a temperature of 80 to 100° C. for 1 to 3 hours.
[0039] According to an embodiment of the present disclosure, the acidic solution may be one or more of a nitric acid solution, a hydrochloric acid solution or a sulfuric acid solution.
[0040] According to the embodiments of the present disclosure, by pretreating the carbon-based material with an acidic solution, the surface of the carbon-based material can be cleaned and the doping structure of the surface layer of the carbon-based material can be modified, thereby increasing the active centers and stability of the catalyst for nickel-hydrogen batteries.
[0041] According to an embodiment of the present disclosure, before pre-sintering the mixture of the nickel source and the carbon-based material, the method further includes: preparing the mixture of the nickel source and the carbon-based material by dry or wet mixing.
[0042] According to an embodiment of the present disclosure, the nickel source and the carbon-based material can be mixed by dry method to obtain a mixture of the nickel source and the carbon-based material. Specifically, the carbon-based material powder and the nickel source material powder can be mixed by grinding or ball milling to obtain a mixture of the nickel source and the carbon-based material.
[0043] According to an embodiment of the present disclosure, the nickel source and the carbon-based material can be mixed by a wet method to obtain a mixture of the nickel source and the carbon-based material. Specifically, the carbon-based material can be added to a solution containing the nickel source by an impregnation method to obtain a mixture of the nickel source and the carbon-based material.
[0044] According to an embodiment of the present disclosure, the carbon-based material includes one or more of carbon nanotubes, activated carbon, graphene, carbon nanofibers, carbon black, and carbon felt. Preferably, the carbon-based material includes one or more of carbon nanotubes and graphene.
[0045] According to an embodiment of the present disclosure, the nickel source may be a nickel salt, and specifically, the nickel source may be one or more of nickel nitrate, nickel chloride, and nickel bromide.
[0046] According to an embodiment of the present disclosure, the pre-sintering is performed in a protective atmosphere or a reducing atmosphere.
[0047] According to an embodiment of the present disclosure, the reducing gas in the reducing atmosphere includes one or more of hydrogen, carbon monoxide or ammonia.
[0048] According to an embodiment of the present disclosure, the volume fraction of the reducing gas in the reducing atmosphere is 2% to 100%, preferably 2% to 5%.
[0049] According to an embodiment of the present disclosure, the protective atmosphere may be one or more of nitrogen and argon.
[0050] According to an embodiment of the present disclosure, the pre-sintering temperature is 400-600°C, and the time is 1-3 hours. Preferably, the pre-sintering temperature is 500-600°C, and the time is 1-2 hours. Specifically, the pre-sintering temperature can be 400°C, 450°C, 500°C, 525°C, 550°C or 600°C, and the time can be 1.0h, 1.5h, 2.0h, 2.5h or 3h.
[0051] According to the embodiments of the present disclosure, reasonable pre-sintering temperature and time can effectively slow down the loss of metal atoms to carbon-based materials; at the same time, nickel atoms are evenly loaded on the surface of carbon-based materials, slowing down the aging and agglomeration process of nickel particles, avoiding the production of large-particle nickel, resulting in insufficient active sites and waste of metal atoms.
[0052] According to an embodiment of the present disclosure, loading a precious metal compound onto a nickel-loaded carbon-based material to obtain a catalyst precursor includes: adding the nickel-loaded carbon-based material to a solution containing a precious metal compound, so that the precious metal compound is loaded onto the nickel-loaded carbon-based material to obtain a catalyst precursor.
[0053] According to an embodiment of the present disclosure, the concentration of the platinum compound in the solution containing the precious metal compound is 0.001-0.020 mol / L.
[0054] For example, a nickel-loaded carbon-based material is added to a platinum compound solution, so that the platinum compound is loaded on the nickel-loaded carbon-based material to obtain a catalyst precursor, wherein the concentration of the platinum compound solution is 0.001-0.020 mol / L, and the immersion time is 8-24 hours.
[0055] According to an embodiment of the present disclosure, the noble metal compound further comprises at least one of a ruthenium compound, an iridium compound, and a palladium compound. Preferably, the noble metal compound further comprises a ruthenium compound,
[0056] For example, the nickel-loaded carbon-based material is sequentially added to a ruthenium compound solution and a platinum compound solution, so that the ruthenium compound and the platinum compound are loaded on the nickel-loaded carbon-based material to obtain a catalyst precursor. The concentration of the ruthenium compound solution is 0.01-0.1 mol / L, and the immersion time is 8-24 hours; the concentration of the platinum compound solution is 0.001-0.020 mol / L, and the immersion time is 8-24 hours.
[0057] According to an embodiment of the present disclosure, the platinum compound may be a platinum salt. Specifically, the platinum compound may be one or more of chloroplatinic acid, platinum nitrate, and platinum sulfate.
[0058] According to an embodiment of the present disclosure, the ruthenium compound may be a ruthenium salt. Specifically, the ruthenium compound may be one or more of ruthenium chloride and ruthenium nitrate.
[0059] According to an embodiment of the present disclosure, the calcination temperature is 300-500°C, and the time is 0.5-2h. Preferably, the calcination temperature is 400-500°C, and the time is 0.5-1h. Specifically, the calcination temperature is 300°C, 350°C, 400°C, 425°C, 450°C or 500°C, and the time is 0.5h, 0.7h, 1.0h, 1.5h or 2.0h.
[0060] According to an embodiment of the present disclosure, the reducing gas in the reducing atmosphere includes one or more of hydrogen, carbon monoxide or ammonia.
[0061] According to an embodiment of the present disclosure, the volume fraction of the reducing gas in the reducing atmosphere is 2% to 5%. For example, the reducing atmosphere can be a mixed gas of hydrogen and argon, wherein the volume fraction of hydrogen is 5%.
[0062] According to the embodiments of the present disclosure, reasonable calcination temperature and time can optimize the electronic structure and surface properties of the catalyst and enhance the catalytic activity and stability of the catalyst. Reasonable calcination temperature and time can effectively slow down the loss of metal atoms to the base material, slow down the ripening and agglomeration process of precious metal particles, avoid the production of large particles, and cause insufficient active sites and waste of metal atoms.
[0063] According to an embodiment of the present disclosure, after the catalyst precursor is calcined in a reducing atmosphere, the method further includes: subjecting the calcined catalyst precursor to inert treatment in an oxidizing atmosphere to obtain a catalyst for a nickel-hydrogen battery.
[0064] According to an embodiment of the present disclosure, the oxidizing gas in the oxidizing atmosphere includes oxygen. The volume fraction of the oxidizing gas in the oxidizing atmosphere is 2% to 5%.
[0065] According to the embodiments of the present disclosure, the storage stability and activity of the catalyst can be improved through inert treatment.
[0066] According to an embodiment of another aspect of the present disclosure, a catalyst for a nickel-hydrogen battery is provided, the catalyst comprising a carbon-based material, nickel and a precious metal, wherein the nickel and the precious metal are loaded on the carbon-based material, and the precious metal is entirely or partially located in an outer layer of the nickel; wherein the precious metal comprises platinum.
[0067] According to an embodiment of the present disclosure, a carbon-based material is used as a carrier, and nickel and precious metals are used as active components, wherein the precious metal including platinum is wholly or partially located in the outer layer of the nickel, thereby reducing the amount of precious metal platinum while ensuring catalytic activity and stability.
[0068] According to an embodiment of the present disclosure, the noble metal further includes at least one of ruthenium, iridium and palladium. Preferably, the noble metal further includes ruthenium.
[0069] According to an embodiment of the present disclosure, the weight ratio of nickel to carbon-based material is (2-10): 100. Preferably, the weight ratio of nickel to carbon-based material is (4-8): 100. Further preferably, the weight ratio of nickel to carbon-based material is (6-8): 100. Specifically, the weight ratio of nickel to carbon-based material is 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100 or 10:100.
[0070] According to an embodiment of the present disclosure, the molar ratio of the noble metal to nickel is (0.2-4): 10. Preferably, the molar ratio of the noble metal to nickel is (1-4): 10. Further preferably, the molar ratio of the noble metal to nickel is (2-4): 10. Specifically, the molar ratio of the noble metal to nickel is 0.2: 10, 0.5: 10, 1: 10, 2: 10, 3: 10 or 4: 10.
[0071] According to an embodiment of the present disclosure, the molar ratio of platinum to nickel is (0.2~2):10.
[0072] According to an embodiment of the present disclosure, the molar ratio of ruthenium to nickel is (1~2):10.
[0073] According to an embodiment of the present disclosure, the carbon-based material includes one or more of carbon nanotubes, activated carbon, graphene, carbon nanofibers, carbon black, and carbon felt. Preferably, the carbon-based material includes one or more of carbon nanotubes and graphene.
[0074] According to an embodiment of another aspect of the present disclosure, a nickel-hydrogen battery is provided, which includes the nickel-hydrogen battery catalyst prepared by the above preparation method or the above nickel-hydrogen battery catalyst.
[0075] According to the embodiments of the present disclosure, in the related art, the catalyst often has insufficient catalytic activity in the HER and HOR reactions, resulting in a slow reaction rate, which affects the overall performance of the battery. The nickel-hydrogen battery catalyst prepared by the preparation method provided by the present disclosure or the nickel-hydrogen battery catalyst provided improves the hydrogen adsorption and dissociation ability, thereby enhancing the catalytic activity of the catalyst and improving the energy conversion efficiency of the battery.
[0076] The following lists a number of specific embodiments to illustrate the technical solution of the present invention in detail. It should be noted that the specific embodiments below are only used for illustration and are not used to limit the present invention.
[0077] Example 1
[0078] This embodiment provides a catalyst for a nickel-hydrogen battery. The catalyst for a nickel-hydrogen battery includes activated carbon, nickel and platinum. The nickel and platinum are loaded on the activated carbon, and the platinum is completely or partially located on the outer layer of the nickel.
[0079] Among them, the molar ratio of platinum to nickel is 1:10;
[0080] The weight ratio of nickel to activated carbon is 5:100.
[0081] The catalyst for nickel-hydrogen batteries provided in this embodiment is prepared by the following method:
[0082] (1) Activated carbon BP2000 with a high specific surface area was selected as the carbon-based material and treated with 2 M nitric acid at 80 °C for 3 hours to clean the surface and modify the doping structure of the surface carbon to obtain pretreated activated carbon.
[0083] (2) Take the activated carbon after the above pretreatment, add nickel nitrate as a nickel source, mix evenly with a ball mill, and pre-sinter in a nitrogen atmosphere at a sintering temperature of 400°C for 2 hours to obtain activated carbon (C) loaded with nickel (Ni), denoted as Ni-C.
[0084] (3) The Ni-C powder is added into a 0.01 mol / L chloroplatinic acid solution for 12 hours to load platinum onto the nickel-loaded carbon-based material to obtain a catalyst precursor.
[0085] (4) The catalyst precursor was then calcined at 500° C. in a 5% hydrogen-argon atmosphere (hydrogen gas volume fraction was 5%) for 1 hour to obtain a catalyst for a nickel-hydrogen battery.
[0086] The nickel-hydrogen battery catalyst prepared above was tested by transmission electron microscopy. Figure 1 As shown. Figure 1 As shown, ruthenium, platinum and nickel are uniformly loaded on the surface of activated carbon.
[0087] Example 2
[0088] This embodiment provides a catalyst for a nickel-hydrogen battery, which includes activated carbon, nickel, ruthenium and platinum. The nickel and platinum are loaded on the activated carbon, and the platinum is completely or partially located on the outer layer of the nickel.
[0089] The molar ratio of ruthenium, platinum and nickel is 1.5:1:10;
[0090] The weight ratio of nickel to activated carbon is 5:100.
[0091] The catalyst for nickel-hydrogen batteries provided in this embodiment is prepared by the following method:
[0092] (1) Activated carbon BP2000 with a high specific surface area was selected as the carbon-based material and treated with 2 M nitric acid at 80 °C for 3 hours to clean the surface and modify the doping structure of the surface carbon to obtain pretreated activated carbon.
[0093] (2) Take the activated carbon after the above pretreatment, add nickel nitrate as a nickel source, mix evenly with a ball mill, and pre-sinter in a nitrogen atmosphere at a sintering temperature of 500°C for 2 hours to obtain nickel-loaded activated carbon, which is recorded as Ni-C.
[0094] (3) The Ni-C powder was immersed in a 0.05M ruthenium chloride solution for 16 hours to achieve ruthenium (Ru) doping on the outer layer of the Ni particles to obtain RuNi-C. The RuNi-C powder was then added to a 0.01mol / L chloroplatinic acid solution for 12 hours. The catalyst precursor was obtained by ball milling for 1 hour.
[0095] (4) The catalyst precursor is then calcined at 450° C. in a 5% hydrogen-argon atmosphere (hydrogen gas volume fraction is 5%) for 1 hour to form a stable active structure of the catalyst, thereby obtaining a catalyst for nickel-hydrogen batteries.
[0096] (5) Cool the nickel-hydrogen battery catalyst to room temperature and introduce 2% oxygen for inert treatment for 30 minutes to improve the storage stability and activity of the catalyst. After the treatment, remove the catalyst and place it in a nitrogen environment for standby use.
[0097] Example 3
[0098] This embodiment provides a catalyst for a nickel-hydrogen battery, which includes graphene, nickel, ruthenium and platinum. The nickel and platinum are loaded on the graphene, and the platinum is completely or partially located on the outer layer of the nickel.
[0099] The molar ratio of ruthenium, platinum and nickel is 1.5:1.5:10;
[0100] The weight ratio of nickel to graphene is 4:100.
[0101] The catalyst for nickel-hydrogen batteries provided in this embodiment is prepared by the following method:
[0102] (1) Graphene was selected as the carbon-based material and treated with 1 M nitric acid at 80 °C for 2 hours to obtain pretreated graphene.
[0103] (2) Take the above-pretreated graphene, add nickel nitrate as a nickel source, grind and mix evenly, and then pre-sinter under a nitrogen atmosphere at a sintering temperature of 450°C for 2 hours to obtain nickel-loaded graphene, which is denoted as Ni-C.
[0104] (3) The Ni-C powder was immersed in a 0.08M ruthenium chloride solution for 12 hours of chemical etching to achieve ruthenium (Ru) doping on the outer layer of the Ni particles to obtain RuNi-C. The RuNi-C powder was then added to a 0.005mol / L chloroplatinic acid solution for 12 hours of immersion. The mixture was ground for 1 hour to obtain a catalyst precursor.
[0105] (4) The catalyst precursor was then calcined at 400° C. in a 5% hydrogen-argon atmosphere (hydrogen gas volume fraction was 5%) for 1.5 hours to obtain a catalyst for nickel-hydrogen batteries.
[0106] (5) Cool the nickel-hydrogen battery catalyst to room temperature and introduce 2% oxygen for inert treatment for 25 minutes. After the treatment, remove the catalyst and place it in a nitrogen environment for standby use.
[0107] Example 4
[0108] This embodiment provides a catalyst for a nickel-hydrogen battery, which includes activated carbon, nickel, ruthenium and platinum. The nickel and platinum are loaded on the activated carbon, and the platinum is completely or partially located on the outer layer of the nickel.
[0109] The molar ratio of ruthenium, platinum and nickel is 1.5:1:10;
[0110] The weight ratio of nickel to activated carbon is 8:100.
[0111] The catalyst for nickel-hydrogen batteries provided in this embodiment is prepared by the following method:
[0112] (1) Activated carbon BP2000 with a high specific surface area was selected as the carbon-based material and treated with 3 M nitric acid at 90 °C for 2 hours to clean the surface and modify the doping structure of the surface carbon to obtain pretreated activated carbon.
[0113] (2) Take the activated carbon after the above pretreatment, add nickel nitrate as a nickel source, mix evenly with a ball mill, and pre-sinter in a nitrogen atmosphere at a sintering temperature of 550°C for 2 hours to obtain nickel-loaded activated carbon, which is recorded as Ni-C.
[0114] (3) The Ni-C powder was immersed in a 0.02M ruthenium chloride solution for 24 hours to achieve ruthenium (Ru) doping on the outer layer of the Ni particles to obtain RuNi-C. The RuNi-C powder was then added to a 0.015mol / L chloroplatinic acid solution for 16 hours. The catalyst precursor was obtained by ball milling for 1 hour.
[0115] (4) The catalyst precursor is then calcined at 350° C. in a 5% hydrogen-argon atmosphere (hydrogen gas volume fraction is 5%) for 1 hour to form a stable active structure of the catalyst, thereby obtaining a catalyst for nickel-hydrogen batteries.
[0116] (5) Cool the nickel-hydrogen battery catalyst to room temperature and introduce 2% oxygen for inert treatment for 10 minutes. After the treatment, remove the catalyst and place it in a nitrogen environment for standby use.
[0117] Example 5
[0118] This embodiment provides a catalyst for a nickel-hydrogen battery, which includes a carbon-based material, nickel, ruthenium and platinum. The nickel and platinum are loaded on graphene, and the platinum is completely or partially located on the outer layer of the nickel.
[0119] The carbon-based material includes carbon nanotubes and graphene, and the weight ratio of the carbon nanotubes to the graphene is 1:1;
[0120] The molar ratio of ruthenium, platinum and nickel is 1.8:0.3:10;
[0121] The weight ratio of nickel to carbon-based material is 3:100.
[0122] The catalyst for nickel-hydrogen batteries provided in this embodiment is prepared by the following method:
[0123] (1) Graphene and carbon nanotubes were selected as carbon-based materials and treated with 1.5 M nitric acid at 70 °C for 1 hour to obtain pretreated carbon-based materials.
[0124] (2) Take the above-mentioned pretreated carbon-based material, add nickel nitrate as a nickel source, mix evenly with a ball mill, and pre-sinter in a nitrogen atmosphere at a sintering temperature of 400°C for 1.5 hours to obtain a nickel-loaded carbon-based material, which is denoted as Ni-C.
[0125] (3) The Ni-C powder was immersed in a 0.07M ruthenium chloride solution for 20 hours of chemical etching to achieve ruthenium (Ru) doping on the outer layer of the Ni particles to obtain RuNi-C. The RuNi-C powder was then added to a 0.003 mol / L chloroplatinic acid solution for 18 hours. Grinding was performed for 1 hour to obtain a catalyst precursor.
[0126] (4) The catalyst precursor was then calcined at 450° C. in a 5% hydrogen-argon atmosphere (hydrogen gas volume fraction is 5%) for 2 hours to obtain a catalyst for a nickel-hydrogen battery.
[0127] (5) Cool the nickel-hydrogen battery catalyst to room temperature and introduce 2% oxygen for inert treatment for 25 minutes. After the treatment, remove the catalyst and place it in a nitrogen environment for standby use.
[0128] Comparative Example 1
[0129] This comparative example provides a catalyst for a nickel-hydrogen battery. The catalyst for a nickel-hydrogen battery comprises activated carbon, nickel and platinum, wherein the nickel and platinum are supported on the activated carbon.
[0130] Among them, the molar ratio of platinum to nickel is 1:10;
[0131] The weight ratio of nickel to activated carbon is 5:100.
[0132] The catalyst for nickel-hydrogen battery provided in this comparative example is prepared by the following method:
[0133] (1) Step (1) is the same as in Example 1 and will not be described in detail.
[0134] (2) Take the activated carbon after the pretreatment, add nickel nitrate as a nickel source, and mix them evenly with a ball mill to obtain a mixture of nickel nitrate and activated carbon.
[0135] Step (3) and step (4) are the same as those in Example 1 and will not be described in detail.
[0136] Comparative Example 2
[0137] This comparative example provides a catalyst for a nickel-hydrogen battery, which includes activated carbon, nickel and ruthenium. The nickel and ruthenium are supported on the activated carbon, and the ruthenium is completely or partially located on the outer layer of the nickel.
[0138] Wherein, the molar ratio of ruthenium to nickel is 1:10;
[0139] The weight ratio of nickel to activated carbon is 5:100.
[0140] The catalyst for nickel-hydrogen battery provided in this comparative example is prepared by the following method:
[0141] (1) Step (1) is the same as in Example 1 and will not be described in detail.
[0142] (2) Take the activated carbon after the above pretreatment, add nickel nitrate as a nickel source, mix evenly with a ball mill, and pre-sinter in a nitrogen atmosphere at a sintering temperature of 500°C for 2 hours to obtain activated carbon (C) loaded with nickel (Ni), denoted as Ni-C.
[0143] (3) Add the above-mentioned mixture of nickel nitrate and activated carbon into a 0.01 mol / L ruthenium chloride solution for 12 hours to load ruthenium onto the nickel-loaded carbon-based material to obtain a catalyst precursor.
[0144] (4) Step (4) is the same as in Example 1 and will not be described in detail.
[0145] Comparative Example 3
[0146] This comparative example provides a catalyst for a nickel-hydrogen battery. The nickel-hydrogen battery catalyst includes activated carbon and nickel, wherein the nickel is loaded on the activated carbon.
[0147] The weight ratio of nickel to activated carbon is 5:100.
[0148] The catalyst for nickel-hydrogen battery provided in this comparative example is prepared by the following method:
[0149] (1) Step (1) is the same as in Example 1 and will not be described in detail.
[0150] (2) Take the activated carbon after the above pretreatment, add nickel nitrate as a nickel source, mix evenly with a ball mill, and pre-sinter in a nitrogen atmosphere at a sintering temperature of 500°C for 2 hours to obtain activated carbon (C) loaded with nickel (Ni), denoted as Ni-C.
[0151] (3) Step (3) is the same as step (4) of Example 1 and will not be described again.
[0152] Comparative Example 4
[0153] This comparative example provides a catalyst for a nickel-hydrogen battery, which is a JM20% platinum-carbon catalyst, the brand is Johnson Matthey, and the platinum content is 20%.
[0154] Comparative Example 5
[0155] This comparative example provides a catalyst for a nickel-hydrogen battery. The catalyst for a nickel-hydrogen battery comprises activated carbon, nickel and platinum. The nickel and platinum are loaded on the activated carbon, and the platinum is completely or partially located on the outer layer of the nickel.
[0156] Among them, the molar ratio of platinum to nickel is 1:10;
[0157] The weight ratio of nickel to activated carbon is 5:100.
[0158] The preparation method of the catalyst for nickel-hydrogen batteries provided in this comparative example refers to that in Example 1, except that the pre-sintering temperature in step (2) is 300° C., which will not be described in detail.
[0159] Comparative Example 6
[0160] This comparative example provides a catalyst for a nickel-hydrogen battery. The catalyst for a nickel-hydrogen battery comprises activated carbon, nickel and platinum. The nickel and platinum are loaded on the activated carbon, and the platinum is completely or partially located on the outer layer of the nickel.
[0161] Among them, the molar ratio of platinum to nickel is 1:10;
[0162] The weight ratio of nickel to activated carbon is 5:100.
[0163] The preparation method of the catalyst for nickel-hydrogen batteries provided in this comparative example refers to that in Example 1, except that the calcination temperature in step (4) is 750° C., which will not be described in detail.
[0164] HER and HOR performance testing
[0165] The catalysts for nickel-hydrogen batteries prepared in the above Examples 1-2 and Comparative Examples 1-6 were respectively subjected to HER and HOR performance tests according to the following steps:
[0166] (1) Preparation of turbid catalyst ink: Add several milligrams of catalyst powder to 1 mL of a mixture containing 960 μL of ethanol and 40 μL of 5% Nafion solution, and sonicate for 30 minutes. Then, use a pipette to drop the homogeneous catalyst ink onto a 5 mm diameter glassy carbon (GC) electrode and bake it dry with a baking lamp.
[0167] (2) In 0.1 M KOH solution, with Ag / AgCl as the reference electrode and graphite as the counter electrode, the catalytic electrode was subjected to LSV test in the HER potential range and the LSV curve was recorded.
[0168] (3) LSV tests in the HOR potential range were carried out under the same conditions to evaluate the HOR performance of the catalyst.
[0169] The HER test results of the catalysts for nickel-hydrogen batteries prepared in Examples 1-2 and Comparative Examples 1-6 are as follows: Figure 2 As shown, the HOR test results are as follows Figure 3 As shown. Figure 2 and Figure 3 It can be seen that the catalysts for nickel-hydrogen batteries prepared in Examples 1-2 have better HER / HOR bifunctional catalytic activity than those prepared in Comparative Examples 1-6.
[0170] Stability test
[0171] The catalysts for nickel-hydrogen batteries prepared in Examples 1-2 and Comparative Examples 1-6 were tested for current density stability, and the test results are shown in Tables 1 and 2. Table 1 shows the 12-hour current density stability (HER) of each sample at -0.2 V vs RHE; Table 2 shows the 12-hour current density stability (HOR) of each sample at 0.1 V vs RHE.
[0172] From the analysis of Table 1 and Table 2, it can be seen that the catalysts for nickel-hydrogen batteries prepared in Examples 1-2 have better stability than those prepared in Comparative Examples 1-6.
[0173] Table 1
[0174]
[0175] Table 2
[0176]
[0177] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.
Claims
1. A method for preparing a catalyst for a nickel-hydrogen battery, characterized in that: include: Pre-sintering a mixture of a nickel source and a carbon-based material to obtain a nickel-loaded carbon-based material; Loading a noble metal compound onto the nickel-loaded carbon-based material to obtain a catalyst precursor; as well as calcining the catalyst precursor in a reducing atmosphere to obtain the catalyst for a nickel-hydrogen battery; Wherein, the noble metal compound includes a platinum compound.
2. The preparation method according to claim 1, characterized in that: The pre-sintering is carried out in a protective atmosphere or a reducing atmosphere; The pre-sintering temperature is 400-600° C. and the time is 1-3 hours.
3. The preparation method according to claim 1 or 2, characterized in that: The calcination temperature is 300-500°C and the calcination time is 0.5-2h; The reducing gas in the reducing atmosphere includes one or more of hydrogen, carbon monoxide or ammonia.
4. The preparation method according to claim 1 or 2, characterized in that: The step of loading the noble metal compound onto the nickel-loaded carbon-based material to obtain a catalyst precursor comprises: Adding the nickel-loaded carbon-based material to a solution containing a noble metal compound, so that the noble metal compound is loaded on the nickel-loaded carbon-based material, to obtain the catalyst precursor; Wherein, the concentration of the platinum compound in the solution containing the precious metal compound is 0.001-0.020 mol / L.
5. The preparation method according to claim 1 or 2, characterized in that: Before pre-sintering the mixture of the nickel source and the carbon-based material, the following steps are also included: Pretreating the carbon-based material with an acidic solution; The mixture of the nickel source and the carbon-based material is prepared by dry or wet mixing.
6. A catalyst for nickel-hydrogen batteries, characterized in that: The catalyst comprises a carbon-based material, nickel and a noble metal, wherein the nickel and the noble metal are loaded on the carbon-based material, and the noble metal is entirely or partially located on the outer layer of the nickel; Wherein, the precious metal includes platinum.
7. The catalyst according to claim 6, characterized in that The noble metal also includes at least one of ruthenium, iridium and palladium.
8. The catalyst according to claim 6 or 7, characterized in that The weight ratio of the nickel to the carbon-based material is (2-10):100; The molar ratio of the noble metal to the nickel is (0.2-4):
10.
9. The catalyst according to claim 6 or 7, characterized in that The carbon-based material includes one or more of carbon nanotubes, activated carbon, graphene, carbon nanofibers, carbon black, and carbon felt.
10. A nickel-metal hydride battery, characterized in that: The nickel-hydrogen battery comprises a nickel-hydrogen battery catalyst prepared by the preparation method according to any one of claims 1 to 5 or a nickel-hydrogen battery catalyst according to any one of claims 6 to 9.