β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel and preparation method thereof
By introducing β-cyclodextrin modified polyp-dioxane into polyvinyl alcohol hydrogels, a hydrogel with network interpenetrating structures is solved in terms of mechanical properties and biocompatibility of traditional hydrogels. The defects have achieved a better wound healing environment and a simple preparation process.
Patent Information
- Application Number
- CN202310043480.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-01-29
AI Technical Summary
Traditional wound dressings have defects in mechanical properties, water absorption-retaining properties and biocompatibility, resulting in limited wound healing and risk of secondary damage.
The hydrogel is prepared by freezing-dissolving of β-cyclodextrin modified polyp-dioxane and polyvinyl alcohol to form a β-cyclodextrin modified polyp-dioxane with network interpenetrating structure/ Polyvinyl alcohol hydrogels, the reinforcement material is evenly dispersed in the main material, forming a polymer network through hydrogen bonding, improving mechanical and swelling properties.
It significantly improves the mechanical strength, water absorption-dehydration performance and biocompatibility of the hydrogel, simplifies the preparation process, and shows broad application prospects in the field of biomedical science.
Smart Images

Figure CN115894972B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical wound dressing materials, and in particular to a beta-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel and a preparation method thereof. Background Art
[0002] When the skin is damaged, bacteria will enter the human body through the wound, disrupt the internal balance of the human body, and cause inflammation, leading to wound infection. In order to ensure the wound healing environment, wound dressings came into being and developed rapidly. Wound dressings are a kind of wound covering material, which has the basic characteristics of isolating external microorganisms, exchanging gas and water with the outside world, absorbing wound exudate, and being non-toxic and harmless. At present, wound dressings mainly include ointments, films, foams and gels. Under the condition that the dressing is non-toxic and non-allergenic, the dressing is covered on the wound to achieve the purpose of blocking microorganisms, allowing water and gas exchange, and maintaining the moist environment required for the wound, thereby avoiding wound inflammation or infection.
[0003] Although traditional wound dressings can keep the wound dry, if the wound is too dry, it will slow down wound healing, and its structural defects will cause adhesion of the wound, causing secondary damage to the wound when the dressing is removed. Specifically, although film dressings are transparent as a whole, which makes it easy to observe the wound, they have the disadvantage of poor fluid absorption and are only suitable for wounds with less exudate. Foam dressings have a certain shape recovery, but they need to be replaced frequently and are prone to adhesion to the wound, causing secondary damage, and are not suitable for low exudate wounds. Although chitosan hydrogel wound dressings have obvious antibacterial activity, their mechanical properties are poor. Hydrogel dressings are a soft material with excellent performance. Their biggest feature is their high water content, which can provide a moist environment for the wound and facilitate wound healing. At the same time, hydrogels have good elasticity, are easy to remove, and have the effect of relieving local pain. Therefore, hydrogel dressings have gradually become the mainstream material for wound dressings.
[0004] From the perspective of chemical structure, hydrogel dressing is a three-dimensional dressing formed by cross-linking natural or synthetic hydrophilic polymers. Its skeleton structure has many hydrophilic groups. Due to the presence of these groups, the hydrogel can absorb a large amount of water and fill the grid gaps of the hydrogel, and utilize the internal cross-linking of the skeleton structure without bursting. Polyvinyl alcohol hydrogel is a hydrogel material with good biocompatibility, high water content and lubricity. However, since its cross-linked network structure is not very strong, it is greatly affected by the outside world, and the cross-linking distribution of the polymer is uneven, resulting in certain defects in the degradation performance, water absorption, water retention, and mechanical strength of polyvinyl alcohol hydrogel. Summary of the invention
[0005] The object of the present invention is to provide a β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel having good mechanical strength, water absorption and water retention performance, and good biological properties.
[0006] Another object of the present invention is to provide a method for preparing the above-mentioned β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel
[0007] To this end, the technical solution of the present invention is as follows:
[0008] A β-cyclodextrin-modified polydioxanone / polyvinyl alcohol hydrogel is prepared by freeze-thawing polyvinyl alcohol, a dimethyl sulfoxide aqueous solution and β-cyclodextrin-modified polydioxanone. β-cyclodextrin-modified polydioxanone is used as a reinforcing material to form a polymer network interpenetrating structure with polyvinyl alcohol in the solution through hydrogen bonding, so as to overcome the above-mentioned defects of traditional polyvinyl alcohol hydrogel.
[0009] Specifically, the preparation method of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel comprises the following steps:
[0010] S1. Dissolving polyvinyl alcohol (PVA) in a dimethyl sulfoxide aqueous solution to obtain a polyvinyl alcohol solution (PVA solution); wherein the weight average molecular weight of the polyvinyl alcohol is 100,000 to 150,000.
[0011] The purpose of step S1 is to prepare a pre-solution for forming the main body material, namely, a polyvinyl alcohol swelling solution.
[0012] S2. Dissolve β-cyclodextrin modified polydioxanone (β-CD / PPDO) in a dimethyl sulfoxide aqueous solution to obtain a β-cyclodextrin modified polydioxanone solution (β-CD / PPDO solution); wherein the amount of β-cyclodextrin modified polydioxanone is 1wt.% to 10wt.% of the amount of polyvinyl alcohol.
[0013] The purpose of step S2 is to prepare a β-cyclodextrin modified polydioxanone solution to form a reinforcing material; specifically, the β-cyclodextrin modified polydioxanone is prepared from β-cyclodextrin and polydioxanone; wherein, β-cyclodextrin is a truncated cone-shaped cavity structure with hydrophobicity inside the cavity and hydrophilicity outside the cavity, and has good water solubility and biocompatibility; the hydrophobicity inside the cavity and the hydrophilicity outside the cavity of β-CD enable it to include various molecules to form a host-guest complex or supramolecular substance; and the cavity diameter of β-CD is similar to the volume of most guest molecules, so that the properties of the formed complex are stable; and polydioxanone (PPDO) is a type of degradable linear aliphatic polymer material with good degradability and biocompatibility, the ether bonds on its molecular chain make the polymer flexible, and the ester bonds on its molecular chain make the polymer degradable, and the degradation products are harmless to the human body, and also greatly reduce the damage and side effects to human organs, that is, it shows biocompatibility.
[0014] The specific preparation steps of β-cyclodextrin modified polydioxanone are as follows: 1) β-cyclodextrin and polydioxanone with a mass ratio of 3:1 are respectively prepared into solutions in ultra-dry DMF, and then the β-cyclodextrin solution is added dropwise to the polydioxanone solution to obtain a mixed solution; 2) the mixed solution is stirred and reacted in a constant temperature oil bath at 60° C. for 12 hours, and then placed at room temperature for 12 hours, and white precipitates remain in the mixed solution; the above heating and stirring-room temperature standing operation is repeated multiple times, until the white precipitate residue in the mixed solution is significantly reduced and remains unchanged to obtain a reaction solution; 3) removing the solvent in the reaction solution by rotary evaporation, and adding the obtained concentrated solution to excess cold ether to precipitate; centrifuging to obtain a precipitated product, and washing the precipitated product with 1,1,2,2-tetrachloroethane, and then filtering and drying; 4) washing the dried product with distilled water, and then filtering, drying, and grinding to obtain β-cyclodextrin modified polydioxanone; wherein the viscosity average molecular weight of PPDO is 1×10 3 ~1×10 5 .
[0015] After the above reaction, β-CD and PPDO use hydrogen bonds and intermolecular forces to prepare β-cyclodextrin-modified polydioxanone assemblies. The addition of water-soluble cyclodextrin increases the hydrophilicity of PPDO; at the same time, the cavity of β-CD protects PPDO from being easily hydrolyzed, maintaining the excellent performance of PPDO, and can be used for the preparation of hydrogels.
[0016] S3. Add the β-cyclodextrin modified polydioxanone solution prepared in step S2 to the polyvinyl alcohol solution prepared in step S1, and place the mixed solution in a constant temperature oil bath at 70°C to 100°C, first stir for 0.5h to mix evenly, then stir for 1.5h to 6.5h to allow the polyvinyl alcohol to be fully hydrated and swollen, and cool to room temperature to obtain a polyvinyl alcohol swelling solution in which β-cyclodextrin modified polydioxanone is dispersed.
[0017] S4. Use ultrasound, vacuum or heating to eliminate bubbles in the polyvinyl alcohol swelling solution in which β-cyclodextrin-modified polydioxanone is dispersed, so as to obtain a polyvinyl alcohol swelling solution (β-CD / PPDO / PVA swelling solution) in which β-cyclodextrin-modified polydioxanone is uniformly dispersed.
[0018] After step S3 and step S4, the reinforcing material β-cyclodextrin modified polydioxanone is uniformly dispersed in the swelling liquid of polyvinyl alcohol. At this time, β-cyclodextrin modified polydioxanone, polyvinyl alcohol and dimethyl sulfoxide form a uniform swelling liquid under the action of hydrogen bonds.
[0019] S5. Freeze the swelling solution obtained in step S4 at -18°C for 6 h to 12 h, and then thaw it at room temperature for 1 h to 5 h.
[0020] S6. Repeat the freezing-thawing operation of step S5 3 to 5 times to obtain β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel (β-CD / PPDO / PVA hydrogel).
[0021] In step S5 and step S6, the β-CD / PPDO / PVA swelling solution is subjected to repeated freeze-thaw method to form a β-CD / PPDO / PVA hydrogel; specifically, the β-CD / PPDO / PVA hydrogel uses polyvinyl alcohol as the main material of the hydrogel and β-cyclodextrin-modified polydioxanone as the reinforcing material. The reinforcing material is uniformly dispersed in the main material and the hydrogel material is formed by freeze-thaw method, thereby realizing a chemically cross-link-free method. β-cyclodextrin-modified polydioxanone is introduced into the PVA hydrogel with a network structure as the second network of the hydrogel. The two form a polymer network interpenetrating structure under the action of hydrogen bonds, and compared with ordinary polyvinyl alcohol hydrogel, the mechanical properties and swelling properties (i.e., water absorption-loss properties) of the hydrogel are greatly improved.
[0022] In the process of selecting the main material, the applicant tried to use polyethylene glycol, chitosan and gelatin, which are also biocompatible and degradable, in addition to polyvinyl alcohol; however, in the process of preparing hydrogel, although polyethylene glycol has the advantages of being non-toxic, non-irritating and having good water solubility, it is easily degraded in an aerobic environment, which has an adverse effect on its use; although chitosan has the advantages of good biocompatibility and in vivo degradability, there are strong hydrogen bonds in the chitosan molecules, and it is only easily soluble in acidic media, and its solubility in water is not large. In addition, chitosan is not stable enough in acidic solutions and will degrade even at room temperature; and although gelatin also has good bioaffinity and degradability, the uncross-linked gelatin film has the disadvantages of being easily soluble in water, being hard and brittle, and having poor mechanical properties; therefore, polyvinyl alcohol was finally used as the material for preparing the gel main body.
[0023] Preferably, in step S1 and step S2, the dimethyl sulfoxide aqueous solution is a mixed solution prepared by dimethyl sulfoxide and deionized water in a volume ratio of 3:10.
[0024] Preferably, in the mixed solution of step S3, the concentration of polyvinyl alcohol in the dimethyl sulfoxide aqueous solution is 0.05 to 0.20 g / mL.
[0025] Preferably, in step S1, the preparation temperature of the polyvinyl alcohol solution is 95-100°C.
[0026] Preferably, in step S2, the preparation temperature of the β-cyclodextrin modified polydioxanone solution is 60-75°C.
[0027] Preferably, in step S4, an ultrasonic method is used to eliminate bubbles, and the steps are: at room temperature, the container of the swelling solution prepared in step S3 is placed in an ultrasonic cleaning machine, and ultrasonicated for 10 minutes to 30 minutes to obtain a polyvinyl alcohol swelling solution in which β-cyclodextrin-modified polydioxanone is uniformly dispersed.
[0028] Preferably, in step S4, a vacuum method is used to eliminate bubbles, and the steps are: at room temperature, the swelling liquid prepared in step S3 is placed in a vacuum oven at a pressure of 0 to -0.1 MPa for 10 to 30 minutes to obtain a polyvinyl alcohol swelling liquid in which β-cyclodextrin-modified polydioxanone is uniformly dispersed.
[0029] Preferably, in step S4, a heating method is used to eliminate bubbles, and the steps are: at room temperature, the swelling liquid prepared in step S3 is placed in an environment with a temperature of 150° C. to 200° C. for 10 to 30 minutes to obtain a polyvinyl alcohol swelling liquid in which β-cyclodextrin-modified polydioxanone is uniformly dispersed.
[0030] A β-cyclodextrin modified polydioxanone hydrogel prepared by adopting the preparation method of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel.
[0031] Compared with the prior art, the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel uses β-cyclodextrin modified polydioxanone as a reinforcing material, which is dispersed in a polyvinyl alcohol hydrogel as a main material and prepared into a hydrogel with a network interpenetrating structure by a physical freeze-thaw method, so that the hydrogel has good mechanical properties (including tensile properties and compression properties), swelling properties (including water absorption and water loss properties), as well as biocompatibility and biodegradability compared with ordinary polyvinyl alcohol hydrogels; at the same time, the preparation method of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is simple, the conditions are controllable, and the hydrogel has broad application prospects in the biomedical field. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The infrared spectra of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogels prepared in Examples 1 to 5 of the present invention and the polyvinyl alcohol hydrogel prepared in Comparative Example 1;
[0033] FIG2( a ) is a scanning electron micrograph of a brittle fracture surface on one side of a β-cyclodextrin-modified polydioxanone / polyvinyl alcohol hydrogel prepared in Example 5 of the present invention;
[0034] FIG2( b ) is a scanning electron micrograph of the brittle fracture surface on the other side of the β-cyclodextrin-modified polydioxanone / polyvinyl alcohol hydrogel prepared in Example 5 of the present invention;
[0035] FIG3( a ) is an atomic force microscope plane image of β-cyclodextrin-modified polydioxanone in an embodiment of the present invention;
[0036] FIG3( b ) is an atomic force microscope stereoscopic scale image of β-cyclodextrin-modified polydioxanone in an embodiment of the present invention;
[0037] Figure 4 The mechanical stretching curves of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogels prepared in Examples 1 to 4 of the present invention and the polyvinyl alcohol hydrogel prepared in Comparative Example 1;
[0038] Figure 5 It is a mechanical compression curve diagram of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel prepared in Examples 1 to 5 of the present invention and the polyvinyl alcohol hydrogel prepared in Comparative Example 1;
[0039] FIG6( a ) is a graph showing the water absorption rate of the β-cyclodextrin-modified polydioxanone / polyvinyl alcohol hydrogels prepared in Examples 1 to 5 of the present invention and the polyvinyl alcohol hydrogel prepared in Comparative Example 1;
[0040] FIG6( b ) is a water loss curve of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogels prepared in Examples 1 to 5 of the present invention and the polyvinyl alcohol hydrogel prepared in Comparative Example 1. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the following embodiments are by no means intended to limit the present invention in any way.
[0042] Example 1
[0043] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0044] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and place the mixture in a 100° C. constant temperature oil bath to stir and dissolve to obtain a PVA solution.
[0045] S2, adding 0.02 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 60° C. to obtain a β-CD / PPDO solution;
[0046] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 70°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0047] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 30 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0048] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 6 hours, and then thawing it at room temperature for 3 hours;
[0049] S6. Repeat the freeze-thaw operation of step S5 three times to obtain β-CD / PPDO / PVA hydrogel.
[0050] In Example 1, PVA is specifically polyvinyl alcohol PVA-117 produced by Shanghai Mairui Chemical Technology Co., Ltd., and its weight average molecular weight is 1.45×10 5 , Examples 2 to 10 and Comparative Example 1 are the same.
[0051] The dimethyl sulfoxide aqueous solution is a mixed solution prepared by dimethyl sulfoxide and deionized water in a volume ratio of 3:10, and Examples 2 to 10 and Comparative Example 1 are the same.
[0052] β-cyclodextrin modified polydioxanone (hereinafter referred to as β-CD / PPDO) is assembled from β-cyclodextrin (hereinafter referred to as β-CD) and polydioxanone (hereinafter referred to as PPDO) in a weight ratio of 3:1, and Examples 2 to 10 are the same.
[0053] The specific preparation steps of β-cyclodextrin modified polydioxanone are as follows:
[0054] 1) Add 0.75 g PPDO and 25 mL ultra-dry DMF into a reaction bottle, place it in an oil bath at 60°C, stir thoroughly to dissolve, and obtain a clear and transparent PPDO solution; wherein the viscosity-average molecular weight of PPDO is 3×10 4 ;
[0055] 2) Dissolve 2.25 g of β-CD in 25 mL of ultra-dry DMF and place in a dry constant pressure funnel to add dropwise to the PPDO solution; after the addition is completed, the mixed solution is stirred in a constant temperature oil bath at 60°C for 12 hours, and then allowed to stand at room temperature for 12 hours. At this time, white precipitate remains in the reaction bottle; the reaction bottle is placed in a 60°C oil bath again, stirred for 12 hours, and then allowed to stand at room temperature; repeat the above heating-standing operation several times until the white precipitate is significantly reduced and remains unchanged, indicating that the reaction is sufficient, and the reaction is stopped;
[0056] 3) using a rotary evaporator to remove most of the solvent to obtain a concentrated solution; adding the concentrated solution dropwise to an excess of cold ether that has been cooled in an ice-water bath to precipitate; using a high-speed centrifuge to obtain a precipitated product, and washing the precipitated product with 1,1,2,2-tetrachloroethane (TCEA) to remove unreacted PPDO; filtering, and vacuum drying the precipitated product in a vacuum drying oven at 45° C.;
[0057] 4) Wash the dried product with a small amount of distilled water to remove free cyclodextrin; filter, place the product in a vacuum drying oven at 45° C. for vacuum drying, and grind it into powder to obtain β-CD / PPDO for later use.
[0058] Example 2
[0059] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0060] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0061] S2, adding 0.06 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 75° C. to obtain a β-CD / PPDO solution;
[0062] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing in a 100° C. constant temperature oil bath and stirring for 0.5 h to mix evenly, and then stirring for 6.5 h to allow the PVA to be fully hydrated and swollen, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0063] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 30 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0064] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 12 hours, and then thawing it at room temperature for 5 hours;
[0065] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0066] Example 3
[0067] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0068] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0069] S2, adding 0.1 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 75° C. to obtain a β-CD / PPDO solution;
[0070] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 95°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0071] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 15 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0072] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 6 hours, and then thawing it at room temperature for 4 hours;
[0073] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0074] Example 4
[0075] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0076] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0077] S2, adding 0.14 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 75° C. to obtain a β-CD / PPDO solution;
[0078] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 95°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0079] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 15 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0080] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 10 hours, and then thawing it at room temperature for 2 hours;
[0081] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0082] Example 5
[0083] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0084] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0085] S2, adding 0.2 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 60° C. to obtain a β-CD / PPDO solution;
[0086] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 95°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0087] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 30 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0088] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 12 hours, and then thawing it at room temperature for 5 hours;
[0089] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0090] Example 6
[0091] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0092] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and place the mixture in a 100° C. constant temperature oil bath to stir and dissolve to obtain a PVA solution.
[0093] S2, adding 0.04 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 60° C. to obtain a β-CD / PPDO solution;
[0094] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing in a 100° C. constant temperature oil bath and stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to be fully hydrated and swollen, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0095] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 20 minutes to remove bubbles to obtain a uniform β-CD / PPDO / PVA swelling solution;
[0096] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 8 hours, and then thawing it at room temperature for 4 hours;
[0097] S6. Repeat the freeze-thaw operation of step S5 4 times to obtain β-CD / PPDO / PVA hydrogel.
[0098] Example 7
[0099] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0100] S1. Add 2 g of PVA into 5 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0101] S2, adding 0.08 g of β-CD / PPDO into 5 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 70° C. to obtain a β-CD / PPDO solution;
[0102] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 95°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0103] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 30 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0104] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 12 hours, and then thawing it at room temperature for 5 hours;
[0105] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0106] Example 8
[0107] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0108] S1. Add 2 g of PVA into 20 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0109] S2, adding 0.12 g of β-CD / PPDO into 20 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 75° C. to obtain a β-CD / PPDO solution;
[0110] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 95°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0111] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 10 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0112] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 12 hours, and then thawing it at room temperature for 1 hour;
[0113] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0114] Example 9
[0115] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0116] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0117] S2, adding 0.16 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 75° C. to obtain a β-CD / PPDO solution;
[0118] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 95°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0119] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 30 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0120] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 12 hours, and then thawing it at room temperature for 3 hours;
[0121] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0122] Example 10
[0123] A β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel is prepared by the following method:
[0124] S1. Add 2 g of PVA into 10 mL of dimethyl sulfoxide aqueous solution, and stir and dissolve in a 95°C constant temperature oil bath to obtain a PVA solution;
[0125] S2, adding 0.18 g of β-CD / PPDO into 10 mL of dimethyl sulfoxide aqueous solution, stirring and dissolving at 60° C. to obtain a β-CD / PPDO solution;
[0126] S3, slowly adding the β-CD / PPDO solution prepared in step S2 to the PVA solution prepared in step S1, and placing the mixture in a 95°C constant temperature oil bath, stirring for 0.5 h to mix evenly, and then stirring for 3.5 h to allow the PVA to fully hydrate and swell, and then cooling to room temperature to obtain a β-CD / PPDO / PVA swelling solution;
[0127] S4, at room temperature, placing the β-CD / PPDO / PVA swelling solution prepared in step S3 in an ultrasonic cleaning machine, and ultrasonicating for 30 minutes to remove bubbles, thereby obtaining a uniform β-CD / PPDO / PVA swelling solution;
[0128] S5, freezing the β-CD / PPDO / PVA swelling solution obtained in step S4 at -18°C for 12 hours, and then thawing it at room temperature for 5 hours;
[0129] S6. Repeat the freeze-thaw operation of step S5 5 times to obtain β-CD / PPDO / PVA hydrogel.
[0130] Comparative Example 1
[0131] A polyvinyl alcohol hydrogel (PVA hydrogel) is prepared by the following method:
[0132] S1. Add 2 g of PVA to 20 mL of dimethyl sulfoxide aqueous solution, and place in a 95°C constant temperature oil bath to stir and dissolve. Continue stirring for 0.5 h to allow the PVA to fully hydrate and swell. After stirring for another 3.5 h, cool to room temperature to obtain a uniform PVA swelling solution.
[0133] S2. At room temperature, the PVA sol prepared in step S1 is placed in an ultrasonic cleaning machine and ultrasonicated for 30 minutes to remove bubbles to obtain a uniform PVA swelling solution;
[0134] S3, freezing the PVA swelling solution obtained in step S2 at -18°C for 12 hours, and then thawing it at room temperature for 5 hours;
[0135] S4. Repeat the freeze-thaw operation of step S3 5 times to obtain a PVA hydrogel.
[0136] Performance Test:
[0137] (I) Microstructural characterization of β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel:
[0138] The β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 10 and the PVA hydrogel prepared in Comparative Example 1 were subjected to infrared testing to verify whether β-CD / PPDO was successfully introduced into the β-CD / PPDO / PVA hydrogel structure. Figure 1 The infrared spectra of the β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 5 and the PVA hydrogel prepared in Comparative Example 1 are shown; Figure 1 It can be seen that compared with the PVA hydrogel of Comparative Example 1, the characteristic peaks in the β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 5 are at a wavelength of 1730 cm -1 Nearby, there is a characteristic peak of C=O, and the characteristic peak in the hydrogel structure is obvious, indicating that β-CD / PPDO is successfully introduced into the β-CD / PPDO / PVA hydrogel structure. Similarly, the infrared spectrum results of Examples 6 to 10 are the same as those of the above examples.
[0139] The brittle fracture surfaces of the β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 10 were subjected to electron microscopic scanning to determine their microstructural characteristics. As shown in FIG2(a), it is a scanning electron microscopic image of the brittle fracture surface on one side of the β-cyclodextrin-modified polydioxanone / polyvinyl alcohol hydrogel prepared in Example 5; as shown in FIG2(b), it is a scanning electron microscopic image of the brittle fracture surface on the other side of the β-cyclodextrin-modified polydioxanone / polyvinyl alcohol hydrogel prepared in Example 5; from the two images, it can be clearly observed that the microstructure of the β-CD / PPDO / PVA hydrogel is a continuous network interpenetrating structure, and uniformly distributed micron pores can be clearly observed on the brittle fracture surface. Similarly, the hydrogel microstructure shown in the scanning electron microscopic images of the brittle fracture surfaces of the β-CD / PPDO / PVA hydrogels prepared in Examples 2 to 10 is the same as the microstructure shown in FIG2.
[0140] As shown in Figure 3(a), it is an atomic force microscope plane image of β-cyclodextrin modified polydioxanone; as shown in Figure 3(b), it is an atomic force microscope stereoscopic scale image of β-cyclodextrin modified polydioxanone; from these two images, it can be observed that in β-cyclodextrin modified polydioxanone, the assembly of PPDO and β-CD is a structure that grows along a straight line, and the particle height of the material is close to 2.0nm, which is close to the outer cavity diameter of β-CD (1.6nm); the particle molecules in the figure are arranged in a linear necklace shape, which proves that cyclodextrin is enclosed in PPDO. The β-CD / PPDO / PVA hydrogel has a polymer network interpenetrating structure and a plurality of cyclodextrin molecules are arranged on the molecular chain; in addition, there are multiple linear lines in the figure, which further proves that the cyclodextrin and PPDO molecular chains are assembled into a whole with a network interpenetrating structure; further, the β-CD / PPDO / PVA hydrogel is a hydrogel with PVA hydrogel as the main material and β-CD / PPDO as the reinforcing material, and the reinforcing material is dispersed in the main material through a dimethyl sulfoxide aqueous solution in a certain appropriate proportion, and a hydrogel with a polymer network interpenetrating structure is formed under the action of hydrogen bonds.
[0141] (II) Mechanical strength test of β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel:
[0142] The β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 10 and the PVA hydrogel prepared in Comparative Example 1 were subjected to a tensile test.
[0143] The specific test method is: fix a long strip of gel of 35mm×20mm×2mm (length×width×height) at both ends of the instrument, and then calculate the tensile strain and tensile strength of the hydrogel at a tensile speed of 100mm / min.
[0144] like Figure 4 Shown are the mechanical tensile curves of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel prepared in Examples 1 to 4 and the polyvinyl alcohol hydrogel prepared in Comparative Example 1; it can be seen from the figure that when the addition amount of β-CD / PPDO in the PVA hydrogel is 1wt.% to 7wt.%, its mechanical properties are greatly improved relative to the PVA hydrogel prepared in Comparative Example 1; specifically, the maximum tensile stress of the β-CD / PPDO / PVA hydrogel is 0.61MPa, which is three times the tensile stress of the PVA hydrogel; the maximum elongation at break of the β-CD / PPDO / PVA hydrogel is 473%, which is twice that of the PVA hydrogel; it can be seen that the mechanical properties and elasticity of the β-CD / PPDO / PVA hydrogel of the present application are greatly improved relative to those of the PVA hydrogel.
[0145] The β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 10 and the PVA hydrogel prepared in Comparative Example 1 were subjected to a compression test.
[0146] The specific test method is as follows: take a 16mm×17mm (diameter×height) cylindrical hydrogel and place it in the test instrument. Under room temperature conditions, compress the gel column sample at a compression speed of 3mm / s, and set the compression deformation to 60%;
[0147] like Figure 5 Shown is a performance curve of mechanical compression of 60% of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel prepared in Examples 1 to 5 and the polyvinyl alcohol hydrogel prepared in Comparative Example 1; it can be seen from the figure that when the addition amount of β-CD / PPDO in the PVA hydrogel is 1% to 10%, the compression performance is better than that of pure PVA hydrogel. Specifically, the maximum compressive stress of the β-CD / PPDO / PVA hydrogel is 0.21 MPa, which is three times that of the PVA hydrogel. It can be seen that the compression performance of the β-CD / PPDO / PVA hydrogel of the present application is greatly improved compared with that of the PVA hydrogel.
[0148] The β-CD / PPDO / PVA hydrogels prepared in Examples 6 to 10 all have the same properties. Specifically, the specific test results of the elongation at break, tensile stress and compressive stress of the β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 10 and the PVA hydrogel prepared in Comparative Example 1 are shown in Table 1 below.
[0149] Table 1:
[0150] Example Elongation at break / % Tensile stress / MPa Compression stress / MPa 1 283 0.25 0.12 2 379 0.29 0.10 3 323 0.55 0.09 4 473 0.60 0.20 5 222 0.09 0.08 6 310 0.24 0.10 7 300 0.30 0.09 8 250 0.26 0.07 9 324 0.31 0.13 10 300 0.12 0.11 Comparative Example 1 285 0.21 0.07
[0151] (III) Swelling-water loss test of β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel:
[0152] The β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 10 and the PVA hydrogel prepared in Comparative Example 1 were subjected to a swelling-water loss test.
[0153] The specific test method is as follows: the hydrogel is placed in a 50°C oven and dried to constant weight, then weighed, and immersed in 37°C deionized water to swell until its weight no longer changes; during the swelling process, it is taken out at certain time intervals, and its weight change is measured after the surface moisture is wiped off to characterize the water absorption performance of the hydrogel; then, the swollen equilibrium sample is placed in room temperature air, and during the water loss process, it is taken out at certain time intervals to measure its weight change to characterize the water loss performance of the hydrogel.
[0154] As shown in Figure 6(a), it is a water absorption curve of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel prepared in Examples 1 to 5 and the polyvinyl alcohol hydrogel prepared in Comparative Example 1; as shown in Figure 6(b), it is a water loss curve of the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel prepared in Examples 1 to 5 and the polyvinyl alcohol hydrogel prepared in Comparative Example 1; it can be seen from the two figures that the β-CD / PPDO / PVA hydrogel of the present application has a water absorption rate similar to that of pure PVA hydrogel, and a significantly reduced water loss rate, that is, the water loss is slow, and the hydrogel can be kept moist for a long time; it can be seen that the β-CD / PPDO / PVA hydrogel of the present application has a greatly optimized water loss performance while maintaining good water absorption performance, and can keep the hydrogel moist for a long time.
[0155] The β-CD / PPDO / PVA hydrogels prepared in Examples 6 to 10 all have the same properties. Specifically, the specific test results of the equilibrium swelling rate and the water storage rate after 12 hours of the β-CD / PPDO / PVA hydrogels prepared in Examples 1 to 10 and the PVA hydrogel prepared in Comparative Example 1 are shown in Table 2 below.
[0156] Table 2:
[0157] Experimental example Equilibrium swelling rate / % Water retention rate after 12h / % Example 1 78.92 93.27 Example 2 71.05 46.13 Example 3 74.68 76.81 Example 4 73.46 76.32 Example 5 77.02 11.32 Example 6 77.14 74.32 Example 7 72.06 66.34 Example 8 75.25 80.20 Example 9 72.25 45.32 Example 10 76.84 30.02 Comparative Example 1 73.66 5.62
Claims
1. A method for preparing a β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel, characterized in that: Here are the steps: S1, dissolving polyvinyl alcohol in a dimethyl sulfoxide aqueous solution to obtain a polyvinyl alcohol solution; wherein the weight average molecular weight of the polyvinyl alcohol is 100,000 to 150,000; S2, dissolving β-cyclodextrin-modified polydioxanone in a dimethyl sulfoxide aqueous solution to obtain a β-cyclodextrin-modified polydioxanone solution; wherein the amount of β-cyclodextrin-modified polydioxanone is 1wt.%~10wt.% of the amount of polyvinyl alcohol; S3, adding the β-cyclodextrin modified polydioxanone solution prepared in step S2 to the polyvinyl alcohol solution prepared in step S1, and placing the mixed solution in a constant temperature oil bath at 70°C to 100°C, stirring for 0.5h to mix evenly, and then stirring for 1.5h to 6.5h to allow the polyvinyl alcohol to be fully hydrated and swollen, and then cooling to room temperature to obtain a polyvinyl alcohol swelling solution in which β-cyclodextrin modified polydioxanone is dispersed; S4, using ultrasound, vacuum or heating to eliminate bubbles in the polyvinyl alcohol swelling solution in which the β-cyclodextrin-modified polydioxanone is dispersed, to obtain a polyvinyl alcohol swelling solution in which the β-cyclodextrin-modified polydioxanone is uniformly dispersed; S5, freezing the swelling solution obtained in step S4 at -18°C for 6h~12h, and then thawing it at room temperature for 1h~5h; S6. Repeat the freezing-thawing operation of step S5 3 to 5 times to obtain β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel.
2. The method for preparing the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel according to claim 1, characterized in that: In step S1 and step S2, the dimethyl sulfoxide aqueous solution is a mixed solution prepared by dimethyl sulfoxide and deionized water in a volume ratio of 3:
10.
3. The method for preparing the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel according to claim 1, characterized in that: In the mixed solution of step S3, the concentration of polyvinyl alcohol in the dimethyl sulfoxide aqueous solution is 0.05-0.20 g / mL.
4. The method for preparing the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel according to claim 1, characterized in that: In step S1, the preparation temperature of the polyvinyl alcohol solution is 95-100°C.
5. The method for preparing the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel according to claim 1, characterized in that: In step S2, the preparation temperature of the β-cyclodextrin modified polydioxanone solution is 60-75°C.
6. The method for preparing the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel according to claim 1, characterized in that: In step S4, an ultrasonic method is used to eliminate bubbles, and the steps are as follows: at room temperature, the container of the swelling solution prepared in step S3 is placed in an ultrasonic cleaning machine, and ultrasonicated for 10 minutes to 30 minutes to obtain a polyvinyl alcohol swelling solution in which β-cyclodextrin-modified polydioxanone is uniformly dispersed.
7. The method for preparing the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel according to claim 1, characterized in that: In step S4, the bubbles are eliminated by vacuuming, and the steps are as follows: at room temperature, the swelling liquid prepared in step S3 is placed in a vacuum oven at a pressure of 0 to -0.1 MPa for 10 to 30 minutes to obtain a polyvinyl alcohol swelling liquid in which β-cyclodextrin-modified polydioxanone is uniformly dispersed.
8. The method for preparing the β-cyclodextrin modified polydioxanone / polyvinyl alcohol hydrogel according to claim 1, characterized in that: In step S4, a heating method is used to eliminate bubbles, and the steps are as follows: at room temperature, the swelling liquid prepared in step S3 is placed in an environment with a temperature of 150° C. to 200° C. for 10 to 30 minutes to obtain a polyvinyl alcohol swelling liquid in which β-cyclodextrin-modified polydioxanone is uniformly dispersed.
9. A β-cyclodextrin-modified poly(p-dioxanone) / poly(vinyl alcohol) hydrogel prepared by the method for preparing a β-cyclodextrin-modified poly(p-dioxanone) / poly(vinyl alcohol) hydrogel according to any one of claims 1 to 8.