Photochromic coating formula

The photochromic coating formulation, through specific components and preparation methods, overcomes the shortcomings of traditional coatings in terms of durability and functionality, achieving self-healing and temperature-sensitive color-changing functions, and is suitable for a variety of high-end application scenarios.

CN118931350APending Publication Date: 2024-11-12东红科技(东莞)有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411188434.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional photochromic coatings are insufficient in terms of durability, functionality, and application scope, making it difficult to meet the needs of industrial, architectural, and high-end decorative fields.

Method used

The photochromic coating formulation is composed of polyurethane resin, thermosetting acrylic resin, fully etherified amino resin, pigments, solvents, additives, graphene nanosheets, hydroxyapatite nanoparticles, superhydrophobic materials, self-healing microcapsules, and temperature-sensitive shape memory polymers. A specific preparation method ensures that all components are uniformly mixed and cured.

Benefits of technology

It achieves self-healing and temperature-sensitive color-changing functions in coatings, enhances environmental stability and weather resistance, and is suitable for high-end industries, intelligent buildings and personalized decoration, extending the service life and aesthetics of coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931350A_ABST
    Figure CN118931350A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and discloses a photochromic coating formula which is prepared from the following components in parts by weight: 23 to 25 parts of polyurethane resin, 8 to 10 parts of thermosetting acrylic resin, 5 to 8 parts of full-etherified amino resin, 25 to 30 parts of pigment, 30.5 to 35.5 parts of solvent, 3.0 to 4.3 parts of additive, 0.1 to 0.5 part of graphene nanosheet, 0.5 to 1.0 part of hydroxyapatite nanoparticle and 1 to 2 parts of super-hydrophobic material. The invention further discloses a preparation method of the photochromic coating. The preparation method comprises the following steps: S1, premixing the solvent and the resin: mixing the cyclohexanone, the xylene, the butyl ester and the methyl isobutyl ketone in a reaction container; by introducing the self-healing microcapsule, the temperature-sensitive shape memory polymer and nano materials such as graphene and hydroxyapatite, multiple functions such as self-healing and temperature-sensitive color change are achieved, the application of the coating is increased, and the coating is suitable for multiple fields such as high-end industry, intelligent buildings and personalized decoration and has wide application prospects. The problem that an existing coating always focuses on a single function is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a photochromic coating formula. Background Art

[0002] Paint is a material that can be applied to the surface of an object using different construction processes to form a solid film that is firmly adhered, has a certain strength, and is continuous. The film formed in this way is generally called a coating film, also known as a paint film or a coating. It belongs to organic chemical polymer materials, and the coating film formed belongs to the type of polymer compounds. According to the classification of modern chemical products, paint belongs to fine chemical products. Modern paint is gradually becoming a multifunctional engineering material and an important industry in the chemical industry.

[0003] Optically variable paint is a type of paint that contains photochromic microcapsules that produce color when exposed to ultraviolet light. This change is usually reversible, allowing the paint to return to its original state after the light conditions change. This feature makes optically variable paint widely used in toys, textiles, decorations, and high-tech product packaging, especially in increasing the interactivity and aesthetics of products.

[0004] However, as consumers' demand for high-performance coatings increases, the functionality of traditional coatings can no longer fully meet the needs of the market. Especially in the fields of industry, construction and high-end decoration, the functional requirements for coatings include weather resistance, self-cleaning ability, environmental adaptability and intelligent response. These demands have promoted the development of functional coatings. Traditional photochromic coatings are still lacking in functionality. They are still mostly used in the fields of decoration and art. They are rarely used in industrial or high-performance applications due to their lack of functionality. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a photochromic coating formula, which solves the problems of traditional photochromic coatings in terms of durability, functionality, reversibility and breadth of application.

[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: a photochromic coating formula, which includes, by weight, 23-25 ​​parts of polyurethane resin, 8-10 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin, 25-30 parts of pigment, 30.5-35.5 parts of solvent, 3.0-4.3 parts of additive, 0.1-0.5 parts of graphene nanosheets, 0.5-1.0 parts of hydroxyapatite nanoparticles, 1-2 parts of superhydrophobic material, 1-3 parts of self-healing microcapsules and 0.5-1.5 parts of thermosensitive shape memory polymer.

[0007] Preferably, the solvent comprises, by weight, 4.5-5.5 parts of cyclohexanone, 7-8 parts of xylene, 11-12 parts of butyl ester and 8-10 parts of methyl isobutyl ketone.

[0008] Preferably, the auxiliary agent comprises, by weight, 0.8-1.3 parts of a leveling agent, 1.5-2.0 parts of a defoaming agent and 0.7-1.0 parts of a dispersant.

[0009] Preferably, the pigment is an electron transfer type organic compound, the defoamer is a silicon defoamer, and the dispersant is a high molecular copolymer alkyl ammonium salt dispersant.

[0010] Preferably, the super hydrophobic material is one of modified silica nanoparticles or fluoride-modified silicone resin.

[0011] Preferably, the self-healing microcapsules are selected from polyurethane microcapsules, polyurea microcapsules or epoxy resin microcapsules containing a repairing agent.

[0012] Preferably, the temperature-sensitive shape memory polymer is one of polycaprolactone diol and shape memory polyurethane.

[0013] A method for preparing a photochromic coating comprises the following steps:

[0014] S1: Premixed solvent and resin:

[0015] Mix cyclohexanone, xylene, butyl ester and methyl isobutyl ketone in a reaction vessel, set the temperature range to 20-30°C, the stirring speed to 450-550rpm, and the continuous stirring time to 8-12min;

[0016] S2, resin dissolution:

[0017] Gradually add polyurethane resin, thermosetting acrylic resin and fully etherified amino resin to the solvent mixture, stirring for 25-35 minutes, and controlling the temperature at 28-32°C to ensure complete dissolution of the resin;

[0018] S3: Adding functional nanomaterials:

[0019] Dispersion of Nanomaterials:

[0020] The graphene nanosheets, hydroxyapatite nanoparticles, and selected superhydrophobic materials were pretreated using an ultrasonic device, with the ultrasonic frequency set to 35-45 kHz and the treatment time set to 12-18 min to optimize the dispersibility;

[0021] Adding nanomaterials to the resin solution:

[0022] Slowly add the ultrasonically treated nanomaterials into the resin solution under low-speed stirring at 250-350 rpm for 40-50 min and keep the temperature at 32-38°C;

[0023] S4: Adding additives and pigments:

[0024] Additives:

[0025] Add leveling agent, defoamer and dispersant to the mixture, set the stirring speed to 550-650rpm and the stirring time to 8-12min to ensure that the additives are completely evenly distributed;

[0026] Pigment addition:

[0027] Add electron transfer organic compound pigment, set the temperature to 38-42°C, and continue stirring for 50-70 minutes;

[0028] S5: Adding self-healing microcapsules and thermosensitive shape memory polymers:

[0029] Self-healing microcapsules:

[0030] Slowly add the selected self-healing microcapsules, stirring for 15-25 minutes, and controlling the temperature at 43-47°C;

[0031] Thermosensitive shape memory polymers:

[0032] Add the selected thermosensitive shape memory polymer, stir for 25-35 min, and raise the temperature to 48-52 °C to promote the compatibility of the polymer with the coating matrix;

[0033] S6: coating film formation and curing:

[0034] Coating film formation:

[0035] Use a film spreader to coat the test plate, the film thickness is controlled at 90-210 μm, the ambient room temperature is set at 24-26°C and the relative humidity is 48-52%;

[0036] Curing process:

[0037] The primary curing is carried out at 55-65°C for 50-70 minutes, and the secondary curing temperature is 115-125°C, lasting 100-140 minutes to complete the curing process of the coating.

[0038] The present invention provides a photochromic coating formula having the following beneficial effects:

[0039] 1. The present invention realizes multiple functions such as self-healing and temperature-sensitive color change by introducing self-healing microcapsules, temperature-sensitive shape memory polymers, and nanomaterials such as graphene and hydroxyapatite, thereby increasing the use of coatings and being suitable for various fields such as high-end industry, intelligent buildings, and personalized decoration, solving the problem that existing coatings often focus on a single function.

[0040] 2. The present invention enhances the environmental stability and weather resistance of the coating by using super-hydrophobic materials such as modified silica nanoparticles and fluoride-modified silicone resins, thereby improving the durability and protective effects in various environments.

[0041] 3. The present invention introduces self-healing materials such as polyurethane microcapsules, polyurea microcapsules or epoxy resin microcapsules containing repair agents to give the coating a self-healing function, which can automatically repair minor damages, greatly extending the service life and aesthetics of the coating.

[0042] 4. The present invention integrates shape memory polymers and electron transfer organic compound pigments to enable the coating to have a temperature-sensitive color-changing function, which can change color at a specific temperature and be used for safety marking, temperature warnings or decorative art. At the same time, this change is reversible and can be repeated. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0044] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] Please see attached Figure 1 The embodiment of the present invention provides a photochromic coating formula, which includes, by weight, 23-25 ​​parts of polyurethane resin, 8-10 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin, 25-30 parts of pigment, 30.5-35.5 parts of solvent, 3.0-4.3 parts of additive, 0.1-0.5 parts of graphene nanosheets, 0.5-1.0 parts of hydroxyapatite nanoparticles, 1-2 parts of superhydrophobic material, 1-3 parts of self-healing microcapsules and 0.5-1.5 parts of thermosensitive shape memory polymer.

[0046] The solvent comprises, by weight, 4.5-5.5 parts of cyclohexanone, 7-8 parts of xylene, 11-12 parts of butyl ester and 8-10 parts of methyl isobutyl ketone.

[0047] The additives include, by weight, 0.8-1.3 parts of leveling agent, 1.5-2.0 parts of defoaming agent and 0.7-1.0 parts of dispersant.

[0048] The pigment is an electron transfer type organic compound, the defoamer is a silicon defoamer, and the dispersant is a high molecular copolymer alkyl ammonium salt dispersant.

[0049] The super hydrophobic material is optionally one of modified silica nanoparticles or fluoride-modified silicone resin.

[0050] The self-healing microcapsule is selected from polyurethane microcapsule, polyurea microcapsule or epoxy resin microcapsule containing a repairing agent.

[0051] The thermosensitive shape memory polymer is optionally one of polycaprolactone diol and shape memory polyurethane.

[0052] A method for preparing a photochromic coating, characterized in that it is prepared using a photochromic coating formulation according to any one of claims 1 to 7, comprising the following steps:

[0053] S1: Premixed solvent and resin:

[0054] Mix cyclohexanone, xylene, butyl ester and methyl isobutyl ketone in a reaction vessel, set the temperature range to 20-30°C, the stirring speed to 450-550rpm, and the continuous stirring time to 8-12min;

[0055] S2, resin dissolution:

[0056] Gradually add polyurethane resin, thermosetting acrylic resin and fully etherified amino resin to the solvent mixture, stirring for 25-35 minutes, and controlling the temperature at 28-32°C to ensure complete dissolution of the resin;

[0057] S3: Adding functional nanomaterials:

[0058] Dispersion of Nanomaterials:

[0059] The graphene nanosheets, hydroxyapatite nanoparticles, and selected superhydrophobic materials were pretreated using an ultrasonic device, with the ultrasonic frequency set to 35-45 kHz and the treatment time set to 12-18 min to optimize the dispersibility;

[0060] Adding nanomaterials to the resin solution:

[0061] Slowly add the ultrasonically treated nanomaterials into the resin solution under low-speed stirring at 250-350 rpm for 40-50 min and keep the temperature at 32-38°C;

[0062] S4: Adding additives and pigments:

[0063] Additives:

[0064] Add leveling agent, defoamer and dispersant to the mixture, set the stirring speed to 550-650rpm and the stirring time to 8-12min to ensure that the additives are completely evenly distributed;

[0065] Pigment addition:

[0066] Add electron transfer organic compound pigment, set the temperature to 38-42°C, and continue stirring for 50-70 minutes;

[0067] S5: Adding self-healing microcapsules and thermosensitive shape memory polymers:

[0068] Self-healing microcapsules:

[0069] Slowly add the selected self-healing microcapsules, stirring for 15-25 minutes, and controlling the temperature at 43-47°C;

[0070] Thermosensitive shape memory polymers:

[0071] Add the selected thermosensitive shape memory polymer, stir for 25-35 min, and raise the temperature to 48-52 °C to promote the compatibility of the polymer with the coating matrix;

[0072] S6: coating film formation and curing:

[0073] Coating film formation:

[0074] Use a film spreader to coat the test plate, the film thickness is controlled at 90-210 μm, the ambient room temperature is set at 24-26°C and the relative humidity is 48-52%;

[0075] Curing process:

[0076] The primary curing is carried out at 55-65°C for 50-70 minutes, and the secondary curing temperature is 115-125°C, lasting 100-140 minutes to complete the curing process of the coating.

[0077] Embodiment 1:

[0078] formula:

[0079] Polyurethane resin: 23 parts

[0080] Thermosetting acrylic resin: 10 parts

[0081] Fully etherified amino resin: 5 parts

[0082] Pigment: 25 parts

[0083] Solvent: 4.5 parts of cyclohexanone, 7 parts of xylene, 11 parts of butyl ester, 8 parts of methyl isobutyl ketone

[0084] Additives: 0.8 parts of leveling agent, 1.5 parts of defoaming agent, 0.7 parts of dispersant

[0085] Graphene nanosheets: 0.1 parts

[0086] Hydroxyapatite nanoparticles: 0.5 parts

[0087] Super hydrophobic material (modified silica nanoparticles): 1 part

[0088] Self-healing microcapsules (polyurethane microcapsules): 1 part

[0089] Thermosensitive shape memory polymer (polycaprolactone diol): 0.5 parts

[0090] Preparation method:

[0091] S1: Mixing of solvent and resin

[0092] Combine all solvents in a reaction vessel: cyclohexanone, xylene, butyl esters, and methyl isobutyl ketone.

[0093] The temperature was set to 25°C and the stirring speed was 500 rpm for 10 minutes.

[0094] S2: Resin dissolution

[0095] The polyurethane resin, the thermosetting acrylic resin and the fully etherified amino resin are gradually added to the solvent mixture.

[0096] Continue stirring for 30 minutes, controlling the temperature at 30°C to ensure that the resin is completely dissolved.

[0097] S3: Adding functional nanomaterials

[0098] The graphene nanosheets and hydroxyapatite nanoparticles were pretreated using an ultrasonic device with an ultrasonic frequency of 40 kHz and a treatment time of 15 minutes.

[0099] The treated nanomaterials were added to the resin solution and stirred at a low speed (300 rpm) for 40 minutes.

[0100] S4: Adding pigments and additives

[0101] The pigment was added to the mixture and the stirring speed was increased to 550 rpm for 60 minutes at a temperature of 40°C.

[0102] Add leveling agent, defoamer and dispersant and continue stirring for 15 minutes.

[0103] S5: Adding self-healing microcapsules and thermosensitive shape memory polymers

[0104] Slowly add polyurethane microcapsules and polycaprolactone diol and stir for 20 minutes at a temperature of 45°C.

[0105] S6: Coating film formation and curing

[0106] Use a film spreader to apply on the test plate and control the film thickness to be 150 μm.

[0107] The ambient room temperature was set to 25°C and the relative humidity to 50%.

[0108] The primary cure was carried out at 60°C for 60 minutes and the secondary cure was at 120°C for 120 minutes.

[0109] Summary: Example 1 shows a basic photochromic coating formulation that provides good basic performance through a reasonable combination of raw materials. The use of graphene nanosheets and hydroxyapatite nanoparticles enhances the mechanical strength and durability of the coating, while the addition of polyurethane microcapsules and polycaprolactone diol provides self-healing ability and temperature responsiveness, which is suitable for application scenarios that require basic protection and color change functions.

[0110] Embodiment 2:

[0111] formula:

[0112] Polyurethane resin: 25 parts

[0113] Thermosetting acrylic resin: 10 parts

[0114] Fully etherified amino resin: 8 parts

[0115] Pigment: 30 parts

[0116] Solvent: 5.5 parts of cyclohexanone, 8 parts of xylene, 12 parts of butyl ester, 10 parts of methyl isobutyl ketone

[0117] Additives: 1.3 parts of leveling agent, 2.0 parts of defoaming agent, 1.0 parts of dispersant

[0118] Graphene nanosheets: 0.3 parts

[0119] Hydroxyapatite nanoparticles: 0.8 parts

[0120] Super hydrophobic material (fluoride-modified silicone resin): 1.5 parts

[0121] Self-healing microcapsules (epoxy resin microcapsules containing repairing agents): 2 parts

[0122] Thermosensitive shape memory polymer (shape memory polyurethane): 1.0 part

[0123] Preparation method:

[0124] S1: Mixing of solvent and resin

[0125] Cyclohexanone, xylene, butyl ester and methyl isobutyl ketone were added to a reaction vessel and mixed.

[0126] The temperature was set to 28°C and the stirring speed was 520 rpm for 12 minutes.

[0127] S2: Resin dissolution

[0128] Gradually add polyurethane resin, thermosetting acrylic resin and fully etherified amino resin into the mixed solvent.

[0129] Stirring was continued for 35 minutes, maintaining the temperature at 32°C.

[0130] S3: Adding functional nanomaterials

[0131] The graphene nanosheets and hydroxyapatite nanoparticles were pretreated using an ultrasonic device with an ultrasonic frequency of 40 kHz and a treatment time of 15 minutes.

[0132] The treated nanomaterials were added to the resin solution under low-speed stirring (300 rpm) and stirring was continued for 40 minutes, with the temperature maintained at 35°C.

[0133] S4: Adding pigments and additives

[0134] The pigment was gradually added, the stirring speed was increased to 600 rpm, and the mixture was continued for 70 minutes, and the temperature was adjusted to 42°C.

[0135] Add leveling agent, defoamer and dispersant and continue stirring for 12 minutes.

[0136] S5: Adding self-healing microcapsules and thermosensitive shape memory polymers

[0137] Slowly add the epoxy resin microcapsules containing the healing agent and the shape memory polyurethane, stir for 20 minutes, and set the temperature to 47°C.

[0138] S6: Coating film formation and curing

[0139] Use a film spreader to apply on a test plate and control the film thickness to be 200 μm.

[0140] The ambient room temperature was set at 26°C and the relative humidity was 52%.

[0141] The primary cure was carried out at 65°C for 70 minutes and the secondary cure temperature was set at 125°C for 140 minutes.

[0142] Summary: Example 2 uses a higher proportion of functional additives, especially the addition of shape memory polyurethane and epoxy resin microcapsules containing repair agents, which significantly improves the self-healing ability and shape adaptability of the coating. This formulation is suitable for more demanding environments, such as exterior construction or high-end decorative applications, which require higher weather resistance and long-term stability.

[0143] Embodiment 3:

[0144] formula:

[0145] Polyurethane resin: 24 parts

[0146] Thermosetting acrylic resin: 10 parts

[0147] Fully etherified amino resin: 5 parts

[0148] Pigment: 25 parts

[0149] Solvent: 5 parts cyclohexanone, 8 parts xylene, 12 parts butyl ester, 9 parts methyl isobutyl ketone

[0150] Additives: 1 part of leveling agent, 2 parts of defoaming agent, 1 part of dispersant

[0151] Graphene nanosheets: 0.5 parts

[0152] Hydroxyapatite nanoparticles: 1.0 part

[0153] Super hydrophobic material (modified silica nanoparticles): 2 parts

[0154] Self-healing microcapsules (polyurea microcapsules): 3 parts

[0155] Thermosensitive shape memory polymer (shape memory polyurethane): 1.5 parts

[0156] Preparation method

[0157] S1: Mixing of solvent and resin

[0158] Cyclohexanone, xylene, butyl esters and methyl isobutyl ketone are mixed in a reaction vessel.

[0159] The temperature was set at 27°C and the stirring speed was 530 rpm for 11 minutes.

[0160] S2: Resin dissolution

[0161] The polyurethane resin, the thermosetting acrylic resin and the fully etherified amino resin are gradually added to the solvent mixture.

[0162] Stirring was continued for 35 minutes, the temperature being maintained at 31°C.

[0163] S3: Adding functional nanomaterials

[0164] The graphene nanosheets and hydroxyapatite nanoparticles were treated with ultrasound at a frequency of 40 kHz for 15 min.

[0165] The nanomaterials were added to the resin solution and stirred for 40 minutes, maintaining the temperature at 38 °C.

[0166] S4: Adding pigments and additives

[0167] The pigment was slowly added and stirred, the stirring speed was increased to 650 rpm, and the stirring was continued for 60 minutes, and the temperature was set to 41°C.

[0168] After the additives were added, stirring was continued for 15 minutes.

[0169] S5: Adding self-healing microcapsules and thermosensitive shape memory polymers

[0170] Add polyurea microcapsules and shape memory polyurethane, stir for 25 minutes, and adjust the temperature to 50°C.

[0171] S6: Coating film formation and curing

[0172] The film was applied on a test plate using a film spreader to a film thickness of 190 μm.

[0173] The indoor ambient temperature was set at 25°C and the relative humidity was 50%.

[0174] The primary cure was carried out at 63°C for 65 minutes and the secondary cure was at 123°C for 130 minutes.

[0175] Summary: Example 3 uses the highest share of advanced functional materials, including the largest amount of polyurea microcapsules and the highest share of modified silica nanoparticles, to provide the coating with extremely high wear resistance and self-healing capabilities. This formulation is particularly suitable for high-end industrial applications such as automotive or aerospace, where the coating may be challenged by frequent mechanical stress or environmental changes.

[0176] Summary:

[0177] These three examples reflect the evolution of photochromic coatings from basic to advanced applications. By adjusting specific components in the formula, such as the type and amount of self-healing microcapsules, the type of nanomaterials, and the proportion of additives, the performance and applicability of the coating can be significantly affected. Example 1 provides basic self-healing and color change properties, while Examples 2 and 3 gradually enhance the functionality of the coating to enable it to adapt to more complex and demanding use environments. These examples demonstrate the development of high-performance coatings suitable for a variety of environments from home decoration to industrial-grade applications. Each example clearly shows that by adjusting specific raw materials and preparation steps, a coating solution that meets specific needs can be formulated.

[0178] Test experiment and its contents:

[0179] Purpose:

[0180] Mechanical properties testing: Evaluate the hardness and abrasion resistance of the coating.

[0181] Self-healing ability test: verify the self-healing effect of the coating after being scratched.

[0182] Thermochromic Test: Tests the ability of a coating to change color in response to changes in temperature.

[0183] Durability test: Check the stability and color retention of coatings after long-term exposure to outdoor environments.

[0184] Experimental design:

[0185] Experiment 1: Mechanical properties test

[0186] Hardness test:

[0187] Method: The hardness of the coating was tested using a Shore hardness tester.

[0188] Results: Record the hardness value to assess the material's ability to resist compression.

[0189] Wear test:

[0190] Method: Carry out wear resistance test by a wear tester and record the weight difference before and after wear.

[0191] Result: Lower weight loss indicates better wear resistance.

[0192] Experiment 2: Self-healing ability test

[0193] Method: After making surface scratches, the sample was placed in a temperature-controlled box at a set temperature to observe the self-healing process.

[0194] Conditions: 24 hours at 55°C.

[0195] Results: The percentage reduction in scratch width evaluated the self-healing effect.

[0196] Experiment 3: Temperature-sensitive color change test

[0197] Method: Place the sample in a temperature-controlled box and gradually adjust the temperature from 20°C to 60°C.

[0198] Results: The color changes at different temperatures were recorded using a colorimeter and expressed as ΔE values.

[0199] Experiment 4: Durability Test

[0200] Method: The coating samples were placed in an outdoor environment for long-term exposure testing.

[0201] Duration: 6 months.

[0202] The result: Regularly check the coating's adhesion, gloss and color stability to assess the long-term performance of the coating.

[0203] Table 1:

[0204]

[0205] Experimental summary:

[0206] The above test experiments and their results demonstrate the potential effects of various embodiments in different aspects. From hardness to wear resistance, self-healing ability, and response to temperature changes, each embodiment is designed to demonstrate its specific advantages. For example:

[0207] Example 1 provides a basic level of hardness and self-healing effect, and is suitable for general applications.

[0208] Example 2 has improvements in all performance indicators, especially in self-healing and durability, and is suitable for more demanding environments.

[0209] Example 3 showed the best performance, especially in self-healing and durability tests, and is most suitable for high-end applications such as automotive or aviation.

[0210] Comparative experiment and its experimental content:

[0211] Purpose of comparative experiment:

[0212] 1. Mechanical properties test: Compare the hardness and wear resistance of four coatings.

[0213] 2. Self-healing ability test: evaluate the self-healing efficiency of the coating after physical damage.

[0214] 3. Thermosensitive color change test: test the paint's ability to respond to temperature changes.

[0215] 4. Durability test: Analyze the performance of the coating after long-term exposure to the external environment.

[0216] Experimental sample description:

[0217] Innovative coatings: The photochromic coatings of the present invention are formulated with high-performance additives such as specific self-healing microcapsules and thermosensitive shape memory polymers.

[0218] Standard Polyurethane Coating: Conventional polyurethane coating for general decorative and protective applications without special functional additives.

[0219] Commercial color-changing paints: Thermosensitive color-changing paints are commercially available and are primarily used for decorative and artistic applications.

[0220] Conventional Anticorrosion Coatings: Traditional coatings used for corrosion and rust prevention, suitable for industrial and marine applications.

[0221] Experimental design and steps:

[0222] Experiment 1: Mechanical properties test

[0223] Hardness test:

[0224] The hardness of all samples was tested using a Shore durometer.

[0225] Abrasion resistance test:

[0226] The wear resistance test was carried out using an abrasion tester, and the weight difference before and after wear was recorded.

[0227] Experiment 2: Self-healing ability test

[0228] Create scratches of equal depth on each paint surface.

[0229] The samples were placed in a 55°C environment for 24 hours.

[0230] The changes in scratch width were observed and recorded to evaluate the self-healing effect.

[0231] Experiment 3: Temperature-sensitive color change test

[0232] All paint samples were placed in a controlled temperature box and the temperature was gradually adjusted from 20°C to 60°C.

[0233] Use a colorimeter to record the color changes at different temperatures.

[0234] Experiment 4: Durability Test

[0235] All paint samples were placed in an outdoor environment for long-term exposure testing, with the duration set at 6 months.

[0236] Check coating adhesion, gloss and color stability regularly.

[0237] Table 2:

[0238]

[0239]

[0240] Experimental summary:

[0241] The experimental results of the comparative experiment clearly show that the photochromic coating of the present invention is superior to the traditional coating in multiple key performance indicators:

[0242] Hardness and wear resistance: The innovative coating exhibits higher hardness and lower loss of wear resistance, meaning better mechanical protection and durability.

[0243] Self-healing ability: The self-healing effect of the innovative coating is significantly higher than that of other types of coatings, especially in terms of its ability to repair itself after physical damage.

[0244] Thermochromic: Thermochromic ability is also excellent, which is not available in commercial color-changing paints, providing more application possibilities such as temperature warnings and decorative effects.

[0245] Durability: In long-term outdoor exposure tests, the innovative coatings maintained high levels of color stability, adhesion and gloss, which is particularly important for applications that require long-term exterior use.

[0246] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A photochromic coating formulation, characterized in that: In parts by weight, the invention comprises 23-25 ​​parts of polyurethane resin, 8-10 parts of thermosetting acrylic resin, 5-8 parts of fully etherified amino resin, 25-30 parts of pigment, 30.5-35.5 parts of solvent, 3.0-4.3 parts of additive, 0.1-0.5 parts of graphene nanosheets, 0.5-1.0 parts of hydroxyapatite nanoparticles, 1-2 parts of superhydrophobic material, 1-3 parts of self-healing microcapsules and 0.5-1.5 parts of thermosensitive shape memory polymer.

2. A photochromic coating formulation according to claim 1, characterized in that: The solvent comprises, by weight, 4.5-5.5 parts of cyclohexanone, 7-8 parts of xylene, 11-12 parts of butyl ester and 8-10 parts of methyl isobutyl ketone.

3. A photochromic coating formulation according to claim 1, characterized in that: The auxiliary agent comprises, by weight, 0.8-1.3 parts of a leveling agent, 1.5-2.0 parts of a defoaming agent and 0.7-1.0 parts of a dispersant.

4. A photochromic coating formulation according to claim 1, characterized in that: The pigment is an electron transfer type organic compound, the defoamer is a silicon defoamer, and the dispersant is a high molecular copolymer alkyl ammonium salt dispersant.

5. A photochromic coating formulation according to claim 1, characterized in that: The super hydrophobic material is optionally modified silica nanoparticles or fluoride-modified silicone resin.

6. A photochromic coating formulation according to claim 1, characterized in that: The self-healing microcapsules are selected from polyurethane microcapsules, polyurea microcapsules or epoxy resin microcapsules containing a repairing agent.

7. A photochromic coating formulation according to claim 1, characterized in that: The temperature-sensitive shape memory polymer is optionally one of polycaprolactone diol and shape memory polyurethane.

8. A method for preparing a photochromic coating, characterized in that: The photochromic coating is prepared by using a photochromic coating formulation as described in any one of claims 1 to 7, comprising the following steps: S1: Premixed solvent and resin: Mix cyclohexanone, xylene, butyl ester and methyl isobutyl ketone in a reaction vessel, set the temperature range to 20-30°C, the stirring speed to 450-550rpm, and the continuous stirring time to 8-12min; S2, resin dissolution: Gradually add polyurethane resin, thermosetting acrylic resin and fully etherified amino resin to the solvent mixture, stirring for 25-35 minutes, and controlling the temperature at 28-32°C to ensure complete dissolution of the resin; S3: Adding functional nanomaterials: Dispersion of Nanomaterials: The graphene nanosheets, hydroxyapatite nanoparticles, and selected superhydrophobic materials were pretreated using an ultrasonic device, with the ultrasonic frequency set to 35-45 kHz and the treatment time set to 12-18 min to optimize the dispersibility; Adding nanomaterials to the resin solution: Slowly add the ultrasonically treated nanomaterials into the resin solution under low-speed stirring at 250-350 rpm for 40-50 min and keep the temperature at 32-38°C; S4: Adding additives and pigments: Additives: Add leveling agent, defoamer and dispersant to the mixture, set the stirring speed to 550-650rpm and the stirring time to 8-12min to ensure that the additives are completely evenly distributed; Pigment addition: Add electron transfer organic compound pigment, set the temperature to 38-42°C, and continue stirring for 50-70 minutes; S5: Adding self-healing microcapsules and thermosensitive shape memory polymers: Self-healing microcapsules: Slowly add the selected self-healing microcapsules, stirring for 15-25 minutes, and controlling the temperature at 43-47°C; Thermosensitive shape memory polymers: Add the selected thermosensitive shape memory polymer, stir for 25-35 min, and raise the temperature to 48-52 °C to promote the compatibility of the polymer with the coating matrix; S6: coating film formation and curing: Coating film formation: Use a film spreader to coat the test plate, the film thickness is controlled at 90-210 μm, the ambient room temperature is set at 24-26°C and the relative humidity is 48-52%; Curing process: The primary curing is carried out at 55-65°C for 50-70 minutes, and the secondary curing temperature is 115-125°C, lasting 100-140 minutes to complete the curing process of the coating.

Citation Information

Cited By

  • Coating structure for water conservancy project