A kind of lightweight melamine waterproof foam plastic and preparation method thereof

Through the use of modified melamine formaldehyde resin and composite catalysts, combined with surfactants and foaming agents, lightweight melamine waterproof foam plastics with significant waterproof properties are prepared, which solves the problem of insufficient waterproof properties of existing foams.

CN115895185BActive Publication Date: 2024-10-25JIAXING HANGXING FINE CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211447676.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-10-25
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

The existing melamine foam has poor waterproof performance and is difficult to meet the high waterproof requirements in the construction, petrochemical, and cold storage fields.

Method used

Using a composite catalyst of modified melamine formaldehyde resin, potassium acetate and ammonium chloride, combined with surfactants and foaming agents, lightweight melamine waterproof foam plastics are prepared through specific process steps to form a stronger molecular chain cross-linked structure to enhance the Waterproof effect.

Benefits of technology

Significantly improves the waterproof performance of foam plastics and improves its compressive strength and waterproof effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003950087340000091
    Figure BDA0003950087340000091
  • Figure BDA0003950087340000101
    Figure BDA0003950087340000101
Patent Text Reader

Abstract

The invention discloses a lightweight melamine waterproof foam plastic, which is composed of the following components in weight percentage: 2-5% of a surfactant, 0.5-1.2% of a composite catalyst, 3-8% of a foaming agent and the remainder of a modified melamine formaldehyde resin. The lightweight melamine waterproof foam plastic adopts a modified melamine formaldehyde resin to replace a traditional melamine resin, and adopts a mixture of potassium acetate and ammonium chloride as a composite catalyst. The prepared melamine molecular chain cross-linking is more complex, and the network structure is more solid, so it has excellent compression strength; at the same time, the complex cross-linking structure significantly improves the waterproof effect of the foam plastic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing foam plastics, in particular to a lightweight melamine waterproof foam plastic and a preparation method thereof, belonging to the technical field of foam plastics. Background Art

[0002] Melamine foam (also known as melamine foam or nanosponge) is a thermosetting elastic organic rubber-plastic foam made of melamine multi-base formaldehyde resin foamed by microwave, with a fine three-dimensional network structure with high open pores. Outlet melamine foam has excellent comprehensive performance and is widely used in architectural acoustics, professional acoustics, rail vehicles, automobile manufacturing, shipbuilding, aerospace applications, pipeline insulation, high temperature insulation, low temperature insulation, power stations, filtration applications, large equipment manufacturing, antistatic, 5G base stations, white appliances, supercapacitors, industrial cleaning, daily cleaning, furniture manufacturing and other fields.

[0003] Melamine foam has nine excellent properties, including:

[0004] 1. Sound absorption performance

[0005] Melamine foam is a fully open-cell three-dimensional grid structure system with a grid aspect ratio (L / D) between 10-20 and a density of 8.5KG / M3. The open-cell rate of melamine foam plastic is as high as over 99%, which allows sound waves to easily and effectively enter the deep layer of the foam and be converted into grid vibrations to be consumed and absorbed, and can effectively eliminate reflected waves, especially for mid- and high-frequency noise. It has outstanding absorption characteristics; melamine foam can be processed into acoustic sound-absorbing panels, pyramid wedges, wedges, suspended sound absorbers and other acoustic materials, which can be widely used in various architectural acoustics, professional acoustics and equipment acoustics.

[0006] 2. Flame retardant properties

[0007] Since melamine foam is made of melamine foamed by microwave, melamine itself is a flame retardant material with a nitrogen content of up to 70%. Therefore, melamine foam does not need to add any flame retardant to achieve excellent flame retardant properties. The surface will only start to burn when it comes into contact with an open flame. After combustion, it will immediately decompose and produce a large amount of inert non-combustible gas, nitrogen, thereby isolating oxygen and slowing down the combustion rate. At the same time, a dense coke layer is quickly formed on the surface of the combustion body to effectively prevent the combustion from developing to a deeper level. It will automatically extinguish after the open flame is removed, that is, it will extinguish as soon as the fire is removed.

[0008] 3. Weather resistance

[0009] Melamine foam is a thermosetting organic plastic with a highly fine three-dimensional network cross-linked structure. Compared with polyethylene, polystyrene thermoplastic materials and polyurethane materials with a lower degree of cross-linking, it has higher thermal stability and aging resistance. It can work for a long time in an environment of -180 degrees Celsius to 200 degrees Celsius, and can withstand a maximum temperature of 240 degrees Celsius without decomposition or deformation. It will only show obvious decomposition in a high temperature environment above 400 degrees Celsius (the working temperature of polyolefin, polystyrene, polyurethane and other foam plastics is only 80 degrees Celsius, and deformation and decomposition will occur when it exceeds 80 degrees Celsius).

[0010] 4. Thermal insulation performance

[0011] Melamine foam is a fully open-cell three-dimensional grid structure system with a grid aspect ratio (L / D) between 10-20 and a density of 8.5KG / M3. The porosity of melamine foam is as high as over 99%. The fine three-dimensional grid structure effectively prevents the convection heat transfer of air. In addition, its unique low thermal stability gives it good thermal insulation effect (thermal conductivity, 0.035W / (m*K)), making it an irreplaceable lightweight thermal insulation material.

[0012] 5. Lightweight

[0013] Melamine foam is a fully open-cell three-dimensional grid structure system with a grid aspect ratio (L / D) between 10-20 and a minimum density of 8.5KG / M3. It is one of the lightest foams in the world and can be used for aircraft seat filling.

[0014] 6. Chemical resistance

[0015] Melamine foam is a thermosetting organic plastic with a highly fine three-dimensional network cross-linked structure, which can resist many organic solvents. Melamine foam is acid and alkali resistant, mildew resistant, and antibacterial.

[0016] 7. Abrasiveness

[0017] The hardness of melamine foam is as hard as fiberglass, but the fine cell structure provides the product with flexibility. When melamine foam is moistened with water, surface dirt can be easily wiped off. Melamine foam is one of the great cleaning materials of the 21st century.

[0018] 8. Environmentally friendly

[0019] Melamine foam is mainly made of melamine multi-base formaldehyde resin. It does not contain other compounds and is non-fiber. It does not contain any dust, halogenated hydrocarbons, flame retardants, or toxic heavy metals. At the same time, the formaldehyde emission of melamine foam produced by Outlet Technology reaches the EU EN717-7 maximum 0.1ppm indoor decoration environmental protection standard, and is one of the safe and environmentally friendly building acoustic materials in China.

[0020] 9. Secondary processing formability

[0021] Melamine foam is a thermosetting elastic organic rubber-plastic foam with a fine three-dimensional mesh structure. In addition to being easy to cut or CNC process, it can also be composited with other materials, such as hot-pressed with non-woven fabrics, aluminum foil, PVC and other materials to form parts, which are widely used in automobile engine sound insulation pads; it can also be treated with hydrophobicity and oleophobicity, and is widely used in the thermal insulation of rail vehicle air-conditioning systems.

[0022] Since lightweight melamine foam plastic has a high open-pore rate, its waterproof performance is poor; and in the fields of construction, petrochemical industry, cold storage and so on, there are also high requirements for the waterproof performance of foam plastic, so it is necessary to study a lightweight melamine waterproof foam plastic and its preparation method. Summary of the invention

[0023] The object of the present invention is to provide a lightweight melamine waterproof foam plastic and a preparation method thereof, so as to solve the problems in the prior art.

[0024] The technical solution adopted by the present invention to solve the technical problem is:

[0025] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 2-5% of a surfactant, 0.5-1.2% of a composite catalyst, 3-8% of a foaming agent and the remainder of modified melamine formaldehyde resin.

[0026] Preferably, the modified melamine formaldehyde resin is formaldehyde and hexamethylenetetramine modified melamine resin.

[0027] Preferably, the surfactant is any one of Tween-40, Tween-80 and OP-10, or a combination of more thereof.

[0028] Preferably, the composite catalyst is a mixture of potassium acetate and ammonium chloride.

[0029] Further preferably, the mass ratio of potassium acetate to ammonium chloride is 100:(30-55).

[0030] Preferably, the foaming agent is any one of dichloromethane, isopentane, n-pentane, cyclopentane and n-butane.

[0031] Preferably, the method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0032] A. Adding a 35-40% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.0-9.5 with a 25-35% sodium hydroxide solution, gradually heating the solution to 80-90° C., adding melamine when the solution is heated to 62-67° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and a dendritic polymer when the water mixing number reaches 100-150%, stirring well, and cooling to room temperature to obtain a modified melamine formaldehyde resin;

[0033] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0034] C Preheat the modified melamine formaldehyde resin to 30-35°C, add surfactant and foaming agent, stir for 90-120s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 90-95°C for pre-foaming for 60-75min, then heat to 105-110°C and bake at high temperature for 90-105min.

[0035] Compared with the prior art, the advantages of the present invention are: the present invention adopts modified melamine formaldehyde resin to replace the traditional melamine resin, and adopts a mixture of potassium acetate and ammonium chloride as a composite catalyst, so that the prepared melamine molecular chain has more complex cross-linking and a stronger network structure, so it has excellent compression strength; at the same time, the complex cross-linking structure significantly improves the waterproof effect of the foam plastic. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described in detail below through specific embodiments. It should be understood that the implementation of the present invention is not limited to the following embodiments, and any form of modification and / or change made to the present invention will fall within the protection scope of the present invention.

[0037] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0038] The reagents used in the following examples, unless otherwise specified, can be purchased from conventional biochemical reagent stores. The quantitative data in the following examples were all set up for three repeated experiments, and the results were averaged.

[0039] Example 1

[0040] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 3.5% of a surfactant, 0.8% of a composite catalyst, 5.5% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0041] The surfactant is Tween-40.

[0042] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:38.

[0043] The foaming agent is n-pentane.

[0044] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0045] A. Adding a 38% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.2 with a 32% sodium hydroxide solution, gradually heating the solution to 85° C., adding melamine when the solution is heated to 65° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 135%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0046] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0047] C Preheat the modified melamine formaldehyde resin to 32°C, add surfactant and foaming agent, stir for 95s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 92°C for pre-foaming for 65min, then raise the temperature to 108°C and bake at high temperature for 98min.

[0048] Example 2

[0049] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 2% of surfactant, 1.2% of composite catalyst, 3% of foaming agent and the remainder of modified melamine formaldehyde resin.

[0050] The surfactant is Tween-80.

[0051] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:30.

[0052] The foaming agent is dichloromethane.

[0053] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0054] A. Adding a 40% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.5 with a 25% sodium hydroxide solution, gradually heating the solution to 80° C., adding melamine when the solution is heated to 67° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 100%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0055] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0056] C Preheat the modified melamine formaldehyde resin to 35°C, add surfactant and foaming agent, stir for 90s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 95°C for pre-foaming for 60min, then heat to 110°C and bake at high temperature for 90min.

[0057] Example 3

[0058] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 5% of a surfactant, 0.5% of a composite catalyst, 8% of a foaming agent and the remainder of modified melamine formaldehyde resin.

[0059] The surfactant is OP-10.

[0060] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:55.

[0061] The foaming agent is n-butane.

[0062] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0063] A. Adding a 35% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.0 with a 35% sodium hydroxide solution, gradually heating the solution to 90° C., adding melamine when the solution is heated to 62° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and a dendritic polymer when the water mixing number reaches 150%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0064] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0065] C Preheat the modified melamine formaldehyde resin to 30°C, add surfactant and foaming agent, stir for 120s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 90°C for pre-foaming for 75min, then raise the temperature to 105°C and bake at high temperature for 105min.

[0066] Example 4

[0067] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 3.8% of a surfactant, 1.1% of a composite catalyst, 6.2% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0068] The surfactant is a combination of Tween-40 and OP-10 in a mass ratio of 3:1.

[0069] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:37.

[0070] The foaming agent is any one of dichloromethane, isopentane, n-pentane, cyclopentane and n-butane.

[0071] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0072] A. Adding a 38% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.2 with a 25% sodium hydroxide solution, gradually heating the solution to 80° C., adding melamine when the solution is heated to 65° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 100%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0073] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0074] C Preheat the modified melamine formaldehyde resin to 32°C, add surfactant and foaming agent, stir for 90s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 92°C for pre-foaming for 60min, then raise the temperature to 107°C and bake at high temperature for 90min.

[0075] Example 5

[0076] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 2.8% of a surfactant, 0.7% of a composite catalyst, 4.2% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0077] The surfactant is a combination of Tween-80 and OP-10 in a mass ratio of 2:4.

[0078] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:43.

[0079] The foaming agent is n-pentane.

[0080] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0081] A. Adding a 40% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.5 with a 28% sodium hydroxide solution, gradually heating the solution to 82° C., adding melamine when the solution is heated to 67° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and a dendritic polymer when the water mixing number reaches 127%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0082] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0083] C Preheat the modified melamine formaldehyde resin to 35°C, add surfactant and foaming agent, stir for 97 seconds, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 95°C for pre-foaming for 67 minutes, then heat to 110°C and bake at high temperature for 94 minutes.

[0084] Some of the raw materials in Example 1 are changed to study the effects of these raw materials on the physical properties of the final foamed plastics.

[0085] Comparative Example 1

[0086] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 3.5% of a surfactant, 0.8% of a composite catalyst, 5.5% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0087] The surfactant is Tween-40.

[0088] The catalyst is potassium acetate.

[0089] The foaming agent is n-pentane.

[0090] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0091] A. Adding a 38% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.2 with a 32% sodium hydroxide solution, gradually heating the solution to 85° C., adding melamine when the solution is heated to 65° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 135%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0092] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0093] C Preheat the modified melamine formaldehyde resin to 32°C, add surfactant and foaming agent, stir for 95s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 92°C for pre-foaming for 65min, then raise the temperature to 108°C and bake at high temperature for 98min.

[0094] Comparative Example 2

[0095] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 3.5% of a surfactant, 0.8% of a composite catalyst, 5.5% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0096] The surfactant is Tween-40.

[0097] The catalyst is ammonium chloride.

[0098] The foaming agent is n-pentane.

[0099] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0100] A. Adding a 38% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.2 with a 32% sodium hydroxide solution, gradually heating the solution to 85° C., adding melamine when the solution is heated to 65° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 135%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0101] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0102] C Preheat the modified melamine formaldehyde resin to 32°C, add surfactant and foaming agent, stir for 95s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 92°C for pre-foaming for 65min, then raise the temperature to 108°C and bake at high temperature for 98min.

[0103] Comparative Example 3

[0104] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 3.5% of a surfactant, 0.8% of a composite catalyst, 5.5% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0105] The surfactant is Tween-40.

[0106] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:300.

[0107] The foaming agent is n-pentane.

[0108] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0109] A. Adding a 38% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.2 with a 32% sodium hydroxide solution, gradually heating the solution to 85° C., adding melamine when the solution is heated to 65° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 135%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0110] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0111] C Preheat the modified melamine formaldehyde resin to 32°C, add surfactant and foaming agent, stir for 95s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 92°C for pre-foaming for 65min, then raise the temperature to 108°C and bake at high temperature for 98min.

[0112] Comparative Example 4

[0113] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 3.5% of a surfactant, 0.8% of a composite catalyst, 5.5% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0114] The surfactant is Tween-40.

[0115] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:5.

[0116] The foaming agent is n-pentane.

[0117] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0118] A. Adding a 38% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.2 with a 32% sodium hydroxide solution, gradually heating the solution to 85° C., adding melamine when the solution is heated to 65° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 135%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin;

[0119] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0120] C Preheat the modified melamine formaldehyde resin to 32°C, add surfactant and foaming agent, stir for 95s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 92°C for pre-foaming for 65min, then raise the temperature to 108°C and bake at high temperature for 98min.

[0121] Comparative Example 5

[0122] A light melamine waterproof foam plastic is composed of the following components in percentage by weight: 3.5% of a surfactant, 0.8% of a composite catalyst, 5.5% of a foaming agent and the remainder of a modified melamine formaldehyde resin.

[0123] The surfactant is Tween-40.

[0124] The composite catalyst is a mixture of potassium acetate and ammonium chloride; the mass ratio of the potassium acetate to the ammonium chloride is 100:38.

[0125] The foaming agent is n-pentane.

[0126] The method for preparing the lightweight melamine waterproof foam plastic comprises the following steps:

[0127] A. Adding a 38% formaldehyde aqueous solution and water into a container, stirring them thoroughly to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.2 with a 32% sodium hydroxide solution, gradually heating it to 85° C., adding melamine when the temperature reaches 65° C., and maintaining the pH value to be not less than 8.0; after the color of the reaction system becomes clear, continuing the reaction, testing the water mixing number, adding triethanolamine and dendritic polymer when the water mixing number reaches 135%, stirring them uniformly, and cooling them to room temperature to obtain a modified melamine formaldehyde resin;

[0128] B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst;

[0129] C Preheat the modified melamine formaldehyde resin to 32°C, add surfactant and foaming agent, stir for 95s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 92°C for pre-foaming for 65min, then raise the temperature to 108°C and bake at high temperature for 98min.

[0130] Test Case

[0131] The physical properties of the melamine waterproof foam plastics prepared in Examples 1-5 and Comparative Examples 1-5 were tested, and the following test results were obtained. The specific test results are shown in Table 1.

[0132] Specific testing methods: Tensile strength and elongation at break shall be tested in accordance with the provisions of GB / T6344-2008, and mass moisture absorption rate shall be tested in accordance with the provisions of GB / T5480-2008.

[0133] Table 1: Test results of physical properties of melamine waterproof foam plastics prepared in Examples 1-5 and Comparative Examples 1-5;

[0134]

[0135]

[0136] From the above test data, it can be seen that after the melamine resin is modified by formaldehyde and hexamethylenetetramine in the present invention, its tensile strength, elongation at break and waterproof performance are significantly improved; and the potassium acetate and ammonium chloride in the composite catalyst have a synergistic effect with each other.

[0137] The above is a detailed introduction to the lightweight melamine waterproof foam plastic and its preparation method provided by the present invention. This article uses specific examples to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and core ideas of the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A lightweight melamine waterproof foam plastic, characterized in that: The invention is composed of the following components in weight percentage: 2-5% of surfactant, 0.5-1.2% of composite catalyst, 3-8% of foaming agent and the balance of modified melamine formaldehyde resin; The modified melamine formaldehyde resin is a melamine resin modified by formaldehyde and hexamethylenetetramine; The composite catalyst is a mixture of potassium acetate and ammonium chloride; The mass ratio of potassium acetate to ammonium chloride is 100:(30-55).

2. The lightweight melamine waterproof foam plastic according to claim 1, characterized in that: The surfactant is any one of Tween-40, Tween-80 and OP-10 or a combination of multiple thereof.

3. The lightweight melamine waterproof foam plastic according to claim 1, characterized in that: The foaming agent is any one of dichloromethane, isopentane, n-pentane, cyclopentane and n-butane.

4. The lightweight melamine waterproof foam plastic according to any one of claims 1 to 3, characterized in that: The preparation method thereof comprises the following steps: A. Adding a 35-40% formaldehyde aqueous solution, hexamethylenetetramine and water into a container, stirring well to obtain a first mixed solution; adjusting the pH value of the first mixed solution to 9.0-9.5 with a 25-35% sodium hydroxide solution, gradually heating the solution to 80-90° C., adding melamine when the solution is heated to 62-67° C., and maintaining the pH value to be not less than 8.0; continuing the reaction after the color of the reaction system becomes clear, testing the water mixing number, adding triethanolamine and a dendritic polymer when the water mixing number reaches 100-150%, stirring well, and cooling the solution to room temperature to obtain a modified melamine formaldehyde resin; B. Mix potassium acetate and ammonium chloride in proportion and stir evenly to obtain a composite catalyst; C Preheat the modified melamine formaldehyde resin to 30-35°C, add surfactant and foaming agent, stir for 90-120s, then add composite catalyst, stir evenly, quickly pour into the mold, send the mold into a far-infrared heating furnace, adjust the temperature to 90-95°C for pre-foaming for 60-75min, then heat to 105-110°C and bake at high temperature for 90-105min.