Anti-fouling wig and preparation method thereof

The problem of contaminants adhering to wigs has been solved by using anti-fouling wigs made of polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent modified titanium dioxide and fluorine-containing POSS. , improves the mechanical properties and anti-fouling properties, and extends the service life of the wig.

CN115896975BActive Publication Date: 2024-10-11SHENZHEN ZHUANZHENG INTELLECTUAL PROPERTY SERVICE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211315756.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-26
Publication Date
2024-10-11
Estimated Expiration
2042-10-26

AI Technical Summary

Technical Problem

When wearing wigs, grease and sweat tend to adhere to them, leading to the growth of bacteria and bad odor. They are also troublesome to clean, accelerate aging, and affect the mechanical properties and appearance.

Method used

Anti-fouling wigs are prepared using raw materials such as polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent modified titanium dioxide and fluorine-containing POSS, which reduce pollution by improving mechanical properties and surface hydrophobicity. material adsorption.

Benefits of technology

Improves the mechanical properties and anti-fouling properties of the wig, keeping it clean during wearing and extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003908693090000081
    Figure BDA0003908693090000081
  • Figure HDA0003908693100000011
    Figure HDA0003908693100000011
Patent Text Reader

Abstract

The invention relates to the field of wig products, in particular to an anti-fouling wig and a preparation method thereof. The wig is prepared from the following raw materials, measured by weight: 80-100 parts of polyvinyl chloride, 20-30 parts of styrene-ethylene-butylene-styrene block copolymer, 5-10 parts of silane coupling agent-modified titanium dioxide-g-maleic anhydride, 10-20 parts of fluorine-containing POSS, and 5-10 parts of an auxiliary agent. The anti-fouling wig prepared by the invention has excellent mechanical properties and anti-fouling properties, can effectively reduce the adsorption of pollutants on the surface of the wig during normal wearing, and can keep the wig clean for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of wig products, in particular to a stain-resistant wig and a preparation method thereof. Background Art

[0002] Wigs, as a type of hair made through artificial technology, can play a relatively good decorative role for people with sparse hair and hair loss. For people who have requirements for appearance, they can change different hairstyles at any time to avoid the damage to real hair caused by frequent perming and dyeing, and can save a lot of time and money. For the film and television industry, wigs are indispensable props. However, when wigs are worn, they are in contact with the scalp. Over time, the oil and sweat secreted from the skin will adhere to the wig, which is easy to breed bacteria and emit unpleasant odors. Therefore, wigs need to be cleaned frequently. However, wig cleaning is troublesome and laborious on the one hand, and on the other hand, it will accelerate the aging of the wig, causing the mechanical properties of the wig to decline, and also affecting the appearance of the wig. Summary of the invention

[0003] Purpose of the invention: In view of the above technical problems, the present invention provides an anti-fouling wig and a preparation method thereof.

[0004] The technical solutions adopted are as follows:

[0005] A stain-resistant wig is prepared from the following raw materials in parts by weight:

[0006] 80-100 parts of polyvinyl chloride, 20-30 parts of styrene-ethylene-butylene-styrene block copolymer, 5-10 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 10-20 parts of fluorine-containing POSS, and 5-10 parts of auxiliary agent.

[0007] Further, it is prepared from the following raw materials in parts by weight:

[0008] 85 parts of polyvinyl chloride, 20 parts of styrene-ethylene-butylene-styrene block copolymer, 10 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 15 parts of fluorine-containing POSS, and 6 parts of auxiliary agent.

[0009] Furthermore, the preparation method of the silane coupling agent modified titanium dioxide grafted with maleic anhydride is as follows:

[0010] Titanium dioxide, silane coupling agent and ethanol are mixed, stirred and heated to reflux reaction for 3-5 hours, and then centrifuged. The precipitate is washed with ethanol and dried to obtain silane coupling agent modified titanium dioxide. Then, under nitrogen protection, the silane coupling agent modified titanium dioxide is mixed with dibenzoyl peroxide, maleic anhydride, xylene and acetone, stirred evenly, heated to 100-120°C and reacted for 3-5 hours. The reaction product is washed with acetone and dried to constant weight.

[0011] Furthermore, the structural formula of the silane coupling agent contains an unsaturated carbon-carbon double bond.

[0012] Furthermore, the silane coupling agent is any one or more of KH-570, A-171, KH-A172, and A-151.

[0013] Further, the preparation method of the fluorine-containing POSS is as follows:

[0014] Vinyl POSS, 1H,1H,2H,2H-perfluorodecanethiol, 2,2-dimethoxyphenylacetophenone and dichloromethane were mixed and stirred evenly, reacted under ultraviolet light for 20-50 minutes, centrifuged, and the obtained precipitate was washed with dichloromethane for multiple times and then vacuum dried to constant weight.

[0015] Furthermore, the auxiliary agent includes any one or more combinations of heat stabilizers, lubricants, plasticizers, matting agents, softeners, antibacterial agents, antioxidants, light stabilizers, flame retardants and colorants.

[0016] Furthermore, the plasticizer is any one or more of citrate esters, trimellitate esters, and cyclohexanedicarboxylate ester plasticizers.

[0017] Furthermore, the flame retardant is di(2,3-dichloropropyl)octyl phosphate and pentaerythritol phosphate, and the mass ratio of the di(2,3-dichloropropyl)octyl phosphate to pentaerythritol phosphate is 1-5:1-5.

[0018] The present invention also provides a method for preparing a stain-resistant wig:

[0019] S1: After drying polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent-modified titanium dioxide-g-maleic anhydride, fluorine-containing POSS, and auxiliary agent, respectively, adding them into a mixer and mixing them evenly to obtain a mixture;

[0020] S2: adding the mixed material into a single screw extruder, heating and melting the extruder to obtain nascent fibers, and then cooling the nascent fibers, applying oil, and drawing at a drawing temperature of 90-95° C., and obtaining a tow after the drawing is completed;

[0021] S3: The tow is subjected to tension heat setting and relaxation heat setting in sequence, and then is collected and packaged.

[0022] Beneficial effects of the present invention:

[0023] The invention provides an anti-fouling type wig. Polyvinyl chloride is a general resin with good performance, low price and wide application field, and is a common raw material for making wigs. However, it has deficiencies in processing performance, thermal stability and the like. Styrene-ethylene-butylene-styrene block copolymer is a thermoplastic elastomer with excellent performance, and has the performance of both plastic and rubber. The molecular chain is highly saturated and the heat aging resistance is good. After being added, the mechanical properties and processing properties of polyvinyl chloride can be improved. Titanium dioxide can be used as a filler to improve the mechanical strength of polyvinyl chloride. The silane coupling agent is modified and grafted with maleic anhydride, which can improve the compatibility of titanium dioxide and resin and prevent agglomeration. The titanium dioxide on the surface of the wig is also conducive to the formation of a super hydrophobic surface and improves the anti-fouling self-cleaning ability. Fluorine-containing POSS can improve the physical and mechanical properties of the wig material, and the introduction of fluorine atoms can reduce the surface energy of the wig and improve the surface hydrophobicity. The anti-fouling type wig prepared by the invention has excellent mechanical properties and anti-fouling properties. In the normal wearing process, the adsorption of pollutants on the surface of the wig can be effectively reduced, so that the wig can be kept clean for a long time. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope image of the anti-fouling wig in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0026] Embodiment 1:

[0027] A stain-resistant wig is prepared from the following raw materials in parts by weight:

[0028] 85 parts of polyvinyl chloride, 20 parts of styrene-ethylene-butylene-styrene block copolymer, 10 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 15 parts of fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, 1 part of di(2,3-dichloropropyl)octyl phosphate, and 2 parts of pentaerythritol phosphate.

[0029] Wherein, the preparation method of silane coupling agent modified titanium dioxide grafted with maleic anhydride is as follows:

[0030] 20g of nano titanium dioxide, 20g of silane coupling agent KH-570, and 1L of 95% ethanol were mixed, stirred and heated to reflux for reaction for 5h, and then centrifuged. The precipitate was washed with ethanol and vacuum dried at 60°C for 15h to obtain silane coupling agent modified titanium dioxide. Then, under nitrogen protection, the silane coupling agent modified titanium dioxide was mixed with 0.8g of dibenzoyl peroxide, 20g of maleic anhydride, 50mL of xylene and 200mL of acetone. After stirring evenly, the temperature was raised to 110°C for reaction for 4h, and the reaction product was washed with acetone and vacuum dried at 60°C to constant weight.

[0031] The preparation method of fluorine-containing POSS is as follows:

[0032] 63.3 g of octavinyl POSS, 48 g of 1H,1H,2H,2H-perfluorodecanethiol, 0.96 g of 2,2-dimethoxyphenylacetophenone and 500 mL of dichloromethane were mixed and stirred evenly, reacted under ultraviolet light for 40 min, and centrifuged. The obtained precipitate was washed with dichloromethane for several times and then dried in vacuum at 60° C. to constant weight.

[0033] The preparation method of the above-mentioned anti-fouling type wig:

[0034] Polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent modified titanium dioxide-g-maleic anhydride, fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, di(2,3-dichloropropyl)octyl phosphate and pentaerythritol phosphate are dried separately and added into a mixer and mixed evenly to obtain a mixture, the mixture is added into a single screw extruder, heated and melt-extruded to obtain spun fibers, the spun fibers are cooled and oiled, stretched at 95°C to obtain a tow, and the tow is successively subjected to tensile heat setting and relaxation heat setting and then collected and packaged, the tensile heat setting temperature is 120°C, the time is 10 min, and the relaxation heat setting temperature is 80°C, the time is 20 min.

[0035] Embodiment 2:

[0036] A stain-resistant wig is prepared from the following raw materials in parts by weight:

[0037] 100 parts of polyvinyl chloride, 30 parts of styrene-ethylene-butylene-styrene block copolymer, 10 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 20 parts of fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, 1 part of di(2,3-dichloropropyl)octyl phosphate, and 2 parts of pentaerythritol phosphate.

[0038] Wherein, the preparation method of silane coupling agent modified titanium dioxide grafted with maleic anhydride and fluorine-containing POSS is the same as that in Example 1.

[0039] The preparation method of the above-mentioned anti-fouling type wig:

[0040] Polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent modified titanium dioxide-g-maleic anhydride, fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, di(2,3-dichloropropyl)octyl phosphate and pentaerythritol phosphate are dried separately and added into a mixer and mixed evenly to obtain a mixture, the mixture is added into a single screw extruder, heated and melt-extruded to obtain spun fibers, the spun fibers are cooled and oiled, stretched at 95°C to obtain a tow, and the tow is successively subjected to tensile heat setting and relaxation heat setting and then collected and packaged, the tensile heat setting temperature is 120°C, the time is 10 min, and the relaxation heat setting temperature is 80°C, the time is 20 min.

[0041] Embodiment 3:

[0042] A stain-resistant wig is prepared from the following raw materials in parts by weight:

[0043] 80 parts of polyvinyl chloride, 20 parts of styrene-ethylene-butylene-styrene block copolymer, 5 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 10 parts of fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, 1 part of di(2,3-dichloropropyl)octyl phosphate, and 2 parts of pentaerythritol phosphate.

[0044] Wherein, the preparation method of silane coupling agent modified titanium dioxide grafted with maleic anhydride and fluorine-containing POSS is the same as that in Example 1.

[0045] The preparation method of the above-mentioned anti-fouling type wig:

[0046] Polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent modified titanium dioxide-g-maleic anhydride, fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, di(2,3-dichloropropyl)octyl phosphate and pentaerythritol phosphate are dried separately and added into a mixer and mixed evenly to obtain a mixture, the mixture is added into a single screw extruder, heated and melt-extruded to obtain spun fibers, the spun fibers are cooled and oiled, stretched at 90°C to obtain a tow, and the tow is successively subjected to tensile heat setting and relaxation heat setting and then collected and packaged, the tensile heat setting temperature is 120°C, the time is 10 min, and the relaxation heat setting temperature is 80°C, the time is 20 min.

[0047] Embodiment 4:

[0048] A stain-resistant wig is prepared from the following raw materials in parts by weight:

[0049] 100 parts of polyvinyl chloride, 20 parts of styrene-ethylene-butylene-styrene block copolymer, 10 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 10 parts of fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, 1 part of di(2,3-dichloropropyl)octyl phosphate, and 2 parts of pentaerythritol phosphate.

[0050] Wherein, the preparation method of silane coupling agent modified titanium dioxide grafted with maleic anhydride and fluorine-containing POSS is the same as that in Example 1.

[0051] The preparation method of the above-mentioned anti-fouling type wig:

[0052] Polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent modified titanium dioxide-g-maleic anhydride, fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, di(2,3-dichloropropyl)octyl phosphate and pentaerythritol phosphate are dried separately and added into a mixer and mixed evenly to obtain a mixture, the mixture is added into a single screw extruder, heated and melt-extruded to obtain spun fibers, the spun fibers are cooled and oiled, stretched at 95°C to obtain a tow, and the tow is successively subjected to tensile heat setting and relaxation heat setting and then collected and packaged, the tensile heat setting temperature is 120°C, the time is 10 min, and the relaxation heat setting temperature is 80°C, the time is 20 min.

[0053] Embodiment 5:

[0054] A stain-resistant wig is prepared from the following raw materials in parts by weight:

[0055] 80 parts of polyvinyl chloride, 30 parts of styrene-ethylene-butylene-styrene block copolymer, 5 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 20 parts of fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, 1 part of di(2,3-dichloropropyl)octyl phosphate, and 2 parts of pentaerythritol phosphate.

[0056] Wherein, the preparation method of silane coupling agent modified titanium dioxide grafted with maleic anhydride and fluorine-containing POSS is the same as that in Example 1.

[0057] The preparation method of the above-mentioned anti-fouling type wig:

[0058] Polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent modified titanium dioxide-g-maleic anhydride, fluorine-containing POSS, 3 parts of cyclohexane-1,2-dicarboxylic acid diisononyl ester, di(2,3-dichloropropyl)octyl phosphate and pentaerythritol phosphate are dried separately and added into a mixer and mixed evenly to obtain a mixture, the mixture is added into a single screw extruder, heated and melt-extruded to obtain spun fibers, the spun fibers are cooled and oiled, stretched at 90°C to obtain a tow, and the tow is successively subjected to tensile heat setting and relaxation heat setting and then collected and packaged, the tensile heat setting temperature is 120°C, the time is 10 min, and the relaxation heat setting temperature is 80°C, the time is 20 min.

[0059] Comparative Example 1:

[0060] The method is substantially the same as Example 1, except that the styrene-ethylene-butylene-styrene block copolymer is not added.

[0061] Comparative Example 2:

[0062] The method is basically the same as Example 1, except that no silane coupling agent is added to modify the titanium dioxide-g-maleic anhydride.

[0063] Comparative Example 3:

[0064] The method is basically the same as Example 1, except that nano titanium dioxide is used instead of the silane coupling agent to modify titanium dioxide-g-maleic anhydride.

[0065] Comparative Example 4:

[0066] The method is substantially the same as Example 1, except that no fluorine-containing POSS is added.

[0067] Comparative Example 5:

[0068] The method is substantially the same as Example 1, except that octavinyl POSS is used instead of fluorine-containing POSS.

[0069] Comparative Example 6:

[0070] The process is substantially the same as Example 1, except that di(2,3-dichloropropyl)octyl phosphate is not added.

[0071] Comparative Example 7:

[0072] The process is substantially the same as Example 1, except that pentaerythritol phosphate is not added.

[0073] Performance Test:

[0074] ① The anti-fouling wigs prepared in Examples 1-5 and Comparative Examples 1-7 of the present invention are used as samples;

[0075] The mechanical properties of the samples were tested on an INSTRON5566 universal material testing machine with a tensile speed of 100 mm / min, a preload of 0.001 cN / dtex, and a clamping distance of 100 mm.

[0076] Limiting Oxygen Index Test (LOI): The oxygen index test is measured according to the national standard GB / T5454-1997.

[0077] Vertical burning test (UL 94): The vertical burning test is measured according to the national standard GB / T5455-2004, and the test levels are divided into NR, V-2, V-1, and V-0.

[0078] The test results are shown in Table 1 below:

[0079] Table 1:

[0080]

[0081] It can be seen from Table 1 above that the anti-fouling wig prepared by the present invention has excellent mechanical properties and flame retardant properties.

[0082] ② The anti-fouling wigs prepared in Examples 1-5 and Comparative Examples 1-5 of the present invention were used as samples;

[0083] The sample is placed in a room with a PM2.5 level of 200 at room temperature. The room is 40 cubic meters and the test time is 60 days. The percentage of dust area on the sample is observed after 20 days, 40 days and 60 days.

[0084] The test results are shown in Table 2 below:

[0085] Table 2:

[0086] 20d 40d 60d Example 1 0.6 3.3 10.5 Example 2 0.8 3.8 10.9 Example 3 1.1 4.2 11.2 Example 4 0.5 3.5 10.6 Example 5 1.4 4.6 11.3 Comparative Example 1 0.7 3.5 11.1 Comparative Example 2 10.3 28.2 50.6 Comparative Example 3 4.4 8.2 20.8 Comparative Example 4 8.5 15.4 32.7 Comparative Example 5 8.8 26.3 34.5

[0087] It can be seen from Table 2 above that the anti-fouling wig prepared by the present invention has excellent anti-fouling performance. During normal wearing, it can effectively reduce the adsorption of pollutants on the surface of the wig, so that the wig can be kept clean for a long time.

[0088] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A stain-resistant wig, It is characterized in that It is prepared from the following raw materials in parts by weight: 80-100 parts of polyvinyl chloride, 20-30 parts of styrene-ethylene-butylene-styrene block copolymer, 5-10 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 10-20 parts of fluorine-containing POSS, and 5-10 parts of auxiliary agent; The preparation method of the silane coupling agent modified titanium dioxide grafted with maleic anhydride is as follows: Mix titanium dioxide, silane coupling agent and ethanol, stir and heat to reflux reaction for 3-5 hours, then centrifuge, wash the precipitate with ethanol and dry to obtain silane coupling agent modified titanium dioxide, then under nitrogen protection, mix the silane coupling agent modified titanium dioxide with dibenzoyl peroxide, maleic anhydride, xylene and acetone, stir evenly, heat to 100-120°C and react for 3-5 hours, wash the reaction product with acetone, and dry to constant weight; The preparation method of the fluorine-containing POSS is as follows: Vinyl POSS, 1H,1H,2H,2H-perfluorodecanethiol, 2,2-dimethoxyphenylacetophenone and dichloromethane were mixed and stirred evenly, reacted under ultraviolet light for 20-50 minutes, centrifuged, and the obtained precipitate was washed with dichloromethane for multiple times and then vacuum dried to constant weight.

2. The stain-resistant wig according to claim 1, It is characterized in that It is prepared from the following raw materials in parts by weight: 85 parts of polyvinyl chloride, 20 parts of styrene-ethylene-butylene-styrene block copolymer, 10 parts of silane coupling agent modified titanium dioxide-g-maleic anhydride, 15 parts of fluorine-containing POSS, and 6 parts of auxiliary agent.

3. The stain-resistant wig according to claim 1, It is characterized in that The structural formula of the silane coupling agent contains an unsaturated carbon-carbon double bond.

4. The stain-resistant wig according to claim 1, It is characterized in that The silane coupling agent is any one or more of KH-570, A-171, KH-A172, and A-151.

5. The stain-resistant wig according to claim 1, It is characterized in that The auxiliary agent includes any one or more combinations of heat stabilizers, lubricants, plasticizers, matting agents, softeners, antibacterial agents, antioxidants, light stabilizers, flame retardants and colorants.

6. The stain-resistant wig according to claim 5, It is characterized in that The plasticizer is diisononyl cyclohexane-1,2-dicarboxylate.

7. The stain-resistant wig according to claim 5, It is characterized in that The flame retardant is di(2,3-dichloropropyl)octyl phosphate and pentaerythritol phosphate, and the mass ratio of the di(2,3-dichloropropyl)octyl phosphate to the pentaerythritol phosphate is 1-5:1-5.

8. A method for preparing a stain-resistant wig as claimed in any one of claims 1 to 7, It is characterized in that The following steps are involved: S1: After drying polyvinyl chloride, styrene-ethylene-butylene-styrene block copolymer, silane coupling agent-modified titanium dioxide-g-maleic anhydride, fluorine-containing POSS, and auxiliary agent, respectively, adding them into a mixer and mixing them evenly to obtain a mixture; S2: adding the mixed material into a single screw extruder, heating and melting the extruder to obtain nascent fibers, and then cooling the nascent fibers, applying oil, and drawing at a drawing temperature of 90-95° C., and obtaining a tow after the drawing is completed; S3: The tow is subjected to tension heat setting and relaxation heat setting in sequence, and then is collected and packaged.

Citation Information

Cited By

  • Preparation method of medicine-carrying hair fiber

    CN122669505A