A method for measuring vertical residual stress at the head-waist connection of rail section
By fixing the strain gauge on the rail cross section and cutting to release the stress, measuring the vertical residual stress at the head and waist connection of the rail cross section, the problem that the prior art cannot directly measure this stress is solved, and an accurate prediction of the risk of rail cracking is achieved. Improves the safety of the rails.
Patent Information
- Application Number
- CN202211658725.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-22
AI Technical Summary
The prior art cannot directly measure the vertical residual stress at the joint of the head and waist of the rail cross-section, which makes it difficult to predict the possibility of vertical cracking of the rail, and the existing methods cannot effectively detect the residual stress of the rail head and waist.
Fix the strain gauge on the rail cross section and cut horizontally at 5mm below the strain gauge to release stress, measure the vertical residual stress at the head and waist connection of the rail cross section, and predict the relationship between the residual stress at this point and the material yield strength by comparing the relationship between the residual stress at this point and the material yield strength Risk of cracking.
Accurate point measurement of stress at the head and waist connection of rail cross-section is realized, and it can be predicted that when the residual stress reaches more than 75% of the material's yield strength, the rail is very prone to cracking in the vertical direction, improving the safety of the rail.
Smart Images

Figure CN115901041B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of physical detection, and in particular relates to a method for measuring vertical residual stress at a head-waist connection of a rail section. Background Art
[0002] At present, the standards cited in my country regarding residual stress of rails are mainly the Iron Standard 2344-2012 "Technical Conditions for Ordering 43kg / m~75kg / m Rails" and the American Standard AREMA-2011 "Engineer's Manual of the American Railway Engineering and Maintenance Association". Among them, the Iron Standard 2344-2012 only stipulates the test method of residual stress at the bottom of the rail and the maximum allowable value of residual stress, and does not make any requirements for the residual stress of the rail head and rail waist. Although the American Standard AREMA-2011 stipulates the residual stress along the rail waist along the rail height direction, this method indirectly measures the magnitude of the residual stress along the rail height direction by measuring the lateral displacement Δy at the opening of the rail section, and cannot directly measure the specific value of the residual stress along the rail height direction.
[0003] Although patent document CN113418642A also discloses a method for measuring residual stress of the waist of a rail, the document discloses a method for detecting vertical residual stress of the waist of a rail, which is not suitable for measuring vertical residual stress at the head-waist connection of a rail section.
[0004] The rolling, cooling, straightening and other processes that the rails undergo during production will produce unevenly distributed residual stress inside them. If the residual stress is too large, it may cause early fatigue and brittle fracture of the rails, posing a greater safety hazard to the service of the rails. In some extreme cases, some quenched rails may crack along the rail height on the cooling bed, such as Figure 1 As shown. This defect occurs because after straightening, large residual stress is generated on both the rail head and rail bottom surfaces, and both are manifested as tensile stress. This tensile stress will generate a moment in the opposite direction in the rail head section. It is precisely because of the existence of this moment that different degrees of tensile stress are also generated in the rail section along the rail height direction. When the residual stress in the rail head and rail bottom of the rail is large, a large moment will be formed in the rail section in the opposite direction; at the same time, the residual stress in the rail section along the rail height direction increases. The cross-section of the rail head and rail waist is significantly changed at the connection point, which easily causes stress concentration at the connection point, thereby causing the rail to crack at this point. Therefore, it is necessary to detect the vertical residual stress at the connection point between the head and waist of the rail section to infer the possibility of vertical cracking of the rail. Summary of the invention
[0005] In order to overcome the shortcomings of the existing residual stress testing methods and to be able to more specifically test the stress concentration point at the connection between the lower jaw of the rail head and the rail waist, the present invention fixes a strain gauge on the rail cross section, the strain gauge is fixed at the position where the stress of the lower jaw of the rail head is concentrated, and then cuts horizontally along the longitudinal direction from 5 mm below the strain gauge to achieve the effect of releasing stress, thereby measuring the magnitude of the vertical residual stress at the stress concentration point at the connection between the head and waist of the rail cross section, and by comparing the magnitude relationship between the residual stress at this point and the yield strength of the material, it is possible to predict whether the rail has a risk of cracking. When the residual stress is close to the yield strength of the material, the risk of vertical cracking of the rail increases.
[0006] The technical solution adopted by the present invention to solve the technical problem is: draw a line in the horizontal direction at the head-waist connection of the rail section to determine the vertical position of the strain gauge, and then draw a line in the vertical symmetry axis direction on the rail section, intersecting the horizontal line at a point, that is, fixing the position of the strain gauge. After the glue for sticking the strain gauge is completely solidified, connect the experimental equipment, measure the initial value, and then cut in the horizontal direction 5mm below the strain gauge, so that the residual stress along the rail height direction at the head-waist connection of the rail is completely released, thereby measuring the residual stress value of the point.
[0007] Specifically, the method for measuring the vertical residual stress at the head-waist connection of a rail section provided by the present invention comprises the following steps:
[0008] S1: Place the rail sample along the vertical direction of the rail with the cross section facing upwards;
[0009] S2: Draw a straight line in the horizontal direction 10mm below the end of the arc where the lower jaw of the rail head and the rail waist are connected on the cross section, marked as line 1, and draw a straight line along the symmetry axis in the vertical direction, marked as line 2. The intersection of lines 1 and 2 is marked as point "O", which is the position of the fixed strain gauge. Draw a straight line in the horizontal direction 5mm below point "O", marked as line 3, which is the starting point of the cutting line;
[0010] S3: Fix the strain gauge at point “O” in the vertical direction and seal the strain gauge;
[0011] S4: Connect the fixed strain gauge to the static resistance strain gauge, and click the balance button of the static resistance strain gauge to return all initial strain values to 0;
[0012] S5: disconnecting the strain gauge from the static resistance strain gauge, and cutting the rail sample in a horizontal direction starting from the straight line 3, with a cutting length of 600 mm, to release stress;
[0013] S6: After cutting, the rail sample is left to stand for 4 hours, the strain gauge is reconnected to the static resistance strain gauge, and the final value, i.e., the residual stress value at point "O", is measured after the indication stabilizes.
[0014] In step S1, the length of the rail sample is 1000 mm.
[0015] In step S3, a strain gauge with a size of 3 mm × 3 mm and a model number of BX-120-3AA is fixed at the "O" point using 406 glue. After the 406 glue solidifies, 704 silicone is applied to the surface of the strain gauge to seal and protect the strain gauge.
[0016] In step S4, the model of the static resistance strain gauge is AFT-CM-10.
[0017] In step S5, the rail sample is cut using a vertical band saw of model G5330-50.
[0018] The beneficial effect of the present invention is that it can accurately measure the residual stress at the location where the stress is concentrated at the head-waist connection of the rail, and compare the experimental results with the yield strength of the material. The results show that when the residual stress at this point reaches more than 75% of the yield strength of the material, the rail is very likely to crack vertically. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a photo of the cracks at the rail head and waist joint.
[0020] Figure 2 Schematic diagram of the cross-sectional structure of the rail specimen.
[0021] Figure 3 Schematic diagram of the three-dimensional structure of the rail sample. DETAILED DESCRIPTION
[0022] The invention aims to provide a method for accurately measuring the vertical residual stress at the head-waist connection of a rail section, so as to infer the possibility of vertical cracking of the rail.
[0023] The present invention is described in detail below through specific examples. The examples are intended to help understand the present invention but are not intended to limit the present invention.
[0024] Example 1: A method for measuring vertical residual stress at the head-waist connection of a rail section
[0025] This embodiment provides a method for measuring the vertical residual stress at the head-waist connection of a rail section, which specifically includes the following steps:
[0026] (1) Select a 1000 mm long rail sample and place it vertically with the cross section facing upward. Figure 2 As shown;
[0027] (2) Figure 2As shown, a straight line is drawn horizontally 10 mm below the end of the arc where the lower jaw of the rail head and the rail waist are connected on the cross section, marked as straight line 1, and a straight line is drawn along the symmetry axis in the vertical direction, marked as straight line 2. The intersection of straight lines 1 and 2 is marked as point "O", which is the position of the fixed strain gauge. 5 mm below point "O" (the reason for choosing to cut 5 mm below point "O" is that it has been verified by experiments that this position can ensure the maximum value of the moment of tensile stress on the tread of the rail head and the operability during sawing) A straight line is drawn horizontally and marked as straight line 3, which is the starting point of the cutting line;
[0028] (3) Use 406 glue to fix the strain gauge with a specification of 3 mm × 3 mm and model number BX-120-3AA at the "O" point in the vertical direction. After the 406 glue solidifies, apply 704 silicone rubber on the surface of the strain gauge to seal and protect the strain gauge to prevent the coolant from entering during the cutting process and affecting the experimental results.
[0029] (4) After the 704 sealing silicone gel solidifies, connect the strain gauge to a static resistance strain gauge of model AFT-CM-10 and measure the initial value of the strain gauge;
[0030] (5) After disconnecting the strain gauge from the static resistance strain gauge, Figure 3 As shown, the rail sample is placed horizontally on a vertical band saw of model G5330-50, and a cut of 600 mm is made in the horizontal direction starting from straight line 3 to release the stress.
[0031] (6) After cutting, let it stand for 4 hours, reconnect the strain gauge to the static resistance strain gauge, and measure the final value after the indication stabilizes, that is, the residual stress value at point "O".
[0032] The method provided in this embodiment can accurately measure the vertical residual stress at the head-waist connection of the rail section, and compare the vertical residual stress with the yield strength of the rail sample. The results show that when the residual stress measured by the method provided in this embodiment reaches more than 75% of the yield strength of the rail sample, the possibility of the rail cracking in the vertical direction increases, that is, the rail is more likely to crack in the vertical direction.
[0033] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for measuring the vertical residual stress at the head-waist connection of a rail section, comprising the following steps: S1: Place the rail sample along the vertical direction of the rail with the cross section facing upwards; S2: Draw a straight line in the horizontal direction 10mm below the end of the arc where the lower jaw of the rail head and the rail waist are connected on the cross section, marked as Line 1, and draw a straight line along the symmetry axis in the vertical direction, marked as Line 2. The intersection of Lines 1 and 2 is marked as Point "O", which is the location of the fixed strain gauge. Draw a straight line in the horizontal direction 5mm below Point "O", marked as Line 3, which is the starting point of the cutting line; S3: Fix the strain gauge at point "O" in the vertical direction and seal the strain gauge; S4: Connect the fixed strain gauge to the static resistance strain gauge, and click the balance button of the static resistance strain gauge to return all initial strain values to 0; S5: disconnecting the strain gauge from the static resistance strain gauge, and cutting the rail sample in a horizontal direction starting from the straight line 3, with a cutting length of 600 mm, to release stress; S6: After cutting, the rail sample is left to stand for 4 hours, the strain gauge is reconnected to the static resistance strain gauge, and the final value, i.e. the residual stress value at point "O", is measured after the indication stabilizes.
2. The method according to claim 1, wherein in step S1, the length of the rail sample is 1000 mm.
3. According to the method of claim 1, in step S3, a strain gauge with a specification of 3 mm × 3 mm and a model number of BX-120-3AA is fixed at the "O" point with 406 glue, and after the 406 glue solidifies, 704 silicone is applied to the surface of the strain gauge to seal and protect the strain gauge.
4. The method according to any one of claims 1 to 3, wherein in step S4, the model of the static resistance strain gauge is AFT-CM-10.
5. The method according to any one of claims 1 to 4, wherein in step S5, a vertical band saw of model G5330-50 is used to cut the rail sample.
Citation Information
Patent Citations
Method for testing residual stress of steel rail
CN103234666A
Resistance strain gauge switching device for testing steel rail residual stress and testing method
CN104535231A
Steel rail residual stress testing method
CN110987261A
Test method for accurately detecting vertical residual stress of rail web of steel rail
CN113418642A
Rail corrugation evaluation and maintenance management method and system and electronic equipment
CN115455747A