Method for producing graphite sheet and polyimide film for graphite sheet
By using polyimide films containing inorganic fine particles and phosphorus-containing non-metallic additives in graphite sheet manufacturing and performing high-temperature heat treatment, the problems of low strength between traditional graphite sheets and film melting are solved, and high thermal diffusion rate and The balance of strength improves production efficiency and product quality.
Patent Information
- Application Number
- CN202180042483.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-09
- Filing Date
- 2021-07-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-07-09
Smart Images

Figure CN115916697B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a graphite sheet and a polyimide film for the graphite sheet. Background Art
[0002] Graphite sheets have excellent heat dissipation properties and can be used as heat dissipation components for semiconductor elements and other heat-generating components installed in various electronic devices such as computers or electrical equipment.
[0003] Such a graphite sheet can be obtained by firing a polyimide film. For example, the technology of Patent Document 1 manufactures a graphite sheet by firing a polyimide film containing inorganic fine particles.
[0004] (Prior art literature)
[0005] Patent Document 1: Japanese Patent Application Publication No. 2014-136721 Summary of the invention
[0006] (Problem to be solved by the invention)
[0007] Various graphite sheets are conventionally known, but there is still room for improvement in order to obtain a graphite sheet having both high thermal diffusivity and interlayer strength. In particular, a newly discovered problem is that when a graphite sheet having high thermal diffusivity is desired, the interlayer strength of the manufacturing method of Patent Document 1 is low, and the films are fused together during the graphitization process, resulting in defective products and reduced productivity.
[0008] An object of one aspect of the present invention is to provide a method for manufacturing a graphite sheet and a polyimide film for a graphite sheet, wherein the method for manufacturing a graphite sheet has a high thermal diffusivity and improved interlayer strength, and a good graphite sheet can be manufactured with high productivity by preventing the melting of the film during graphitization.
[0009] (Technical means to solve the problem)
[0010] The present inventors have made intensive studies to solve the above problems and have found that a polyimide film containing inorganic fine particles and a phosphorus-containing non-metallic additive and having an inorganic fine particle and a total phosphorus content within a predetermined range can be used as a raw material to prevent the films from fusing with each other during graphitization of a graphite sheet having a high thermal diffusivity and improved interlayer strength, thereby manufacturing a graphite sheet with high productivity, thereby completing the present invention. The present invention includes the following contents.
[0011] A method for manufacturing a graphite sheet, comprising the step of heat-treating a polyimide film to a temperature of 2800° C. or higher, wherein the polyimide film contains inorganic particles and a phosphorus-containing non-metallic additive, wherein the content of the inorganic particles is 0.01% by weight or higher and 0.08% by weight or lower, and the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive is 0.018% by weight or higher and 0.032% by weight or lower, and the thermal diffusivity of the graphite sheet is 10.0 cm 2 / s or more.
[0012] A polyimide film for a graphite sheet,
[0013] It contains inorganic particles and phosphorus-containing non-metallic additives.
[0014] The content of the inorganic fine particles is 0.01 wt % or more and 0.08 wt % or less,
[0015] The total phosphorus content of the inorganic fine particles and the phosphorus-containing non-metallic additive is 0.018 wt % or more and 0.032 wt % or less.
[0016] (Effects of the Invention)
[0017] According to one aspect of the present invention, a graphite sheet having excellent thermal diffusivity and interlayer strength can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the continuous carbonization process and the continuous carbonization device of the present invention.
[0019] Figure 2 This is an example of a method for setting a film in a graphitization step. DETAILED DESCRIPTION
[0020] An embodiment of the present invention is described below, but the present invention is not limited thereto. The present invention is not limited to the various schemes described below, and various changes can be made within the scope shown in the specification. The embodiments and embodiments obtained by appropriately combining the technical means respectively disclosed in different embodiments and embodiments are also included in the technical scope of the present invention. In addition, all academic documents and patent documents recorded in this specification are cited in this specification as references. In addition, in this specification, unless otherwise specified, "A to B" indicating a numerical range means "Above A and Below B".
[0021] <1. Technical concept of the present invention>
[0022] The graphite sheet obtained by the conventional graphite sheet production method described in Patent Document 1 has problems in terms of thermal diffusivity and interlayer strength.
[0023] The present inventors have made intensive studies to provide a method for producing a graphite sheet having excellent thermal diffusivity and interlayer strength, and have found for the first time that a graphite sheet having excellent thermal diffusivity and interlayer strength can be provided by heat-treating a polyimide film containing (i) a phosphorus-containing non-metallic additive in addition to conventionally known inorganic fine particles, and (ii) the phosphorus content (total amount) contained in the inorganic fine particles and the phosphorus-containing non-metallic additive is within a certain range. In addition, the present inventors have found for the first time that according to the above method, the carbonaceous film can be prevented from fusing during the graphitization step, thereby providing a graphite sheet with high productivity.
[0024] Conventionally, graphite sheets composed of polyimide films containing inorganic particles are significantly inferior in thermal diffusivity and interlayer strength. Under such circumstances, the present inventors have found that by adding "phosphorus-containing non-metallic additives" and controlling the "total phosphorus content of inorganic particles and the phosphorus-containing non-metallic additives" within a certain range, a method for manufacturing a graphite sheet having excellent thermal diffusivity and interlayer strength and preventing film fusion during the manufacturing process can be provided.
[0025] The present inventors presume as follows why the above-mentioned method for producing a graphite sheet can provide a graphite sheet having excellent thermal diffusivity and interlaminar strength.
[0026] In the method for manufacturing a graphite sheet, when a carbonaceous film formed by carbonizing a polyimide film is graphitized, inorganic particles derived from the polyimide film are sublimated by heating. At this time, the conventionally used inorganic particles (such as calcium) have a high affinity for carbon, and therefore sublimate while reacting with the carbon (graphite) forming the graphite sheet. As a result, the orientation of the graphite in the graphite sheet is disturbed, and the thermal diffusivity and interlayer strength of the graphite sheet are reduced.
[0027] On the other hand, the phosphorus-containing non-metallic additive does not interfere with the orientation of graphite during sublimation. Therefore, the orientation of graphite is maintained, and the decrease in the thermal diffusivity and interlayer strength of the graphite sheet is suppressed.
[0028] <2. Method for producing graphite sheet>
[0029] A method for producing a graphite sheet according to one aspect of the present invention may include a step of heat treating a polyimide film having an inorganic fine particle content of 0.01 wt % to 0.08 wt % and a total phosphorus content of 0.018 wt % to 0.032 wt % to a temperature of 2800° C. or higher. In this specification, “a method for producing a graphite sheet according to one aspect of the present invention” may be referred to as “the present production method”.
[0030] This manufacturing method is a so-called polymer pyrolysis method in which a polyimide film is heat-treated in an inert gas atmosphere and under reduced pressure. Specifically, a graphite sheet is obtained by the following steps: a carbonization step in which the polyimide film is preheated to a temperature of about 1000°C to obtain a carbonized polyimide film; a graphitization step in which the carbonized polyimide film produced by the carbonization step is heat-treated (heated) to a temperature of more than 2800°C to graphitize; and an arbitrary compression step in which the graphite is compressed. The carbonization step and the graphitization step can be performed continuously, or the carbonization step can be completed first, and then only the graphitization step can be performed separately.
[0031] (Carbonization process)
[0032] The carbonization process is a process of heat-treating the polyimide film to a temperature of about 1000°C to carbonize (carbonize) the polyimide film. The carbonization method of the polyimide film in the carbonization process is not particularly limited. For example, the carbonization can be carried out in a state where the rectangular polyimide film is stacked, or the roll-shaped polyimide film can be carbonized in a roll state, or the film can be released from the roll-shaped polyimide film and continuously carbonized. Among them, the continuous carbonization method of releasing the film from the roll-shaped polyimide film and continuously carbonizing it has excellent productivity and is therefore preferred. The carbonization process is carried out under reduced pressure or in an inert gas, and nitrogen is preferably used as the inert gas. In this specification, the carbonized polyimide film obtained by the carbonization process is sometimes referred to as a carbonaceous film.
[0033] (Graphitization process)
[0034] The graphitization process is a process of heat-treating the carbonaceous film obtained in the carbonization process to a temperature of 2800°C or more, thereby graphitizing the carbonaceous film. The graphitization process can also be said to be a process of heat-treating the carbonaceous film to obtain a graphite sheet. In the graphitization process, the temperature (maximum temperature) when the carbonaceous film obtained in the carbonization process is heat-treated is preferably 2800°C or more, 2900°C or more, or 3000°C or more. The upper limit is not particularly limited, preferably below 3300°C, and more preferably below 3200°C. In the graphitization process, the temperature (maximum temperature) when the carbonaceous film obtained in the carbonization process is heat-treated is 2800°C or more, which has the advantage of good thermal diffusivity of the obtained graphite sheet, and the temperature is below 3300°C, which has the advantage of being able to suppress the sublimation of the graphite parts in the graphitization furnace. The graphitization process is carried out under reduced pressure or in an inert gas, and argon or helium is suitable as an inert gas.
[0035] In the graphitization step, the rectangular carbonaceous films may be graphitized in a stacked state, or a roll-shaped carbonaceous film may be graphitized in a roll state, or a film may be released from a roll-shaped carbonaceous film and graphitized continuously. It is preferred to graphitize in a roll state, or to release a roll-shaped carbonaceous film and graphitize continuously, thereby obtaining a longer film.
[0036] (Compression process)
[0037] The foamed graphite sheet after graphitization can be subjected to a compression process. By performing the compression process, flexibility can be imparted to the graphite sheet. The compression process can be performed by a surface compression method, a rolling method using a metal roller, etc. The compression process can be performed at room temperature or during the graphitization process. The compression process can also be referred to as a softening process.
[0038] <3. Graphite sheet>
[0039] The thermal diffusivity of the graphite sheet obtained by the present production method is preferably 10.0 cm 2 / s or more, more preferably 10.4cm 2 / s or more, more preferably 10.8cm 2 / s or more.
[0040] In addition, the interlayer strength of the graphite sheet according to one embodiment of the present invention is preferably 35 gf / inch or more, more preferably 40 gf / inch or more, and even more preferably 45 gf / inch or more. When the interlayer strength is within this range, interlayer delamination that causes a decrease in the thermal diffusivity of the graphite sheet does not occur when the release film of the double-sided tape attached to the graphite sheet is peeled off, which is preferred.
[0041] In addition, the thickness of the graphite sheet of one embodiment of the present invention is preferably 16 to 85 μm, more preferably 16 to 80 μm, further preferably 23 to 60 μm, and further preferably 30 to 50 μm. When the thickness of the graphite sheet is within the above range, it has the advantage of being able to exert excellent heat dissipation effect when used in thin electronic devices (such as high-function smartphones, etc.).
[0042] The lower limit of the thickness of the graphite sheet of one embodiment of the present invention is preferably 16 μm or more, more preferably 20 μm or more, further preferably 23 μm or more, further preferably 30 μm or more. In addition, the upper limit of the thickness of the graphite sheet is preferably 85 μm or less, more preferably 80 μm or less, further preferably 60 μm or less, and further preferably 50 μm or less. If the thickness of the graphite sheet is 16 μm or more, it has a sufficient heat dissipation effect on the heat generated by the electronic device, and if the thickness is 85 μm or less, it has the advantage of being able to be installed in a thin electronic device with less space.
[0043] The density of the graphite sheet according to one embodiment of the present invention is preferably 1.80 g / cm 3 More preferably, 2.00 g / cm 3 More preferably, 2.05 g / cm 3 More preferably, 2.10 g / cm 3 More preferably, 2.15 g / cm 3 The upper limit of density is not particularly limited, but usually, the upper limit of density of graphite sheet is 2.26 g / cm 3 When the density of the graphite sheet is within the above range, the graphite sheet has the advantage of being able to exert an excellent heat dissipation effect.
[0044] <4. Polyimide film for graphite sheet>
[0045] The polyimide film that can be used in one embodiment of the present invention is described in detail below. The polyimide film for a graphite sheet used in the present production method is a polyimide film made of an acid dianhydride component and a diamine component as raw materials, and contains predetermined amounts of inorganic fine particles and phosphorus.
[0046] (Inorganic particles)
[0047] The inorganic particle content lower limit of the polyimide film of one embodiment of the present invention is preferably 0.01 weight %, more preferably 0.02 weight %, and further preferably 0.03 weight %. The inorganic particle content upper limit is preferably 0.10 weight %, more preferably 0.08 weight %, and further preferably 0.06 weight %, and particularly preferably 0.05 weight %. When the content of inorganic particles is within this range, the thermal diffusivity and interlaminar strength of the graphite sheet finally obtained are both excellent and the transportability is also good. In addition, when the content of inorganic particles in the polyimide film is more than 0.01 weight %, the transportability of the polyimide film is excellent. Therefore, in the manufacturing process (such as carbonization process), the polyimide film does not have the risk of rupture. In addition, when the content of inorganic particles in the polyimide film is less than 0.10 weight %, the thermal diffusivity of the graphite sheet finally obtained is excellent.
[0048] Examples of inorganic fine particles that can be used in one embodiment of the present invention include calcium carbonate (CaCO 3 ), silicon dioxide, calcium hydrogen phosphate (CaHPO 4 ), calcium phosphate (Ca 2 P 2 O 7 ) etc. Among these inorganic fine particles, phosphorus-containing inorganic fine particles such as calcium hydrogen phosphate and calcium phosphate are preferably used, which can reduce the amount of phosphorus-containing non-metallic additives described later and make it easier for the graphite sheet to have both thermal diffusivity and interlayer strength.
[0049] (Phosphorus-containing non-metallic additives)
[0050] The polyimide film of one embodiment of the present invention preferably contains a phosphorus-containing non-metallic additive in a manner such that the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive described later is within a preferred range. As phosphorus-containing non-metallic additives that can be used in one embodiment of the present invention, phosphates, phosphorus oxides, phosphites, phosphines, phosphonates, hypophosphites, pyrophosphoric acid, metaphosphoric acid, red phosphorus, etc. can be cited. Among them, organic phosphorus compounds such as phosphates, phosphorus oxides, phosphites, phosphines, phosphonates, hypophosphites are stable relative to polyamic acid and polyimide, and are therefore preferably used. In addition, from the viewpoint of stability, the organic phosphorus compound is preferably composed of pentavalent phosphorus as the main component. The polyimide film of one embodiment of the present invention contains a phosphorus-containing non-metallic additive, and the polyimide film can be used to provide a graphite sheet having excellent thermal diffusivity and interlayer strength, and, since the melting and adhesion of the carbonaceous film in the graphitization process can be prevented, the graphite sheet can be provided with higher productivity.
[0051] In addition, in the TG-DTA measurement of the phosphorus-containing non-metallic additive, the temperature at which the weight loss rate of the phosphorus-containing non-metallic additive reaches 5% is preferably 200° C. or more, more preferably 250° C. or more, and further preferably 300° C. or more. If the temperature at which the weight loss rate of the phosphorus-containing non-metallic additive reaches 5% is 200° C. or more, the contamination of the polyimide film carbonization furnace can be reduced.
[0052] It is preferable to use a phosphorus-containing non-metallic additive having excellent compatibility with the polyimide resin. Such an additive can be well dispersed in the polyimide film, thereby obtaining a graphite sheet with less uneven foaming degree in the plane.
[0053] In addition, it is preferable to use a phosphorus-containing non-metallic additive that is liquid at room temperature and pressure. Such an additive does not precipitate in the polyimide film, and a graphite sheet that rarely causes abnormal foaming during graphitization can be obtained.
[0054] (Total phosphorus content of inorganic particles and phosphorus-containing non-metallic additives)
[0055] In the polyimide film of one embodiment of the present invention, the lower limit of the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive is higher than 0.015% by weight, preferably 0.018% by weight, more preferably 0.021% by weight, and further preferably 0.025% by weight. The upper limit of the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive is preferably 0.032% by weight, more preferably 0.031% by weight, and further preferably 0.030% by weight. When the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive in the polyimide film is 0.018% by weight to 0.032% by weight, the thermal diffusivity and interlayer strength of the graphite sheet finally obtained are both excellent. In particular, when the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive in the polyimide film is higher than 0.015% by weight, the carbonaceous film formed by carbonization of the polyimide film does not have the risk of melting and bonding each other even if the carbonaceous film is graphitized in a roll state in the graphitization process, and a longer graphite sheet can be provided. In addition, when the total phosphorus content of the inorganic fine particles and the phosphorus-containing non-metallic additive in the polyimide film is 0.021 wt % to 0.031 wt %, both thermal diffusivity and interlayer strength are advantageously more excellent.
[0056] (Acid dianhydride component)
[0057] The acid dianhydride component that can be used as a raw material of the polyimide film of one embodiment of the present invention includes pyromellitic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,1-(3,4 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, oxybis(phthalic acid) dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, p-phenylene bis(trimellitic acid monoester anhydride), ethylene bis(trimellitic acid monoester anhydride), bisphenol A bis(trimellitic acid monoester anhydride), and their analogs. As the acid dianhydride component, these acid dianhydrides may be used alone, or a plurality of these acid dianhydrides may be mixed and used in any proportion. Among these acid dianhydrides, pyromellitic acid dianhydride or 3,3',4,4'-biphenyltetracarboxylic acid dianhydride is preferably used. By using the acid dianhydride component, the thermal diffusivity of the graphite sheet finally obtained is good.
[0058] (Diamine component)
[0059] The diamine component that can be used as a raw material of the polyimide film according to one embodiment of the present invention includes 4,4'-diaminodiphenyl ether, p-phenylenediamine, 4,4'-diaminodiphenylmethane, diaminobiphenyl, 3,3'-dichloro(diaminobiphenyl), 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-aniline, 1,3-diaminobenzene, 1,2-diaminobenzene, and the like. These can be mixed in any ratio. Among them, 4,4'-diaminodiphenyl ether and p-phenylenediamine are preferably used. By using such a diamine component, the thermal diffusivity of the graphite sheet finally obtained is good.
[0060] As a raw material of the polyimide film according to one embodiment of the present invention, it is preferred to use pyromellitic dianhydride in combination with 4,4'-diaminodiphenyl ether and / or p-phenylenediamine. According to this embodiment, there is an advantage that the polyimide film has excellent film-forming properties.
[0061] (Thickness of polyimide film)
[0062] The thickness of the polyimide film of one embodiment of the present invention is preferably 37 μm to 160 μm, more preferably 37 μm to 150 μm, further preferably 50 μm to 125 μm, and further preferably 62 μm to 100 μm. When the thickness of the polyimide film is within the above range, a graphite sheet having both good thermal diffusivity and interlayer strength can be obtained.
[0063] The lower limit of the thickness of the polyimide film of one embodiment of the present invention is preferably 37 μm or more, more preferably 50 μm or more, and more preferably 62 μm or more. In addition, the upper limit of the thickness of the polyimide film is preferably 160 μm or less, more preferably 150 μm or less, and more preferably 125 μm or less, and more preferably 100 μm or less. When the thickness of the polyimide film is 37 μm or more, it has the advantage of excellent interlayer strength, and when the thickness of the polyimide film is 160 μm or less, it has the advantage of excellent thermal diffusivity.
[0064] (Method for producing polyimide film)
[0065] The polyimide film of one embodiment of the present invention can be prepared by imidizing (imide conversion) the polyamic acid as a precursor. In the method for preparing the polyimide film, the method for imidizing the polyamic acid as a precursor can be, for example, any of the following methods: a thermal curing method, in which the polyamic acid as a precursor is heated to complete the imide conversion; or a chemical curing method, in which a shrinking agent represented by anhydrides such as acetic anhydride or an imidization promoter represented by tertiary amines such as picoline, quinoline, isoquinoline, and pyridine is used to convert the polyamic acid as a precursor into imide. When the chemical curing method is used, the tertiary amines mentioned above are preferably used as the imidization promoter.
[0066] In particular, from the perspective that the obtained film has a small linear expansion coefficient, a high elastic modulus, is easy to achieve a high birefringence, can quickly complete graphitization at a relatively low temperature, and can obtain a graphite sheet of good quality, the chemical curing method is preferred. It is particularly preferred to use a shrinking agent and an imidization accelerator together, so that the obtained film has a small linear expansion coefficient, a large elastic modulus, and a large birefringence. In addition, the chemical curing method can make the imidization reaction proceed faster, so that the imidization reaction can be completed in a short time during the heat treatment, and is therefore a method with excellent productivity and conducive to industrial production.
[0067] (Method for producing polyamic acid)
[0068] There is no particular limitation on the method for producing polyamic acid. For example, aromatic acid dianhydride and diamine can be dissolved in an organic solvent in substantially equimolar amounts, and the organic solution can be stirred under controlled temperature conditions until the polymerization of the dianhydride and diamine is completed, thereby producing polyamic acid. There is no particular limitation on the polymerization method. For example, any one of the following polymerization methods (1) to (5) is preferred. In this specification, substantially equimolar amounts means that the ratio of the molar amounts of two or more different substances is in the range of 100:98 to 100:102.
[0069] Method (1): An aromatic diamine is dissolved in an organic polar solvent, and the aromatic diamine is reacted with aromatic tetracarboxylic dianhydride in an amount substantially equimolar to the aromatic diamine to polymerize.
[0070] Method (2): Aromatic tetracarboxylic acid dianhydride is reacted with an aromatic diamine compound in a molar amount less than the aromatic tetracarboxylic acid dianhydride in an organic polar solvent to obtain a prepolymer having anhydride groups at both ends; then, the prepolymer is polymerized with an aromatic diamine compound in a substantially equimolar amount relative to the aromatic tetracarboxylic acid dianhydride.
[0071] As a specific example of the above method (2), a prepolymer having the acid dianhydride at both ends can be synthesized using a diamine and an acid dianhydride, and then a diamine of the same or different type as the diamine used in the synthesis of the prepolymer is reacted with the prepolymer to synthesize a polyamic acid. In method (2), the aromatic diamine reacting with the prepolymer can also be an aromatic diamine of the same or different type as the aromatic diamine used in the synthesis of the prepolymer.
[0072] Method (3): Aromatic tetracarboxylic dianhydride is reacted with an aromatic diamine compound in an excess molar amount relative to the aromatic tetracarboxylic dianhydride in an organic polar solvent to obtain a prepolymer having amino groups at both ends; then, the aromatic diamine compound is added to the prepolymer, and then the prepolymer and the aromatic tetracarboxylic dianhydride are polymerized in a manner such that the aromatic tetracarboxylic dianhydride and the aromatic diamine compound are substantially in equimolar amounts.
[0073] Method (4): After dissolving and / or dispersing aromatic tetracarboxylic dianhydride in an organic polar solvent, an aromatic diamine compound is added in a substantially equimolar amount relative to the acid dianhydride to polymerize the aromatic tetracarboxylic dianhydride and the aromatic diamine compound.
[0074] Method (5): A mixture of substantially equimolar amounts of an aromatic tetracarboxylic dianhydride and an aromatic diamine compound is reacted in an organic polar solvent to polymerize.
[0075] One embodiment of the present invention may be as follows.
[0076] [1] A method for producing a graphite sheet, comprising the step of heat-treating a polyimide film to a temperature of 2800° C. or higher, wherein the polyimide film contains inorganic particles and a phosphorus-containing non-metallic additive, wherein the content of the inorganic particles is 0.01% by weight or higher and 0.08% by weight or lower, and the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive is 0.018% by weight or higher and 0.032% by weight or lower, and the thermal diffusivity of the graphite sheet is 10.0 cm 2 / s or more.
[0077] [2] The method for producing a graphite sheet according to [1], wherein the inorganic fine particles are calcium hydrogen phosphate or calcium phosphate.
[0078] [3] The method for producing a graphite sheet according to [1] or [2], wherein the phosphorus-containing non-metallic additive is an organic phosphorus compound.
[0079] [4] The method for producing a graphite sheet according to [3], wherein the phosphorus in the organic phosphorus compound has a valence of five.
[0080] [5] The method for producing a graphite sheet according to any one of [1] to [4], wherein in a TG-DTA measurement of the phosphorus-containing non-metallic additive, the temperature at which the weight loss rate of the phosphorus-containing non-metallic additive reaches 5% is 200° C. or higher.
[0081] [6] The method for producing a graphite sheet according to any one of [1] to [5], wherein the graphite sheet is graphitized in a roll form.
[0082] [7] The method for producing a graphite sheet according to any one of [1] to [6], wherein the polyimide film has a thickness of 37 μm to 160 μm.
[0083] [8] The method for producing a graphite sheet according to any one of [1] to [7], wherein the polyimide film contains 4,4'-diaminodiphenyl ether.
[0084] [9] The method for producing a graphite sheet according to any one of [1] to [8], wherein the graphite sheet has a thickness of 16 μm to 85 μm.
[0085]
[10] The method for producing a graphite sheet according to any one of [1] to [9], wherein the total phosphorus content of the inorganic fine particles and the phosphorus-containing non-metallic additive is 0.021 wt % to 0.031 wt %.
[0086]
[11] A polyimide film for a graphite sheet, comprising inorganic particles and a phosphorus-containing non-metallic additive, wherein the content of the inorganic particles is from 0.01 wt % to 0.08 wt %, and the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive is from 0.018 wt % to 0.032 wt %.
[0087]
[12] The polyimide film for a graphite sheet according to
[11] , wherein the inorganic fine particles are calcium hydrogen phosphate or calcium phosphate.
[0088]
[13] The polyimide film for a graphite sheet according to
[11] or
[12] , wherein the phosphorus-containing non-metallic additive is an organic phosphorus compound.
[0089]
[14] The polyimide film for a graphite sheet according to
[13] , wherein the phosphorus in the organic phosphorus compound has a valence of five.
[0090]
[15] The polyimide film for a graphite sheet according to any one of
[11] to
[14] , wherein in TG-DTA measurement of the phosphorus-containing non-metallic additive, the temperature at which the weight loss rate of the phosphorus-containing non-metallic additive reaches 5% is 200° C. or higher.
[0091]
[16] The polyimide film for a graphite sheet according to any one of
[11] to
[15] , wherein the thickness is 37 μm to 160 μm.
[0092]
[17] The polyimide film for a graphite sheet according to any one of
[11] to
[16] , comprising 4,4'-diaminodiphenyl ether.
[0093]
[18] The polyimide film for a graphite sheet according to any one of
[11] to
[17] , wherein the total phosphorus content of the inorganic fine particles and the phosphorus-containing non-metallic additive is 0.021 wt % to 0.031 wt %.
[0094] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the following examples.
[0095] (Example)
[0096] <Phosphorus content in polyimide film>
[0097] The phosphorus content in the polyimide film was determined by using a wavelength dispersive X-ray fluorescence analyzer (ZSX Primus II manufactured by Rigaku Corporation) from a ratio with a polyimide film having a known phosphorus concentration.
[0098] <Transportability of polyimide film>
[0099] The transportability of the polyimide film was evaluated based on whether or not abnormality occurred in the polyimide film during the continuous carbonization step described in Examples below.
[0100] The evaluation criteria of the transportability of the polyimide film are as follows.
[0101] A: No problems were found in terms of handling and appearance.
[0102] B: Static electricity causes the films to adhere to each other, but there is no problem with the appearance and it can be treated
[0103] C: Minor scratches and wrinkles formed during transportation, but can be treated
[0104] D: Large wrinkles and scars were formed during transportation, and the film broke during the carbonization process
[0105] <Contamination of continuous carbonization furnace>
[0106] Regarding the contamination of the continuous carbonization furnace, the degree of contamination of the continuous carbonization furnace in the continuous carbonization step described in the Examples below was evaluated.
[0107] The evaluation criteria for contamination of the continuous carbonization furnace are as follows.
[0108] A: Almost no dirt was found
[0109] B: Dirt that can be easily wiped off
[0110] C: There is dirt that can be removed using an organic solvent
[0111] D: Dirt accumulates during continuous carbonization, causing small scratches on the membrane
[0112] <Melt-bonding of film during graphitization process>
[0113] Regarding the films after the graphitization step described in the Examples below, the degree of fusion between the films when the films were unwound was evaluated for the fusion of the films in the graphitization step.
[0114] The evaluation criteria of the fusion of the film in the graphitization step are as follows.
[0115] A: No melting or bonding was found
[0116] B: There is a fusion bonded area in part, but it can be easily peeled off when unwinding
[0117] C: There is a melt-bonded area, which breaks when unwinding continuously and needs to be peeled off manually
[0118] D: Strongly fused, can be broken even when peeled off by hand
[0119] <Thermal diffusivity in the plane direction of graphite sheet>
[0120] The thermal diffusivity in the surface direction of the graphite sheet was obtained by using the "Thermal Wave Analyzer TA3" of Bethel Co., Ltd., and measuring the sample of the graphite sheet cut into a shape of 30 mm × 30 mm in an atmosphere of 25°C and a frequency of 100 Hz. The sample was punched out in the center of the graphite sheet. Here, the "center" refers to the center part of the obtained graphite sheet in both the width direction and the length direction.
[0121] <Interlaminar strength of graphite sheets>
[0122] The interlayer strength of the graphite sheet was determined as follows. Double-sided tape was pasted on both sides of the obtained graphite sheet, and a 25 mm × 80 mm portion was punched out in the center to obtain a sample. One side of the sample was fixed to a SUS plate, and the double-sided tape on the opposite side was peeled off while maintaining a 90° angle. At this time, the force when peeling occurred inside the graphite sheet was measured using a digital force gauge (ZTS-5N manufactured by IMADA Co., Ltd.), and it was used as the interlayer strength of the graphite sheet.
[0123] <Density of graphite sheet>
[0124] A 50 mm square portion was punched out from the center of the obtained graphite sheet to obtain a sample. Then, the weight, area, and thickness of the sample were measured. Based on the measured weight value, the density of the graphite sheet was calculated using the mathematical formula: density of graphite sheet = weight of sample / (area of sample × thickness of sample).
[0125] <Thickness of graphite sheet>
[0126] The thickness of the obtained graphite sheet was measured at the four corners and one center using a micrometer manufactured by MITUTOYO Co., Ltd. Here, "one center" refers to the intersection of diagonal lines drawn from the measurement positions at the four corners to the measurement positions at the diagonal corners of the obtained graphite sheet. The average value of the obtained thickness measurement values was taken as the thickness of the graphite sheet.
[0127] (Example 1)
[0128] <Method for producing polyimide film>
[0129] In a dimethylformamide solution in which 75 mol% of 4,4'-diaminodiphenyl ether (ODA) was dissolved, 100 mol% of pyromellitic dianhydride (PMDA) was dissolved, followed by 25 mol% of p-phenylenediamine (PDA), to obtain a polyamic acid solution containing 18.5 wt% of polyamic acid. Calcium hydrogen phosphate was added to the obtained polyamic acid solution so that the concentration of calcium hydrogen phosphate relative to the solid content of the polyamic acid was 0.04 wt%. While cooling the solution, an imidization catalyst was added, and after degassing, a mixed solution was obtained, wherein the imidization catalyst contained: 1 equivalent of acetic anhydride and 1 equivalent of isoquinoline relative to the carboxylic acid group contained in the polyamic acid; dimethylformamide; and 0.32 wt% of resorcinol diphenyl phosphate relative to the solid content of the polyamic acid. The phosphorus content of the resorcinol diphenyl phosphate used at this time was 10.5 wt%, and the 5% weight loss temperature under TG-DTA measurement was 261°C.
[0130] Next, the mixed solution was applied on an aluminum foil so that the thickness after drying was 75 μm, thereby obtaining a mixed solution layer. The mixed solution layer on the aluminum foil was dried using a hot air oven and a far-infrared heater.
[0131] The specific drying method is as follows. First, the mixed solution layer on the aluminum foil is dried in a hot air oven at 120°C for 240 seconds to obtain a self-supporting gel film. The gel film is peeled off from the aluminum foil and fixed on a frame. Then, the gel film is heated in a hot air oven at 120°C for 30 seconds, at 275°C for 40 seconds, at 400°C for 42 seconds, at 450°C for 50 seconds, and at 460°C for 22 seconds in a far-infrared heater, thereby performing heat drying in stages. Part of the resorcinol bis(diphenyl phosphate) volatilizes during the drying process (film formation process). Through this operation, a polyimide film (A-1) with a calcium hydrogen phosphate content of 0.04% by weight, a resorcinol bis(diphenyl phosphate) content of 0.21% by weight, a total phosphorus content of 0.032% by weight, and a thickness of 75 μm was obtained.
[0132] <Method for producing graphite sheet>
[0133] A roll of a polyimide film (A-1) having a thickness of 75 μm, a width of 250 mm, and a length of 300 m was placed on the unwinding side of a film conveyor, and a continuous carbonization step was performed while the film was continuously moved to a heat treatment apparatus.
[0134] Continuous carbonization process Figure 1 The continuous carbonization device shown in the figure is carried out. The continuous carbonization device is composed of a device 12 for conveying a polyimide film 13 and a heat treatment device 11 having an inlet and outlet and a heating space. The polyimide film 13 is subjected to a heat treatment (carbonization process) in the heat treatment device 11, thereby continuously obtaining a carbonaceous film 14. The heat treatment device 11 has 6 heating spaces in the MD direction, each of which has a length of 500 mm in the MD direction and a length of 300 mm in the TD direction. Each heating space is substituted with nitrogen and the device is placed in a nitrogen atmosphere flow state (2L / min). The set temperatures are adjusted to 600°C, 615°C, 630°C, 645°C, 670°C, and 720°C, respectively. The conveying speed of the film (the polyimide film 13 and the carbonaceous film 14) in the continuous carbonization process is adjusted to 1.6 m / min, and the film is conveyed along the conveying direction 15 in such a way that the tension applied to the film reaches 10N. In the heating space of the heat treatment device 11, the film is conveyed by sandwiching the film from above and below with expanded graphite sheets (thermal conductivity 200 W / m·K, thickness 400 μm) as furnace materials. The furnace materials are arranged in contact with the film, and in the continuous carbonization process, the film is conveyed in a manner that the film slides along the furnace materials. In addition, the furnace materials are arranged so that their coverage range is larger than the passing range of the film in the heating space.
[0135] Next, the carbonaceous film 14 after the continuous carbonization step was cooled to room temperature (23° C.) and rolled into a roll having an inner diameter of 100 mm to obtain Figure 2 The carbonaceous film roll 21 shown. Figure 2 As shown, the carbonaceous film roll 21 was placed on the furnace 22 so that the width direction of the film was perpendicular to the furnace 22, and the temperature was raised to 3100°C at a heating rate of 1°C / min to perform a graphitization step. Figure 2 The middle arrow 23 indicates the direction of gravity.
[0136] Next, the film after the graphitization step was cooled to room temperature (23°C), and the graphitized film was subjected to a compression step (softening step) at room temperature (23°C) at a pressure of 10 MPa to obtain a graphite sheet. The properties of the compressed graphite sheet were examined through the above test.
[0137] (Examples 2 to 10, Comparative Examples 1 to 5)
[0138] A polyimide film was produced in the same manner as in Example 1 except that the added amounts of calcium hydrogen phosphate and resorcinol bis(diphenyl phosphate) were set to the amounts shown in Table 1, and a graphite sheet was produced using the polyimide film.
[0139] (Example 11)
[0140] A polyimide film having a resorcinol bis(diphenyl phosphate) content of 0.21 wt %, a total phosphorus content of 0.022 wt %, and a thickness of 75 μm was prepared in the same manner as in Example 1 except that calcium carbonate was used instead of calcium hydrogen phosphate, and a graphite sheet was prepared using the polyimide film.
[0141] (Example 12)
[0142] A polyimide film having a resorcinol bis(diphenyl phosphate) content of 0.21 wt %, a total phosphorus content of 0.022 wt %, and a thickness of 75 μm was prepared in the same manner as in Example 1 except that silicon dioxide was used instead of calcium hydrogen phosphate, and a graphite sheet was prepared using the polyimide film.
[0143] (Example 13)
[0144] A polyimide film having a resorcinol bis(diphenyl phosphate) content of 0.11 wt %, a total phosphorus content of 0.020 wt %, and a thickness of 75 μm was prepared in the same manner as in Example 3 except that calcium phosphate was used instead of calcium hydrogen phosphate, and a graphite sheet was prepared using the polyimide film.
[0145] (Example 14)
[0146] 0.49 wt % of triphenyl phosphate (phosphorus content: 9.5 wt %, 5% weight loss temperature under TG-DTA measurement: 220° C.) was added instead of resorcinol bis(diphenyl phosphate). In addition, a polyimide film having a triphenyl phosphate content of 0.13 wt %, a total phosphorus content of 0.022 wt %, and a thickness of 75 μm was prepared in the same manner as in Example 1, and a graphite sheet was prepared using the same.
[0147] (Example 15)
[0148] 0.30 wt % of triphenyl phosphine oxide (phosphorus content: 11.1 wt %, 5% weight loss temperature under TG-DTA measurement: 243° C.) was added instead of resorcinol bis(diphenyl phosphate). In addition, a polyimide film having a triphenyl phosphine oxide content of 0.11 wt %, a total phosphorus content of 0.022 wt %, and a thickness of 75 μm was prepared in the same manner as in Example 1, and a graphite sheet was prepared using the same.
[0149] (Example 16)
[0150] 0.15 wt% of diphenol bis(diphenyl phosphate) (phosphorus content: 9.5 wt%; 5% weight loss temperature under TG-DTA measurement: 395°C) was added instead of resorcinol bis(diphenyl phosphate). In addition, a polyimide film having a diphenol bis(diphenyl phosphate) content of 0.13 wt%, a total phosphorus content of 0.022 wt%, and a thickness of 75 μm was prepared in the same manner as in Example 1, and a graphite sheet was prepared using the film.
[0151] (Examples 17 to 20)
[0152] The polyimide film was prepared in the same manner as in Example 1 except that the thickness of the polyimide film was set to the thickness described in Table 1, and a graphite sheet was prepared using the polyimide film. The film formation time of the polyimide film and the temperature rise time of the graphitization process were adjusted in proportion to the thickness. For example, in the case of a film with a thickness of 50 μm, the firing time was shortened to 1 / 2 compared to the case of a film with a thickness of 100 μm.
[0153] Table 1 shows the production conditions and physical properties of the graphite sheets of Examples 1 to 20 and Comparative Examples 1 to 5.
[0154] (Table 1)
[0155]
[0156] According to Examples 1 to 20, the graphite sheets obtained from the polyimide film having an inorganic particle content of 0.01 wt% to 0.08 wt% and a phosphorus content of 0.018 wt% to 0.032 wt% were excellent in both thermal diffusivity and interlayer strength, and the fusion between the films in the graphitization process was improved. On the other hand, according to Comparative Example 1, the graphite sheets obtained from the polyimide film having an inorganic particle content of 0.10 wt% or more had high interlayer strength and no major problems were found in the fusion between the films in the graphitization process, but the thermal diffusivity was poor. In addition, according to Comparative Examples 2 to 4, the graphite sheets obtained from the polyimide film having a phosphorus content of 0.015 wt% or less had fusion between the films during graphitization, and cracks occurred when peeling, and no longer graphite sheets were obtained. In addition, according to Comparative Example 5, the polyimide film having an inorganic fine particle content of less than 0.01 wt % had poor transportability and cracked during the continuous carbonization step, and no graphite sheet was obtained.
[0157] (Industrial Applicability)
[0158] The graphite sheet obtained in the present invention has excellent productivity because fusion between films rarely occurs during the graphitization step, and has good thermal diffusivity and interlayer strength, so it can be preferably used as a heat dissipation component of electronic equipment.
Claims
1. A method for manufacturing a graphite sheet, The method comprises the steps of heat treating the polyimide film to above 2800°C. The polyimide film contains inorganic particles and a phosphorus-containing non-metallic additive, wherein the content of the inorganic particles is 0.01 wt % to 0.04 wt %, and the total phosphorus content of the inorganic particles and the phosphorus-containing non-metallic additive is 0.018 wt % to 0.032 wt %. The thermal diffusivity of the graphite sheet is 10.0 cm 2 / s or more.
2. The method for producing a graphite sheet according to claim 1, wherein: The inorganic particles are calcium hydrogen phosphate or calcium phosphate.
3. The method for producing a graphite sheet according to claim 1 or 2, wherein: The phosphorus-containing non-metallic additive is an organic phosphorus compound.
4. The method for producing a graphite sheet according to claim 3, wherein: The phosphorus valence of the organic phosphorus compound is 5.
5. The method for producing a graphite sheet according to claim 1 or 2, wherein: In TG-DTA measurement of the phosphorus-containing non-metallic additive, the temperature at which the weight loss rate of the phosphorus-containing non-metallic additive reaches 5% is 200° C. or higher.
6. The method for producing a graphite sheet according to claim 1 or 2, characterized in that: The graphite sheet is graphitized in the form of a scroll.
7. The method for producing a graphite sheet according to claim 1 or 2, wherein: The thickness of the polyimide film is 37 μm to 160 μm.
8. The method for producing a graphite sheet according to claim 1 or 2, wherein: The polyimide film contains 4,4'-diaminodiphenyl ether.
9. The method for producing a graphite sheet according to claim 1 or 2, wherein: The thickness of the graphite sheet is 16 μm to 85 μm.
10. The method for producing a graphite sheet according to claim 1 or 2, wherein: The total phosphorus content of the inorganic fine particles and the phosphorus-containing non-metallic additive is 0.021 wt % or more and 0.031 wt % or less.
11. A polyimide film for a graphite sheet, It contains inorganic particles and phosphorus-containing non-metallic additives. The content of the inorganic fine particles is 0.01 wt % or more and 0.04 wt % or less, The total phosphorus content of the inorganic fine particles and the phosphorus-containing non-metallic additive is 0.018 wt % or more and 0.032 wt % or less.
12. The polyimide film for a graphite sheet according to claim 11, wherein The inorganic particles are calcium hydrogen phosphate or calcium phosphate.
13. The polyimide film for a graphite sheet according to claim 11 or 12, wherein The phosphorus-containing non-metallic additive is an organic phosphorus compound.
14. The polyimide film for a graphite sheet according to claim 13, wherein The phosphorus valence of the organic phosphorus compound is 5.
15. The polyimide film for a graphite sheet according to claim 11 or 12, wherein In TG-DTA measurement of the phosphorus-containing non-metallic additive, the temperature at which the weight loss rate of the phosphorus-containing non-metallic additive reaches 5% is 200° C. or higher.
16. The polyimide film for a graphite sheet according to claim 11 or 12, Its thickness is 37 μm to 160 μm.
17. The polyimide film for a graphite sheet according to claim 11 or 12, It contains 4,4'-diaminodiphenyl ether.
18. The polyimide film for a graphite sheet according to claim 11 or 12, wherein The total phosphorus content of the inorganic fine particles and the phosphorus-containing non-metallic additive is 0.021 wt % or more and 0.031 wt % or less.
Citation Information
Patent Citations
Polyimide film and method for preparing the film