Curing of reactive resins using unsaturated peroxides as initiators and organic phosphites as accelerators

By using a two-component reactive resin system in road marking materials, combined with organic phosphites and unsaturated peroxides, the toxicology and environmental friendliness problems of the existing technology are solved, rapid curing and long-term stability are achieved, and improved Improved mechanical properties and durability, and reduced yellowing.

CN115916895BInactive Publication Date: 2024-10-29ROHM GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202180044321.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-01
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing road marking materials have problems in terms of toxicology and environmental friendliness. For example, dibenzoyl peroxide and aromatic amines are harmful to aquatic life when used as initiators and accelerators, and have long curing times, short durability, and easy Yellowing, affecting service life.

Method used

Adopting a two-component reactive resin system, one component contains organic phosphite as an accelerator, and the other component contains unsaturated peroxide as an initiator, combined with specific composition ratios and additives to achieve rapid curing and long-term curing stability while avoiding the use of aromatic amines and other harmful compounds.

Benefits of technology

It achieves rapid curing under low temperature conditions, shortens the curing time, improves the mechanical properties and durability of road markings, reduces yellowing, improves the friendliness to the environment and human health, and is suitable for a variety of application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004009657280000191
    Figure BDA0004009657280000191
  • Figure BDA0004009657280000201
    Figure BDA0004009657280000201
  • Figure BDA0004009657280000211
    Figure BDA0004009657280000211
Patent Text Reader

Abstract

The present invention relates to novel reaction resin formulations, for example for marking roads or for coating surfaces, which have a significantly improved property profile compared to the prior art. The reaction resins, in particular reaction resins based on novel curing agent systems, exhibit an improved combination of the following properties: higher long-term storage stability, improved toxicological profile, shortened curing times and low yellowing tendency, and better color fastness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to novel reaction resin formulations, which are used, for example, for marking roads or for coating surfaces, which offer a significantly improved property profile compared to the prior art. These reaction resins, in particular reaction resins based on novel curing systems, exhibit an improved combination of the following properties: higher long-term storage stability, improved toxicological profile, shortened curing times and low tendency to yellowing, and also better color fastnesses.

[0002] A number of requirements are imposed on modern road markings. On the one hand, it is desirable that such systems can be easily applied to the road surface and at the same time also provide for high storage stability and a long service life of the resulting marking. Equally important is rapid processing and, in particular, processing within as wide a temperature window as possible. In addition, it is required that the reaction resins used have as few toxicological problems as possible and that no highly toxic raw materials have to be handled during their preparation. In particular, reaction resins which exhibit rapid curing with as low a content of accelerating amines as possible are required. On the one hand, such amines constitute a health hazard for the processing personnel. On the other hand, undesirable side effects may also occur, such as yellowing of the coating when exposed to UV light. Background Art

[0003] At present, the following systems are used as road marking materials, such as solvent-based paints, water-based paints, thermoplastic paints, paints based on reactive resins and prefabricated adhesive tapes. The latter have the disadvantage that they are difficult to produce and apply. In addition, with regard to the desired durability of the markings, there is only limited freedom in the configuration of the markings (for example with glass beads).

[0004] Thermoplastic coatings, which are applied to the road surface in the molten state, can themselves also be optimized for fast curing speeds. Their use has the great disadvantage that an additional process step is required in which the product must first be melted, for example at 200° C., before it can be applied. This is not only potentially dangerous due to the high temperatures, but thermoplastic systems themselves also show increased wear and reduced resistance to thermal stress. The service life of thermoplastic systems is often significantly shorter than, for example, systems based on reactive resins and reacting during crosslinking.

[0005] Established systems for marking roads or for floor coatings are so-called reaction resins. Typically, these are two-component systems, which contain monomers, polymers and further components, such as fillers, auxiliaries or glass beads. Here, one component of the two-component system contains an initiator component and the second component contains an accelerator. Prior to application, the two components are mixed with one another and applied to the road or the floor within the pot life. Here, a suitable combination of initiator and accelerator matched thereto is very important. An inappropriate combination leads either to a short pot life, in which too strong a curing occurs before application, or to long curing times, in which the coating cures very late and usually incompletely.

[0006] Furthermore, reaction resins are often transported over long distances after their preparation. This results in long transport times, particularly in international shipping. Often, the resins are not used immediately after their preparation and must therefore have sufficient storage stability over a longer period of time. Reaction resins that have sufficient storage stability even at relatively high temperatures have the advantage of keeping requirements on storage and transport low, such as temperature-controlled transport or storage in cooled storage facilities. Furthermore, high storage stability is desirable from a safety point of view in order to avoid uncontrolled polymerization during preparation and storage.

[0007] For cold-curing systems at ambient temperatures, which prevail in outdoor applications (e.g. on roads or roofs), peroxides, such as dibenzoyl peroxide, are usually used as initiators. However, dibenzoyl peroxide is problematic from an ecotoxicity point of view, since it is harmful to aquatic organisms and has long-term effects.

[0008] In cold curing systems, aromatic tertiary amines such as N,N-dimethyl-p-toluidine, N,N-bis-(2-hydroxyethyl)-p-toluidine or N,N-bis-(2-hydroxypropyl)-p-toluidine are often used as accelerators. Such aromatic amines are also problematic in terms of toxicology.

[0009] For example, WO 2011 / 091908 describes reaction resins containing these components for coating road surfaces. DE 102012210121 A1 describes asymmetric aromatic amines as accelerators, which are less problematic in terms of toxicology. In the described systems, the yellowing typical for aromatic amines cannot be completely avoided. This effect is undesirable for coatings and, in particular, road markings.

[0010] A solution to improve curing and at the same time enable lower yellowing values ​​is to develop new curing agent systems which do not use aromatic amines.

[0011] US 3,639,370 describes triaryl phosphites and trialkyl phosphites with a chain length of 1 to 6 carbon atoms, which are used to activate permaleate. However, short-chain trialkyl phosphites, and particularly triethyl phosphites, which are preferably used to activate the compound, have extremely bad smells even at low concentrations due to their low odor threshold, so their use in reaction resins is problematic in processing open to the atmosphere. In addition, the short-chain trialkyl phosphites disclosed in US 3,639,370 for activating permaleate also show considerable disadvantages: they cause reaction resin gelation in a very short time, with the result that only very short processing time is available. In practice, too short processing time can lead to poor applicability because the curing or polymerization of reaction resin occurs too early. In Example 47 of US 3,639,370, it is mentioned that the gel time is 1 minute and the duration until the maximum temperature is reached during the curing process is 7 minutes when using triethyl phosphite. It can be seen that the curing time exceeds 7 minutes. In view of the extremely short gel time, it is not practically possible to process these systems manually. Even in machine laying, for example in spraying methods, the extremely short pot life poses a challenge, since in the event of an interruption, there is only a very short time left for cleaning the contaminated machine parts. In addition, US Pat. No. 3,639,370 also describes other compounds for activating permaleic esters, which are however toxicologically problematic and in some cases carcinogenic and have primarily an unpleasant odor.

[0012] WO 2012 / 146438 A1 discloses an accelerator system containing a combination of permaleate and zinc-, sulfur- and phosphorus compounds for curing (meth) acrylate resins in thin layers. However, the main disadvantage of this curing agent system is that the corresponding reaction resin has only a short pot life or processing time, and at the same time has a relatively long curing time (the time required until a non-sticky surface is obtained). Example 15 of WO 2012 / 146438 mentions a gel time of 3 minutes and a curing time of 35 minutes. In practice, this can only allow machine processing, such as by spraying methods, to mark roads. Compared with conventional cold spray plastic systems with BPO / amine curing systems (which have a typical curing time of less than 10 minutes), the system disclosed in WO 2012 / 146438 is much slower in terms of complete curing. This means that the corresponding coating can only be driven through later, which can cause longer traffic jams during marking work. Summary of the invention

[0013] Purpose of the Invention

[0014] In view of the prior art in question, it is an object of the present invention to provide a novel reaction resin which is less dangerous to humans and the environment than the prior art. This means, in particular, that the activators or accelerators used should be less problematic from a human toxicological point of view and that the initiators used should be less toxic to aquatic organisms.

[0015] Furthermore, the object of the present invention is to provide a reaction resin which has a sufficient pot life compared to the prior art and thus results in a coating which can be processed both by machine (with immediate drive-over capability) and manually. In particular, the curing time should be at most five times the pot life. This means that the coating can be mechanically loaded sufficiently quickly so that, for example, newly applied road markings can be driven over immediately by traffic.

[0016] Furthermore, it was an object that the reaction resins can be used, in particular, even at relatively cold application temperatures, ie, for example, in the range from 5° C. to 25° C. and also in contact with oxygen or air and exhibit tack-free curing.

[0017] Furthermore, it was an object to provide reaction resins which, after application in suitable compositions, show virtually no discoloration, for example yellowing, over a longer period of time, in particular under UV weathering.

[0018] Furthermore, the newly developed two-component reaction resins should exhibit comparable mechanical properties and likewise comparable durability when applied as road markings compared to two-component resins known from the prior art with hardener systems based, for example, on dibenzoyl peroxide and amines. For technically simple preparation and processing of the reaction resins, the accelerator component should in particular be liquid at room temperature so that simple mixing into the reaction resin is possible. In this way, the reaction resin can be additionally activated at low temperatures, if desired, shortly before application, for example on a construction site, by adding a further accelerator.

[0019] In this case, the use of the newly developed reaction resins is not limited to road markings, but they can also be used in other fields of application, such as reactive coatings and reactive sealants, for example roof and bridge sealants, floor coatings, corrosion protection, intumescent coatings, but also in reaction resin compositions, such as those for artificial stone, polymer concrete, hygiene products or also dental or orthopedic resins or bone cements, and reaction resin compositions for adhesives.

[0020] Further objects not explicitly mentioned result from the overall context of the following description, claims and exemplary embodiments.

[0021] Solution

[0022] The object is achieved by providing a novel two-component reaction resin system which contains in one component at least one organic phosphite as accelerator, which has at least one alkyl group which is longer than in the prior art, and in the other component an unsaturated peroxide as initiator.

[0023] Here, according to the invention, the two components of the two-component reaction resin based on (meth)acrylates together contain the following ingredients:

[0024] 0 to 30% by weight of a crosslinking agent,

[0025] 20 to 85% by weight of monomers,

[0026] 0 to 60% by weight of urethane (meth)acrylate,

[0027] 0 to 40% by weight of a prepolymer,

[0028] Optional other adjuvants, and

[0029] 1. 15 to 10 wt. % of a curing agent system, the curing agent system comprising:

[0030] 0.15 to 5 wt. % of a permaleate, and

[0031] 1.0 to 10 wt. % of a tertiary organic phosphite.

[0032] The content data given here for the permaleate and the tertiary organic phosphite are based on the total amount of the two-component reaction resin.

[0033] Here, the permaleate on the one hand and the tertiary organic phosphite on the other hand are contained in separate components of the two-component reaction resin before the two components are mixed together.

[0034] Furthermore, the two-component reaction resin according to the invention is characterized in that the tertiary organic phosphite has the general formula P(OR1)(OR2)(OR3), wherein R1, R2 and R3 are identical or different radicals from one another and at least one of these radicals has more than 6 C atoms.

[0035] If crosslinkers are present, they are preferably used in a minimum concentration of 0.5% by weight.

[0036] Preference is given here to compositions in which the two components together contain the following ingredients:

[0037] 2 to 20% by weight, particularly preferably 3 to 15% by weight, of a crosslinker, preferably a polyfunctional (meth)acrylate, most particularly preferably a di-, tri- or tetra-(meth)acrylate,

[0038] 25 to 75% by weight, particularly preferably 30 to 40% by weight, of (meth)acrylates and / or monomers copolymerizable with (meth)acrylates, the acrylate content being a maximum of 5% by weight of the two-component reaction resin,

[0039] 0 to 45% by weight, particularly preferably up to 30% by weight, of urethane (meth)acrylates,

[0040] 10% to 35% by weight, particularly preferably 15% to 25% by weight, of prepolymers, preferably poly(meth)acrylates and / or polyesters, particularly preferably poly(meth)acrylates,

[0041] Optional other adjuvants, and

[0042] 2 to 7.5 wt. %, particularly preferably 2 to 7 wt. %, of a curing agent system containing, based on the two-component reaction resin,

[0043] 0.5 to 4.0% by weight, particularly preferably 0.75 to 3.5% by weight, of permaleic acid esters, and

[0044] 1.5 to 6.0% by weight, particularly preferably 2.0 to 5.0% by weight, of a tertiary organic phosphite.

[0045] The further auxiliaries may be, for example, stabilizers, inhibitors, chain transfer agents or waxes. Preferably, the reaction resins according to the invention are halogen-free.

[0046] The permaleate is preferably tert-butyl monopermaleate.

[0047] In a particular embodiment of the present invention, the two-component reaction resin is a two-component reaction resin with a particularly high content of urethane (meth) acrylate. Such a two-component reaction resin preferably contains the following substances as components in both components of the reaction resin:

[0048] 0 to 20% by weight of a multifunctional (meth)acrylate,

[0049] 25 to 75% by weight of (meth)acrylates and / or monomers copolymerizable with (meth)acrylates, wherein the content of acrylates is at most 5% by weight of the two-component reaction resin,

[0050] 10 to 60% by weight of urethane (meth)acrylate,

[0051] 10 to 35% by weight of a prepolymer,

[0052] Optional other adjuvants, and

[0053] 2.0 wt % to 7.5 wt % of a curing agent system, the curing agent system containing, based on the two-component reaction resin,

[0054] 0.5 to 4.0 wt. % of permaleate, and

[0055] 1.5 to 6.0 wt. % of a tertiary organic phosphite.

[0056] Surprisingly, it has been found that with the aid of organophosphites, the activation reaction is accelerated, in particular compared to systems according to the prior art, to such an extent that curing occurs even at temperatures of 5° C. and below. In addition, the curing is accelerated to such an extent that shorter curing times are achieved.

[0057] As the organic tertiary phosphite, tertiary phosphites and tertiary thiophosphites of alkyl, aryl, alkoxyaryl, alkoxyalkyl and heterocyclic with the formula P(XR1)(XR2)(XR3) are used. Here, R1, R2 and R3 are identical to or different from each other and refer to alkyl, cycloalkyl, aryl, alkoxyalkyl, arylalkyl or tetrahydrofurfuryl groups. X can be oxygen or sulfur.

[0058] Typical examples of such tertiary phosphites or thiophosphites to be used according to the invention are tri-2-ethylhexyl phosphite, tri-2-ethylhexyl trithiophosphite, triisooctyl phosphite, triisooctyl trithiophosphite, tridecyl phosphite, tridecyl trithiophosphite, trilauryl phosphite, trilauryl trithiophosphite, trioctadecyl phosphite, trioctadecyl trithiophosphite, phenyl didecyl phosphite, trithiophosphite, trioctadecyl phosphite, trioctadecyl trithiophosphite, tri ... Phenyl didecyl phosphate, phenyl dilauryl phosphite, phenyl distearyl phosphite, phenyl distearyl trithiophosphite, diphenyl decyl phosphite, diphenyl lauryl phosphite, diphenyl stearyl phosphite, diphenyl stearyl trithiophosphite, tri-p-tolyl phosphite, tri-m-tolyl phosphite, tri-o-tolyl phosphite, tri-p-tolyl dithiophosphite, tri-p-octylphenyl trithiophosphite, tri-o-octylphenyl phosphite, phosphorus Phosphite tris (dipropylene glycol) ester, triethoxyethyl phosphite, tributoxyethyl phosphite, tris (tetrahydrofurfuryl) phosphite, tris (tetrahydrofurfuryl) trithiophosphite, triphenylethyl phosphite, S-phenyl dilauryl monothiophosphite, S-phenyl didecyl monothiophosphite, SS-diphenyl lauryl dithiophosphite, SS-diphenyl decyl dithiophosphite, tri-o-naphthyl phosphite, SS-diphenyl decyl dithiophosphite, tri-o-naphthyl phosphite, SS-diphenyl decyl dithiophosphite, tri-o-naphthyl phosphite Phenyl dilauryl phosphite, tris(trip dodecylphenyl) phosphite, tri-o-chlorophenyl phosphite, diphenyl lauryl trithiophosphite, S-lauryl diphenyl monothiophosphite, tri-p-methoxyphenyl phosphite, SO-diphenyl-S-lauryl dithiophosphite, tri-o-methoxyphenyl dithiophosphite, SS-dilaurylphenyl dithiophosphite and SO-dilauryl-S-phenyl dithiophosphite.

[0059] The tertiary organic phosphite is preferably a compound having three identical alkyl groups R1, R2 and R3, wherein accordingly all three alkyl groups have more than 6 C atoms. A particularly preferred example of the tertiary organic phosphite is triisodecyl phosphite.

[0060] Furthermore, the reaction resin according to the invention may contain further accelerators, for example in the form of symmetrical aromatic tertiary amines, such as those known from the prior art. In such an embodiment of the invention, this addition leads to an additional acceleration of the reaction resin and a shortened curing time compared to the prior art. Examples of such symmetrical aromatic tertiary amines may include N,N-dimethyl-p-toluidine, N,N-bis-(2-hydroxyethyl)-p-toluidine or N,N-bis-(2-hydroxypropyl)-p-toluidine.

[0061] However, preference is given to embodiments in which only organic phosphites are used as accelerators and the two-component reaction resin accordingly contains no amines overall. Surprisingly, it has been found that in contrast to the prior art, the reaction resin can be cured in the absence of amines at a rate comparable to established systems. This means that, overall, the formulation is significantly less critical from a toxicological point of view than the systems of the prior art.

[0062] The two-component reaction resin according to the invention preferably contains less than 5% by weight of acrylates and particularly preferably contains no acrylates.

[0063] The two-component reaction resin according to the invention can be provided in different embodiments. In a first such embodiment, the second component of the reaction resin consists exclusively of the components of the hardener system. These are then not contained in the first component of the two-component reaction resin. In such an embodiment, for example, the accelerator is added to the remaining components containing the initiator, followed by mixing and application. Alternatively, the initiator can be added accordingly to the otherwise fully formulated reaction resin containing the accelerator.

[0064] In another embodiment, the first and second components of the reaction resin have the same composition except for the components of the curing agent system. In this case, two separate components containing the initiator on the one hand and the accelerator on the other hand are mixed with each other before application.

[0065] Other embodiments, for example divided into more than two components, are also conceivable.

[0066] It has been found to be very advantageous if the two-component reaction resin according to the invention additionally contains 0.3% to 3% by weight of one or more paraffin waxes. These paraffin waxes are characterized in that their solidification point according to DIN-ISO 2207 is in the temperature range of 35° C. to 75° C.

[0067] Surprisingly, it has also been found that embodiments of the two-component reaction resin according to the invention can be used in a particularly advantageous manner when the two-component reaction resin contains up to 5% by weight of acrylate groups, based on the sum of acrylate groups and methacrylate groups. From this point of view, therefore, not only the polymerizable acrylate and methacrylate content of the monomers must be taken into account, but also other groups, such as are contained or may be contained in particular in the crosslinker or in the urethane (meth)acrylate.

[0068] In particular, in addition to the two-component reaction resins described, cold plastics produced with these two-component reaction resins are also part of the invention. These cold plastics contain the following components:

[0069] This cold plastic according to the invention can be used, for example, as a road marking, a sealant or a floor coating. In particular, it is characterized in that the cold plastic contains the following substances as components:

[0070] 5 to 80% by weight, preferably 10 to 60% by weight, of a two-component reaction resin according to the above description,

[0071] 0.15 to 25% by weight, preferably 1 to 20% by weight and particularly preferably 1.5 to 15% by weight, of one or more pigments, preferably inorganic pigments, particularly preferably titanium dioxide,

[0072] 15 to 90% by weight of inorganic or mineral fillers,

[0073] 0% to 5% by weight, preferably 0.3% to 3% by weight, of further stabilizers and / or additives not contained in the two-component reaction resin, and

[0074] 0 to 90 wt% of organic fillers, preferably polymer fillers.

[0075] The total amount of the filler here preferably amounts to 50% to 80% by weight of the cold plastic.

[0076] In the case of use for marking road surfaces, the components of the cold plastic are mixed before or during application to the road surface. In the case of other uses, the components are mixed shortly before or during casting, coating or filling. In this case, the final formulation of the cold plastic and the mixing of the individual components of the two-component reaction resin can, for example, be carried out simultaneously.

[0077] Surprisingly, it has been found that the cold plastics according to the invention applied as road markings have particularly fast re-roadability. The term "drive-through capability" or the synonymous term "re-roadability" is understood to mean that a load is applied to the road marking, for example in the form of a vehicle driving over it. The time period until the drive-through capability is reached is the time interval between the application of the road marking until the point in time when the marking compound no longer spreads on the road when a tire passes over it.

[0078] Detailed description of the components of the cold plastic or the reaction resin

[0079] In addition, the cold plastic or cold spray plastic may contain other additives, such as crosslinking agents and / or dispersants, anti-skid fillers and anti-settling agents that improve the anti-skid properties of automobiles. Glass beads can also be added to improve reflection, or glass beads may already be included in the components of the cold plastic. Alternatively, the glass beads can be put in place after being applied to the surface. In the case of an operation used, for example, in a modern marking vehicle with a second nozzle, the beads are sprayed directly onto these components after applying the first two components. The advantage of this operation is that only a portion of the glass beads embedded in the marking matrix is ​​wetted by the components of the other two components, and thus the best reflective properties are obtained. However, most particularly, in the application of this technology, the particularly good embeddability of the glass beads and the corresponding good adhesion of the marking matrix or road marking formulation to the surface of the glass beads are important. Surprisingly, it has been found that the reaction resin according to the present invention or the cold spray plastic containing this reaction resin meets these required properties, at least to the level of the prior art. The required properties for road markings are clearly defined in DIN EN 1436.

[0080] In order to further improve the desired properties, the glass beads can be applied together with an adhesion promoter or pretreated with such an adhesion promoter. In this way, the retroreflective properties and day and night visibility of the cold plastic according to the invention are at least comparable to the prior art. The same applies to the durability, in particular the durability of the embedding of the glass beads.

[0081] In the novel curing agent system, unsaturated peroxides, in particular tert-butyl permaleate, are used as initiators. In some cases, it may be advantageous to use a mixture of different initiators. Typically, the peroxide in the second component is mixed with a diluent, such as an oil or a plasticizer. However, the concentrations described above in the reaction resin according to the invention only relate to pure initiators.

[0082] Optional components of the reaction resin according to the invention are crosslinkers, in particular polyfunctional methacrylates, such as allyl (meth)acrylate. Particularly preferred are di- or tri-(meth)acrylates, such as 1,4-butanediol di(meth)acrylate, poly(urethane) (meth)acrylate, tetraethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate or trimethylolpropane tri(meth)acrylate.

[0083] The optionally contained urethane (meth) acrylates are understood in the context of the present invention to mean compounds containing (meth) acrylate functionalities bonded to one another via urethane groups. They can be obtained by reacting hydroxyalkyl (meth) acrylates with polyisocyanates and polyoxyalkylenes having at least two hydroxyl functionalities. Instead of hydroxyalkyl (meth) acrylates, esters of (meth) acrylic acid with oxiranes, such as ethylene oxide or propylene oxide, or corresponding oligomeric or polyoxiranes can also be used. For example, an overview of urethane (meth) acrylates with a functionality greater than 2 can be found in DE 19902685. A commercially available example prepared from polyols, isocyanates and hydroxyl-functional (meth) acrylates is EBECRYL 210-5129 from Allnex. In reaction resins, urethane (meth) acrylates increase flexibility, tear resistance and elongation at break without a large temperature dependence. Surprisingly, it has been found that with the new curing system, even urethane acrylates can be cured tack-free without problems at relatively high weight contents. This opens up the possibility of preparing flexible reaction resins, such as those required, for example, for road markings or sealing systems, while largely dispensing with acrylate monomers which usually have a low glass transition temperature.

[0084] In particular, the monomers contained in the reaction resin are compounds selected from (meth)acrylates, such as alkyl (meth)acrylates of linear, branched or alicyclic alcohols having 1 to 40 C atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate; aryl (meth)acrylates, such as benzyl (meth)acrylate; Mono(meth)acrylates of ethers having 5 to 80 carbon atoms, polyethylene glycols, polypropylene glycols or mixtures thereof, for example tetrahydrofurfuryl(meth)acrylate, methoxy(methoxy)ethoxyethyl(meth)acrylate, benzyloxymethyl(meth)acrylate, 1-ethoxybutyl(meth)acrylate, 1-ethoxyethyl(meth)acrylate, ethoxymethyl(meth)acrylate, poly(ethylene glycol)methyl ether(meth)acrylate and poly(propylene glycol)methyl ether(meth)acrylate.

[0085] The (meth)acrylic acid esters also include esters formed from (meth)acrylic acid and acetals, ketals or carbonates of glycerol, substituted glycerol or trimethylolpropane or substituted trimethylolpropane.

[0086] Preferred examples of such monomers are glycerol formal (meth)acrylate, trimethylolpropane formal (meth)acrylate or isopropylidene glycerol (meth)acrylate (glycerol acetonate methacrylate).

[0087] Surprisingly, it has been found that the reaction resin composition according to the invention preferably contains up to 5% by weight of acrylate monomers, based on the two-component reaction resin. This allows for a short curing time compared to the pot life. In a very particularly preferred embodiment, the two-component reaction resin contains no acrylate monomers.

[0088] Suitable monomer mixture components also include further monomers with other functional groups, for example α,β-unsaturated mono- or dicarboxylic acids, such as acrylic acid, methacrylic acid or itaconic acid; esters of acrylic acid or methacrylic acid with diols, such as hydroxyethyl (meth)acrylate or hydroxypropyl (meth)acrylate; acrylamide or methacrylamide; or dimethylaminoethyl (meth)acrylate. Other suitable components of the monomer mixture are, for example, glycidyl (meth)acrylate or silyl-functional (meth)acrylates.

[0089] In addition to these (meth)acrylates, the monomer mixture may also contain other unsaturated monomers which are copolymerizable with the above-mentioned (meth)acrylates by means of free-radical polymerization. These include, in particular, 1-olefins or styrenes. In the individual case, the poly(meth)acrylates are selected in terms of content and composition, taking into account the desired technical function.

[0090] In the so-called MO-PO systems, in addition to the monomers listed, there are also polymers, which are referred to herein as prepolymers for better differentiation, preferably polyesters or poly(meth)acrylates. These are added to the resins to improve the polymerization properties, mechanical properties, adhesion to substrates and optical requirements. Since in a preferred embodiment only small amounts of acrylate monomers with a low glass transition temperature are used to flexibilize the reaction resins, in addition to methacrylate monomers with a corresponding glass transition temperature, prepolymers with a low glass transition temperature can also be used for this purpose, wherein the prepolymers themselves can in turn consist of acrylate monomers.

[0091] Both the polyester and the poly(meth)acrylate may have additional functional groups for adhesion promotion or for copolymerization in the crosslinking reaction, for example in the form of double bonds. However, in view of better color fastness of the road marking, the prepolymer preferably does not have any double bonds. The poly(meth)acrylates are generally composed of the same monomers as those already listed for the monomers in the resin system. They can be obtained by solution polymerization, emulsion polymerization, suspension polymerization, bulk polymerization or precipitation polymerization and added to the system as pure substances. The polyesters are essentially obtained by polycondensation or ring-opening polymerization and they consist of structural units known for these applications.

[0092] As auxiliary agents and additives, chain transfer agents, plasticizers, paraffins, stabilizers, inhibitors, waxes and / or oils can additionally be used. Paraffins are added to prevent polymerization from being inhibited by oxygen in the air. For this purpose, a variety of paraffins with different melting points can be used in different concentrations. It has been found to be very advantageous if the two-component reaction resin according to the invention additionally contains 0.3% by weight to 3% by weight of one or more paraffins. These paraffins are characterized in that their solidification point according to DIN-ISO 2207 is in the temperature range of 35° C. to 75° C.

[0093] All compounds known from free-radical polymerization can be used as chain transfer agents. Preferably, mercaptans are used, for example n-dodecyl mercaptan. Preferably, esters, polyols, oils, low molecular weight polyethers or phthalates are used as plasticizers.

[0094] UV stabilizers can also be used. Preferably, the UV stabilizer is selected from benzophenone derivatives, benzotriazole derivatives, thioxanthonate derivatives, piperidinol carboxylate derivatives or cinnamate derivatives. From the group of stabilizers or inhibitors, substituted phenols and hydroquinone derivatives are preferably used.

[0095] The two-component reaction resin or cold plastic or in other final formulations based on the two-component reaction resin according to the invention may optionally also contain the following components:

[0096] Wetting agents, dispersants and leveling assistants are preferably selected from alcohols, hydrocarbons, glycol derivatives, glycolate derivatives, acetates and polysiloxanes, polyethers, polysiloxanes, polycarboxylic acids and saturated and unsaturated polycarboxylic acid aminoamides.

[0097] Preferred for use as rheological additives are polyhydroxycarboxylic acid amides, urea derivatives, salts of unsaturated carboxylic acid esters, alkylammonium salts of acidic phosphoric acid derivatives, ketoximes, amine salts of p-toluenesulfonic acid, amine salts of sulfonic acid derivatives and aqueous or organic solutions or mixtures of these compounds. It has been found that particularly suitable rheological additives are based on pyrogenic or precipitated, optionally also silanized, silicic acid, whose BET surface area is from 10 to 700 nm. 2 / g.

[0098] Preference is given to using defoamers selected from the group consisting of alcohols, hydrocarbons, paraffin-based mineral oils, glycol derivatives, glycolate derivatives, acetates and silicones.

[0099] Similar components may be involved in the auxiliaries and additives additionally used in the cold plastics.

[0100] As already mentioned above, dyes, glass beads, fine and coarse fillers, wetting agents, dispersants and leveling agents, UV stabilizers, defoamers and rheological additives, which can be used, for example, for road markings, can be added to the cold plastics. For the application of the formulation as road markings, for example lines, stripes or symbols, or for marking areas such as bicycle lanes or bus lanes or parking spaces, auxiliaries and additives, preferably dyes, are added. Particularly preferred are white, red, blue, green and yellow inorganic pigments, and particularly preferred are white pigments, for example titanium dioxide.

[0101] Glass beads are preferably used as reflectors in formulations for road markings and area markings. Commercially customary glass beads have a diameter of 10 μm to 2000 μm, preferably 50 μm to 800 μm. The glass beads may have an adhesion promoter for better processing and adhesion. Preferably, the glass beads may be silanized.

[0102] One or more mineral fine and coarse fillers may also be added to the cold plastic. These materials also act as anti-slip agents and are therefore used in particular to improve the grip and also for coloring the road markings. The fine fillers used are selected from calcium carbonate, barium sulfate, quartz, quartz powder, precipitated and pyrolytic silicic acid, pigments and cristobalite and corundum. As coarse fillers, quartz, cristobalite, corundum and aluminosilicates are used.

[0103] The two-component reaction resins according to the invention allow such great freedom in formulation that the two-component reaction resins according to the invention or the cold plastics / cold spray plastics according to the invention containing the reaction resins can be formulated and doped with additives just like the established systems of the prior art. Thus, the wear resistance, durability, whiteness, pigmentation and grip properties are also at least as good as those of the prior art systems.

[0104] This quality, which is at least comparable to that of the prior art, also applies to the storage stability of the reaction resins. The system can also be optimized with respect to the substrate to be coated by selecting suitable monomers, prepolymers and / or adhesion promoters. Accordingly, the system according to the invention can be variably optimized for marking surfaces of asphalt, concrete or natural stone.

[0105] Use of the reactive resin or cold plastic / cold spray plastic

[0106] In addition to the described two-component reaction resins according to the invention and the cold plastics containing them, a method for applying the two-component reaction resins is also part of the invention. The method is characterized in that the two components of the two-component reaction resin according to the invention are mixed with one another within 2 minutes to 40 minutes before application to the substrate or during application. Here, the expression "application to the substrate" is to be interpreted in a broad sense. It therefore includes not only, for example, the coating of the surface, but also actions such as mold filling.

[0107] In this case, the substrate can be, in particular, a road surface, paving stones, concrete, screed, asphalt, ceramic or steel, in particular steel in the form of steel beams.

[0108] The two-component reaction resins according to the invention furthermore allow the production of yellowing-free artificial stone moldings at ambient temperature, for example for the production of sanitary products in unheated casting molds.

[0109] Preferably, the two-component reaction resins according to the invention or cold plastics containing these reaction resins are used for road markings, in particular for producing durable road markings, or for floor coatings or sealants, in particular in the industrial or commercial sector. However, this enumeration is not intended to limit the applications of the reaction resins or cold plastics according to the invention in any way.

[0110] The system according to the invention is also flexible in terms of application technology. For example, the reaction resin or cold plastic according to the invention can be applied in a spraying, pouring or extrusion method or manually applied with the aid of a spatula, roller or scraper.

[0111] The individual components of the cold plastic, for example the two-component reaction resin according to the invention, can be mixed before, after or during further processing, for example application to a road surface. Methods for mixing in before further processing are already established, wherein it should be noted that after mixing in the curing agent component, only a limited open time remains for application, for example 2 or 40 minutes. Mixing in the process can be achieved, for example, in modern marking machines, which are equipped with a mixing chamber upstream of the application nozzle. The mixing in of the curing agent after application can be carried out, for example, by subsequent application with two or more nozzles or by applying glass beads coated with a curing agent. Alternatively, a primer containing the curing component can be sprayed in advance before applying the cold plastic or cold spray plastic.

[0112] Furthermore, the mechanical properties of the road markings produced with the two-component reaction resins according to the invention are very good in the typical range between 200 μm and 7000 μm, regardless of the application thickness. The application thickness of the cold plastic or cold spray plastic according to the invention is preferably between 400 μm and 1000 μm and particularly preferably between 600 μm and 800 μm. Thicker and thinner layers are also possible, depending on the application.

[0113] Preferably, the two-component reaction resins according to the invention or the cold plastics produced therefrom are used for producing durable road markings.

[0114] For example, the two-component reaction resin or cold plastic is used in a method in which the glass beads are added before, during or shortly after the cold plastic is applied to the road surface.

[0115] Alternatively, the reaction resins and / or cold plastics according to the invention can also be used in other technical fields. Examples include floor coverings, preferably for industrial applications, for the production of cast parts, for sealing or coating roofs, bridges or their joints, in particular as sealing films, for general bridge coatings, as sealing films on roofs, for the production of panels, for example for further use as decking, for the production of protective coatings, in particular for metal surfaces, as trough resins, for the production of sanitary products, for the production of adhesives, for filling cracks, for example in buildings, or in the field of orthopedics. DETAILED DESCRIPTION

[0116] Example

[0117] The examples given below are given in order to better illustrate the present invention and are not intended to limit the present invention to the features disclosed herein.

[0118] As curing agent, a mixture of tert-butyl permaleate with plasticizers, desensitizers and other auxiliaries was used, which had a peroxide content of about 25% by weight. In particular, in the following examples—unless otherwise indicated—PEROXAN PM-25 S from the company Pergan was used.

[0119] The pot life is determined as the time required for the material to rise from room temperature (i.e. a temperature of 20 to 22° C.) to 32° C. after the curing agent has been stirred in and after the components of the two-component reaction resin have been mixed. For this purpose, a sample amount of 20 g of the two-component reaction resin is mixed together in a plastic container.

[0120] In the so-called O-test, the time required to achieve a tack-free surface is determined. For this purpose, the timer is started when the hardener is stirred into the material and, after the hardener has been completely mixed in, the mixture is poured into a tin lid in a layer thickness of 2 mm. The time is then stopped when the surface is no longer found to be tacky when touched with a gloved finger. All these tests are carried out by the same operator.

[0121] Curing of methacrylate-based reaction resins

[0122] Comparative Example 1

[0123] In this comparative example, a two-component reaction resin based on methacrylate was cured with a benzoyl peroxide / N,N′-dihydroxyethyl-p-toluidine curing agent system according to the prior art.

[0124] 98.5 g of DEGADUR MDP Membrane SG (a commercially available methacrylate-based reactive resin without accelerator, GmbH) was mixed with 1.50 g of N,N'-dihydroxyethyl-p-toluidine. Thereafter, for curing, 2.0 g of Perkadox CH-50 (dibenzoyl peroxide powder, 50%, with dicyclohexyl phthalate, Nouryon) were added and stirred until the added peroxide was completely dissolved in the reaction resin.

[0125] This yields the following results:

[0126] Applicable period: 11 minutes

[0127] T 最大 =119℃

[0128] T 最大 After 17 minutes

[0129] O-test = 23 minutes

[0130] After 24 hours, the color of the 2 mm thick polymer films from the O-test was visually evaluated on a white substrate. A clear yellowing could be discerned.

[0131] Example 1

[0132] In this example according to the invention, the corresponding two-component reaction resin was cured with a hardener system based on TBPM (tert-butyl permaleate) and phosphites.

[0133] 98.0 g of DEGADUR MDP Membrane SG were mixed with 2.00 g of tris(2-ethylhexyl) phosphite. Thereafter, for curing, 4.0 g of PEROXAN PM-25 S (25% by weight suspension of tert-butyl permaleate in TBPM with plasticizer from Pergan) were added and stirred until the added peroxide was completely dissolved in the reaction resin.

[0134] This yields the following results:

[0135] Pot life = 10 minutes

[0136] T 最大 =129℃

[0137] T 最大 After 15 minutes

[0138] O-test = 20 minutes

[0139] After 24 hours, the color of the 2 mm thick polymer films from the O-test was visually evaluated on a white substrate. No yellowing was visible.

[0140] A comparison of the corresponding results of comparative example 1 and example 1 shows that the reaction resins according to the invention exhibit comparable pot lives and curing times, but without causing yellowing of the polymer.

[0141] Examples 2 to 4

[0142] The curing of these two-component reaction resins according to the examples of the invention with the TBPM / phosphite curing agent system was carried out as follows:

[0143] DEGADUR MDP Membrane SG was mixed with triisodecyl phosphite as an accelerator in each case. The reaction resin was then placed in a climate chamber for heat treatment. After temperature adjustment, PEROXAN PM-25 S was then added for curing and stirred until the added peroxide was completely dissolved in the reaction resin. The curing of the reaction resin was also carried out in a climate chamber. Table 1 shows the external temperature, the respective mixing ratios and the measurement results:

[0144] Table 1

[0145]

[0146] Examples 2 to 4 show that when using the two-component reaction resins according to the invention, by adapting the amount of curing agent, complete, tack-free curing can be achieved within a short time even within a wide temperature range, down to low temperatures, wherein the pot life is long enough for processing practice.

[0147] Curing of reactive resins containing methacrylates and acrylates

[0148] In the following, the influence of the acrylates in the reaction resin on the curing behavior was investigated.

[0149] In Examples 5 to 12, DEGADUR MDP Primer SG B (a commercially available amine-free methacrylate-based reactive resin, GmbH, containing 0.5% by weight of triisodecyl phosphite) was mixed in each case with different amounts of 2-ethylhexyl acrylate and additional triisodecyl phosphite as an accelerator. Then, for curing, PEROXAN PM-25S (tert-butyl permaleate, 25%, suspension, with plasticizer, Pergan) was added and stirred until the added peroxide was completely dissolved in the reaction resin. The respective mixing ratios of Examples 5 to 8 and the measurement results are shown in Table 2.

[0150] Table 2

[0151]

[0152] Examples 5 to 8 show that the curing performance deteriorates with increasing weight content of acrylate monomers. Therefore, in such new systems, higher acrylate content is disadvantageous.

[0153] The results and compositions of the initiator systems of Examples 9 to 12 are shown in Table 3. In these Examples 9 to 12 a relatively large amount of phosphite was used.

[0154] Table 3

[0155]

[0156] Surprisingly, it has been found that in Examples 9 to 12, by using relatively large amounts of organic phosphites, complete and tack-free curing can be achieved even with increased weight contents of acrylate monomers.

[0157] Calculation of the content of acrylate groups in the compositions according to Examples 5 to 12

[0158] For illustrative purposes, the weight content of acrylate groups in the resin components of Examples 5 to 12 was calculated as follows.

[0159]

[0160] The acrylate groups have an equivalent weight of 55.06 g / mol, which results in a weight content of 29.9% (55.06 g / mol / 184.28 g / mol=29.9%), for example, in 2-ethylhexyl acrylate.

[0161] Table 4

[0162]

[0163] Embodiment 13

[0164] 49.0 g of Ebecryl 230 (commercially available urethane acrylate, Allnex) was mixed with 46.2 g of methyl methacrylate, 0.80 g of paraffin wax (Sasolwax 5105) and 4.0 g of triisodecyl phosphite as an accelerator at 55°C until the paraffin wax was completely dissolved. The resin was then cooled to 23°C.

[0165] For curing, 4.0 g of PEROXAN PM-25S (tert-butyl permaleate, 25%, suspension, with plasticizer, Pergan) were added and stirred until the added peroxide was completely dissolved in the reaction resin. Table 5 shows the composition and results.

[0166] Table 5

[0167]

[0168] Example 13 shows that it is not the weight content of acrylate compounds that is relevant for tack-free curing, but rather the quantitative proportion of functional acrylate groups. Thus, despite the presence of a high content of acrylate compounds in the form of urethane acrylates, this does not lead to any substantial impairment of the curing due to the low weight proportion of functional acrylate groups.

Claims

1. A two-component reaction resin based on (meth)acrylates, wherein the reaction resin comprises a first component and a second component, which together contain the following substances as constituents: 0 to 30% by weight of a crosslinking agent, 20 to 85% by weight of monomers, 0 to 60% by weight of urethane (meth)acrylate, 0 to 40% by weight of a prepolymer, Optional other adjuvants, and 1.15 wt % to 10 wt % of a curing agent system, the curing agent system containing, based on the two-component reaction resin 0.15 to 5% by weight of permaleate, 1.0 to 10% by weight of a tertiary organic phosphite, and the permaleate on the one hand and the tertiary organic phosphite on the other hand are contained in separate components of the two-component reaction resin before the two components are mixed together, and the tertiary organic phosphite has the general formula P(OR1)(OR2)(OR3), wherein R1, R2 and R3 are identical or different groups from each other, and at least one of these groups has more than 6 C atoms; The reaction resins contain up to 5% by weight of acrylate monomers, based on the two-component reaction resin.

2. The two-component reaction resin according to claim 1, characterized in that The two components of the reaction resin together contain the following substances as ingredients: 2 to 20% by weight of a multifunctional (meth)acrylate, 25 to 75% by weight of (meth)acrylate and / or a monomer copolymerizable with (meth)acrylate, 0 to 45% by weight of urethane (meth)acrylate, 10 to 35% by weight of a prepolymer, Optional other adjuvants, and 2 wt % to 7.5 wt % of a curing agent system, the curing agent system containing, based on the two-component reaction resin, 0.5 to 4.0 wt% of a permaleate, and 1.5 to 6.0 wt % of a tertiary organic phosphite.

3. The two-component reaction resin according to claim 1, characterized in that The two components of the reaction resin together contain the following substances as ingredients: 0 to 20% by weight of a multifunctional (meth)acrylate, 25 to 75% by weight of (meth)acrylate and / or a monomer copolymerizable with (meth)acrylate, 10 to 60% by weight of urethane (meth)acrylate, 10 to 35% by weight of a prepolymer, Optional other adjuvants, and 2 wt % to 7.5 wt % of a curing agent system, the curing agent system containing, based on the two-component reaction resin, 0.5 to 4.0 wt% of a permaleate, and 1.5 to 6.0 wt % of a tertiary organic phosphite.

4. The two-component reaction resin according to claim 1 or 2, characterized in that The two components of the reaction resin together contain the following substances as ingredients: 3 to 15% by weight of a multifunctional methacrylate, 30% to 40% by weight of (meth)acrylates and / or monomers copolymerizable with (meth)acrylates, wherein at most 5% by weight of the monomers, based on the total amount of the two-component reaction resin, are acrylates, 0 to 30% by weight of urethane (meth)acrylate, 15 to 25% by weight of a prepolymer, Optional other adjuvants, and 2 to 7 wt % of a curing agent system, the curing agent system comprising 0.75% to 3.5% by weight of permaleate, 2.0 to 5.0 wt. % of a tertiary organic phosphite.

5. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The permaleate is tert-butyl monopermaleate.

6. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The tertiary organic phosphite is triisodecyl phosphite.

7. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The two-component reaction resin is free of amines.

8. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The two-component reaction resin does not contain acrylates.

9. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The second component of the reaction resin consists exclusively of the constituents of the hardener system which are not contained in the first component.

10. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The first component and the second component of the reaction resin have the same composition, except for the constituents of the hardener system.

11. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The reaction resin contains 0.3% to 3% by weight of one or more paraffin waxes whose solidification point according to DIN-ISO 2207 is in the temperature range of 35° C. to 75° C.

12. The two-component reaction resin according to any one of claims 1 to 3, characterized in that The two-component reaction resin contains up to 5% by weight of acrylate groups, based on the total amount of acrylate and methacrylate groups.

13. Method for applying a two-component reaction resin, characterized in that The two components of the reaction resin according to any one of claims 1 to 12 are mixed with one another within 2 minutes to 40 minutes before application to the substrate or during application.

14. The method according to claim 13, characterized in that The substrate is a road surface, paving stones, concrete, screed, asphalt, ceramic or steel.

15. The method according to claim 14, characterized in that The substrate is steel in the form of a steel beam.

16. Cold plastics for use as road markings, sealants or floor coatings, characterized in that The cold plastic contains the following substances as ingredients: 5% to 80% by weight of a two-component reaction resin according to any one of claims 1 to 12, 0.15% to 25% by weight of one or more pigments, 15 to 90% by weight of an inorganic filler, 0% to 5% by weight of further stabilizers and / or additives not contained in the two-component reaction resin, and 0 to 90 wt% organic filler.

17. Cold plastic according to claim 16, characterized in that The cold plastic contains the following substances as ingredients: 10% to 60% by weight of a two-component reaction resin according to any one of claims 1 to 11, 1.5 to 15% by weight of one or more inorganic pigments, 0.3% to 3% by weight of further stabilizers and / or additives not contained in the two-component reaction resin, and A total of 50 to 80 wt% of inorganic fillers and organic fillers, wherein the organic filler is a polymer.

18. Cold plastic according to claim 17, characterized in that The inorganic pigment is titanium dioxide.

Citation Information

Patent Citations

  • Urethane (meth)acrylate, useful for the production of coatings for flat roof and parking decks, has at least 3 terminal ethylenically unsaturated reactive groups.

    DE19902685A1

  • Process for polymerization of olefinic compounds

    US3639370A

  • Formulations for producing roadway markings with adhesion on dry and damp concrete

    WO2011091908A1

  • Accelerant system for curing reaction resins having permaleinate below room temperature

    WO2012146438A1

  • Low-odour (meth)acrylic reaction resins

    CN103649194A