Preparation method and application of a carbohydrate-modified activated carbon carrier and catalyst

Through the combination of sugar-modified activated carbon carrier and metal palladium and copper salts, the problem of poor stability of the carbonylation catalyst of methyl nitrite is solved, the catalytic activity and stability are improved, and the carbonylation of methyl nitrite to dimethyl carbonate is realized Efficient catalysis of reactions.

CN115920873BActive Publication Date: 2024-10-08FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211349456.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-10-08
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

The existing chlorine-containing catalysts for the carbonylation of methyl nitrite have poor stability, causing the catalytic activity to decrease with the loss of chloride ions, making it difficult to achieve industrial application.

Method used

By modifying the chlorine-containing catalyst carrier with sugar, a sugar-modified activated carbon carrier is prepared, and combined with metal palladium salt and metal copper salt for impregnation treatment to form a high-efficiency catalyst for the carbonylation reaction of methyl nitrite to dimethyl carbonate. .

Benefits of technology

It significantly improves the stability and catalytic activity of the catalyst, enhances the interaction between the active metal and the carrier, increases the microporosity and Lewis acid strength of the catalyst, and extends the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115920873B_ABST
    Figure CN115920873B_ABST
Patent Text Reader

Abstract

The present application discloses a preparation method and application of a carbohydrate-modified activated carbon carrier and catalyst, belonging to the field of activated carbon modification technology and catalyst. A preparation method of a carbohydrate-modified activated carbon carrier comprises the following steps: S1, heating a mixture containing activated carbon and water to obtain pretreated activated carbon; S2, adding the pretreated activated carbon to a mixed liquid containing sugars and water for closed impregnation to obtain impregnation-treated activated carbon; S3, calcining the impregnation-treated activated carbon to obtain carbohydrate-modified activated carbon. The catalyst prepared by this preparation method has higher microporosity, carbon defect degree and Lewis acid strength; and exhibits excellent catalytic activity in the reaction of catalyzing the carbonylation of methyl nitrite to synthesize dimethyl carbonate. The active metal dispersion of the catalyst is high, and the interaction between the active metal and the carrier is enhanced, thereby greatly improving the catalytic activity and stability of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a preparation method and application of a carbohydrate-modified activated carbon carrier and catalyst, and belongs to the technical field of activated carbon modification and the field of catalysts. Background Art

[0002] Dimethyl carbonate has a unique molecular structure with multiple functional groups such as carbonyl, methoxy and methoxycarbonyl. It can be used as a carbonylation agent, methylation agent, fuel additive and lithium-ion battery electrolyte additive, etc. It is an important chemical substance. There are many methods for the synthesis of dimethyl carbonate, mainly including phosgene method, ester exchange method, urea alcoholysis method, methanol oxidative carbonylation method, CO2 direct conversion method and methyl nitrite carbonylation method. Among them, the methyl nitrite carbonylation method with mild reaction conditions and green raw materials is a hot topic of research.

[0003] The catalysts for the carbonylation of methyl nitrite are divided into chlorine-free systems and chlorine-containing systems. The former has outstanding stability but low activity, while the latter has outstanding catalytic activity but poor stability. The activity of the catalyst often decreases with the loss of chloride ions. Therefore, developing a catalyst with both high activity and high stability is the only way to achieve industrialization of the carbonylation of methyl nitrite to produce dimethyl carbonate.

[0004] In chlorine-containing catalytic systems, activated carbon with excellent properties such as developed pore structure, large specific surface area and good thermal stability is recognized as a good catalyst carrier. In addition, the pore structure and surface physicochemical properties of activated carbon can be regulated by physical or chemical means, which further expands the application of activated carbon in catalyst carriers.

[0005] Li Rui and others from Ningxia University used transition metals as activators to modify activated carbon carriers and applied them to the synthesis of dimethyl carbonate by methanol gas-phase oxidation carbonylation. The study found that the catalytic performance of the modified catalysts was significantly improved, among which CuCl2 was used as the activator and the mass ratio of the activator to the carrier was 1:1, and the methanol conversion rate increased from 18.9% before modification to 33.1%. Jiang Ruixia's team from Hebei University of Technology found that changing the electronic microenvironment of the active site of the catalyst can change the catalytic performance. The team found that CH3COOK interacts with the active metal on the activated carbon carrier. The introduction of CH3COOK helps to inhibit the loss of chloride ions, thereby improving the catalytic activity of the catalyst and inhibiting the deactivation of the catalyst. Ren Jun's team from Taiyuan University of Technology found that adding an appropriate concentration of KOH is beneficial to increasing the oxygen-containing functional groups on the surface of the activated carbon carrier, thereby improving the dispersion of the active metal and improving the catalytic activity. Sugars, as widely available, inexpensive, environmentally friendly and sustainably renewable materials, are gaining more and more attention and are widely used as catalyst carriers. To date, there has been no report on the use of sugar-modified activated carbon to generate a composite carrier for the catalytic carbonylation of methyl nitrite to synthesize dimethyl carbonate. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcoming of poor stability of chlorine-containing system catalysts in the prior art for carbonylation of methyl nitrite, and to improve the stability of the catalyst while maintaining the high catalytic activity of the chlorine-containing system catalyst by modifying the chlorine-containing system catalyst carrier, thereby providing a preparation and application of a sugar-modified activated carbon carrier for the carbonylation reaction of methyl nitrite.

[0007] According to the first aspect of the present application, a method for preparing a carbohydrate-modified activated carbon carrier is provided.

[0008] A method for preparing a sugar-modified activated carbon carrier comprises the following steps:

[0009] S1, heating a mixture containing activated carbon and water to obtain pretreated activated carbon;

[0010] S2, adding the pretreated activated carbon into a mixture containing sugars and water for sealed immersion to obtain impregnated activated carbon;

[0011] S3, calcining the impregnated activated carbon to obtain sugar-modified activated carbon.

[0012] Optionally, in step S1, the particle size of the activated carbon is 10 mesh to 60 mesh;

[0013] The internal pore size of the activated carbon is 2nm to 100nm;

[0014] The specific surface area of ​​the activated carbon is 500m 2 / g~3500m2 / g.

[0015] Optionally, the particle size of the activated carbon is independently selected from any value of 10 mesh, 20 mesh, 30 mesh, 40 mesh, 50 mesh, 60 mesh, or any range value between two of them.

[0016] Optionally, the specific surface area of ​​the activated carbon is independently selected from 500m 2 / g、1000m 2 / g、1500m 2 / g, 2000m 2 / g、2500m 2 / g、3000m 2 / g、3500m 2 / g, or any range of values ​​between them.

[0017] Optionally, the mass ratio of the activated carbon to water is 2 to 20:500.

[0018] Optionally, the mass ratio of the activated carbon to water is independently selected from any value among 2:500, 4:500, 6:500, 8:500, 10:500, 12:500, 14:500, 16:500, 18:500, 20:500 or any range value between two of them.

[0019] Optionally, in step S1, the heating conditions are as follows:

[0020] The temperature is 90℃~120℃;

[0021] The time is 12h~48h.

[0022] Optionally, the temperature is independently selected from any value among 90°C, 95°C, 100°C, 105°C, 110°C, 120°C or any range therebetween.

[0023] Optionally, the time is independently selected from any value of 12h, 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h, 36h, 40h, 44h, 48h, or a range between any two of them.

[0024] Optionally, in step S2, the sugar is selected from at least one of glucose, fructose, sucrose, maltose, starch and cellulose.

[0025] Optionally, in step S2, the mass concentration of the sugar in the mixed solution is 0.5wt% to 10wt%.

[0026] Optionally, the mass concentration of the sugar in the mixed solution is independently selected from any value among 0.5wt%, 1.0wt%, 2.0wt%, 3.0wt%, 4.0wt%, 5.0wt%, 6.0wt%, 7.0wt%, 8.0wt%, 9.0wt%, 10.0wt% or any range between two of them.

[0027] Optionally, in step S2, the mass ratio of the pretreated activated carbon to the mixed liquid is 1:1-20.

[0028] Optionally, the mass ratio of the pretreated activated carbon to the mixed liquor is independently selected from any value among 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20 or any range value between two of them.

[0029] Optionally, in step S2, the immersion time is 12 hours to 48 hours.

[0030] Optionally, the immersion time is independently selected from any value of 12h, 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h, 36h, 40h, 44h, 48h, or any range therebetween.

[0031] Optionally, in step S3, the calcination conditions are as follows:

[0032] The temperature is 400℃~900℃;

[0033] The time is 6h~18h.

[0034] Optionally, the temperature is independently selected from any value of 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, or any range therebetween.

[0035] Optionally, the time is independently selected from any value of 6h, 8h, 10h, 12h, 14h, 16h, 18h, or a range between any two of them.

[0036] Optionally, in step S3, the heating rate is 2°C / min to 10°C / min;

[0037] The cooling rate is 2℃ / min~10℃ / min.

[0038] Optionally, in step S3, the calcination atmosphere is an inert gas;

[0039] The inert gas is selected from nitrogen, argon and helium.

[0040] Optionally, in step S3, the inert gas flow rate is 40 mL / min to 400 mL / min.

[0041] According to a second aspect of the present application, a method for preparing a methyl nitrite carbonylation catalyst is provided.

[0042] A method for preparing a methyl nitrite carbonylation catalyst comprises the following steps:

[0043] Sealingly impregnating a mixed solution containing a carrier and a metal palladium salt / metal copper salt to obtain the catalyst;

[0044] The carrier is selected from the sugar-modified activated carbon obtained by the above-mentioned preparation method.

[0045] Optionally, the metal palladium salt is selected from at least one of palladium chloride, palladium bromide, palladium nitrate, palladium sulfate, palladium acetate, and palladium acetylacetonate.

[0046] Optionally, the metal copper salt is selected from at least one of copper chloride, copper bromide, copper nitrate, copper sulfate, copper acetate and copper acetylacetonate.

[0047] Optionally, the mass ratio of the metal palladium salt to the carrier is 0.1 to 20:100.

[0048] Optionally, the mass ratio of the metal palladium salt to the carrier is independently selected from any value among 0.1:100, 0.5:100, 1.0:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, 11:100, 12:100, 13:100, 14:100, 15:100, 16:100, 17:100, 18:100, 19:100, 20:100 or any range value between two of them.

[0049] Optionally, the mass ratio of the metal copper salt to the carrier is 0.2-30:100.

[0050] Optionally, the mass ratio of the metal copper salt to the carrier is independently selected from any value among 0.2:100, 0.5:100, 1.0:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, 11:100, 12:100, 13:100, 14:100, 15:100, 16:100, 17:100, 18:100, 19:100, 20:100, 25:100, 30:100, or any range value between two of them.

[0051] Optionally, the immersion time is 6 hours to 24 hours.

[0052] According to a third aspect of the present application, a use of a methyl nitrite carbonylation catalyst is provided.

[0053] The methyl nitrite carbonylation catalyst obtained by the preparation method is used in the reaction of preparing dimethyl carbonate by carbonylation of methyl nitrite.

[0054] Optionally, methyl nitrite and CO are contacted and reacted in the presence of a methyl nitrite carbonylation catalyst.

[0055] Optionally, the contacting process is carried out in a fixed bed reactor or a fluidized bed reactor.

[0056] Optionally, the molar ratio of CO to methyl nitrite is 1:1-20.

[0057] Optionally, the reaction conditions are as follows:

[0058] The temperature is 90℃~150℃;

[0059] Pressure 0Mpa~3Mpa.

[0060] Optionally, the buffer gas is nitrogen.

[0061] Optionally, the total space velocity of nitrogen, methyl nitrite and CO is 1000 L / (kg·h) to 20000 L / (kg·h).

[0062] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme: Preparation and application of a carbohydrate-modified activated carbon carrier

[0063] It includes four steps: pretreatment, impregnation, calcination and loading.

[0064] The specific implementation steps are as follows:

[0065] Step 1: Preprocessing

[0066] The pretreatment method comprises placing the activated carbon in ultrapure water, controlling the temperature at 90°C to 120°C, removing the upper black oil film while heating and stirring, and the process lasts for 12 to 48 hours, then filtering out the activated carbon, rinsing it with ultrapure water, placing it in an oven, and drying it at 100°C to 140°C for 6 to 24 hours to obtain the pretreated activated carbon;

[0067] The activated carbon has a particle size of 10 to 60 meshes, an internal pore size of 2 to 100 nanometers, and a specific surface area of ​​1500 to 2000 m 2 / g;

[0068] The mass ratio of the activated carbon to the ultrapure water used for pretreatment is 2-20:500;

[0069] Step 2: Dipping

[0070] The impregnation method comprises dissolving the sugar in ultrapure water, transferring the solution into a volumetric flask to obtain an impregnation solution, placing the pretreated activated carbon into the impregnation solution and covering it with a layer of plastic wrap, removing the plastic wrap after impregnation for 12 to 36 hours, standing for 12 to 48 hours, placing the solution in an oven after the liquid basically disappears, drying the solution at 100 to 140 degrees Celsius for 6 to 24 hours, and taking the solution out to obtain the impregnation-treated activated carbon;

[0071] The sugar is one of glucose, fructose, sucrose, maltose, starch and cellulose;

[0072] The sugar dissolving temperature is 80°C to 120°C;

[0073] The mass concentration of the impregnation liquid is 0.5wt% to 10wt%;

[0074] The mass ratio of the pretreated activated carbon to the impregnation liquid is 1:1 to 20;

[0075] Step 3: Calcination

[0076] The calcination method comprises placing the impregnated activated carbon into a tubular furnace, introducing an inert gas after evacuation, heating the furnace to 400° C. to 900° C., keeping the temperature for 6 to 18 hours, cooling the furnace to room temperature, taking the activated carbon out, and obtaining the sugar-modified activated carbon after sieving.

[0077] The inert gas is one of nitrogen, argon and helium;

[0078] The inert gas flow rate is 40 mL / min to 400 mL / min;

[0079] The heating rate is 2°C / min to 8°C / min;

[0080] The cooling rate is 4°C / min to 10°C / min;

[0081] The particle size of the sugar-modified activated carbon obtained by the screening is 10 to 60 meshes;

[0082] Step 4: Load

[0083] The loading is to use sugar-modified activated carbon as a carrier, load metal palladium salt and metal copper salt by impregnation method, cover with plastic wrap and let stand for 6 to 24 hours, remove the plastic wrap and let stand for another 6 to 24 hours, put into an oven after the liquid basically disappears, dry at 100° C. / min to 140° C. for 6 to 24 hours, and then take out to obtain a catalyst;

[0084] The impregnation method is one of an excess impregnation method, an equal volume impregnation method, a multiple impregnation method, and an impregnation precipitation method;

[0085] The metal palladium salt is one of palladium chloride, palladium bromide, palladium nitrate, palladium sulfate, palladium acetate, and palladium acetylacetonate;

[0086] The metal copper salt is one of copper chloride, copper bromide, copper nitrate, copper sulfate, copper acetate, and copper acetylacetonate;

[0087] The mass ratio of the loaded metal palladium salt to the sugar-modified activated carbon is 0.1 to 10:100;

[0088] The mass ratio of the loaded metal copper salt to the sugar-modified activated carbon is 0.1 to 10:100;

[0089] The catalytic reaction of synthesizing dimethyl carbonate from methyl nitrite is a reaction in which CO and methyl nitrite are used as reaction raw materials and dimethyl carbonate is generated as a main product under the action of the catalyst.

[0090] The beneficial effects of this application include:

[0091] The present application provides a method for preparing a methyl nitrite carbonylation catalyst. The catalyst prepared by the preparation method has higher microporosity, carbon defect degree and Lewis acid strength. The catalyst prepared by the preparation method exhibits excellent catalytic activity in the reaction of catalyzing the carbonylation of methyl nitrite to synthesize dimethyl carbonate. The active metal dispersion of the catalyst is high, and the interaction between the active metal and the carrier is enhanced, thereby greatly improving the catalytic activity and stability of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0092] Figure 1 This is a graph showing the change in CO conversion rate versus reaction time when the catalysts of Examples 1, 2, 3 and the comparative example react continuously for 10 hours.

[0093] Figure 2 It is a comparison chart of the space-time yield of the catalysts of Examples 1, 2, 3 and the comparative example after being stabilized for 22 hours.

[0094] Figure 3 It is the Raman characterization result of the catalyst of Example 1, 2, 3 and the comparative example.

[0095] Figure 4 It is the H2-TPR characterization result of the catalysts of Examples 1, 2, 3 and the comparative example. DETAILED DESCRIPTION

[0096] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0097] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0098] The analysis method in the examples of this application is as follows:

[0099] Nitrogen adsorption-desorption analysis was performed using ASAP 2460 apparatus (Micromeritics, America).

[0100] H2-TPR analysis was performed using AutoChem II 2920 Chemisorber (Micromeritics, America).

[0101] Raman analysis was performed using a Micro Confocal Raman spectrometer (Horiba Jobin Yvon).

[0102] Example 1: Preparation of sugar-modified activated carbon carrier and catalyst

[0103] The following steps are involved:

[0104] Step 1: Preprocessing

[0105] The pretreatment method comprises placing the activated carbon in ultrapure water, controlling the temperature at 100° C., removing the upper black oil film while heating and stirring, and the process lasts for 24 hours, then filtering out the activated carbon, rinsing it with ultrapure water, placing it in an oven, and drying it at 120° C. for 12 hours to obtain the pretreated activated carbon;

[0106] The particle size of the activated carbon is 30 mesh;

[0107] The mass ratio of the activated carbon to the ultrapure water used for pretreatment is 5:500.

[0108] Step 2: Dipping

[0109] The impregnation method comprises dissolving the sugar in ultrapure water, transferring the solution into a volumetric flask to obtain an impregnation solution, placing the pretreated activated carbon into the impregnation solution and covering it with a layer of plastic wrap, removing the plastic wrap after impregnation for 12 hours, standing for 12 hours, placing the solution in an oven after the liquid basically disappears, drying the solution at 120° C. for 12 hours, and taking the solution out to obtain the impregnation-treated activated carbon;

[0110] The sugar is starch;

[0111] The sugar dissolving temperature is 100°C;

[0112] The mass concentration of the impregnation liquid is 3wt%;

[0113] The mass ratio of the pretreated activated carbon to the impregnation liquid is 1:3.3.

[0114] Step 3: Calcination

[0115] The calcination method comprises placing the impregnated activated carbon into a tubular furnace, introducing an inert gas after evacuation, heating to 600° C., keeping the temperature for 8 hours, and then cooling down. After cooling to room temperature, the activated carbon is taken out and sieved to obtain the sugar-modified activated carbon.

[0116] The inert gas is nitrogen;

[0117] The inert gas flow rate is 300 mL / min;

[0118] The heating rate is 2°C / min;

[0119] The cooling rate is 5°C / min;

[0120] The particle size of the sugar-modified activated carbon obtained by screening is 30 mesh, the average internal pore size is 2.5 nanometers, and the specific surface area is 1667 m 2 / g.

[0121] Step 4: Load

[0122] The loading is to use sugar-modified activated carbon as a carrier, load metal palladium salt and metal copper salt by impregnation method, cover with plastic wrap and let stand for 12 hours, remove the plastic wrap and let stand for another 12 hours, put into an oven after the liquid basically disappears, and take out after drying at 120° C. for 12 hours to obtain a catalyst;

[0123] The impregnation method is an equal volume impregnation method;

[0124] The metal palladium salt is palladium chloride;

[0125] The metal copper salt is copper chloride;

[0126] The mass ratio of the loaded metal palladium salt to the sugar-modified activated carbon is 1.7:100;

[0127] The mass ratio of the loaded metal copper salt to the sugar-modified activated carbon is 3.2:100.

[0128] Example 2: Preparation of sugar-modified activated carbon carrier and catalyst

[0129] The following steps are involved:

[0130] Step 1: Preprocessing

[0131] The pretreatment method comprises placing the activated carbon in ultrapure water, controlling the temperature at 100° C., removing the upper black oil film while heating and stirring, and the process lasts for 24 hours, then filtering out the activated carbon, rinsing it with ultrapure water, placing it in an oven, and drying it at 120° C. for 12 hours to obtain the pretreated activated carbon;

[0132] The particle size of the activated carbon is 30 mesh;

[0133] The mass ratio of the activated carbon to the ultrapure water used for pretreatment is 5:500.

[0134] Step 2: Dipping

[0135] The impregnation method comprises dissolving the sugar in ultrapure water, transferring the solution into a volumetric flask to obtain an impregnation solution, placing the pretreated activated carbon into the impregnation solution and covering it with a layer of plastic wrap, removing the plastic wrap after impregnation for 12 hours, standing for 12 hours, placing the solution in an oven after the liquid basically disappears, drying the solution at 120° C. for 12 hours, and taking the solution out to obtain the impregnation-treated activated carbon;

[0136] The sugar is starch;

[0137] The sugar dissolving temperature is 100°C;

[0138] The mass concentration of the impregnation liquid is 4wt%;

[0139] The mass ratio of the pretreated activated carbon to the impregnation liquid is 1:3.3.

[0140] Step 3: Calcination

[0141] The calcination method comprises placing the impregnated activated carbon into a tubular furnace, introducing an inert gas after evacuation, heating to 600° C., keeping the temperature for 8 hours, and then cooling down. After cooling to room temperature, the activated carbon is taken out and sieved to obtain the sugar-modified activated carbon.

[0142] The inert gas is nitrogen;

[0143] The inert gas flow rate is 300 mL / min;

[0144] The heating rate is 2°C / min;

[0145] The cooling rate is 5°C / min;

[0146] The particle size of the sugar-modified activated carbon obtained by screening is 30 mesh, the average internal pore size is 2.5 nanometers, and the specific surface area is 1669 m 2 / g.

[0147] Step 4: Load

[0148] The loading is to use sugar-modified activated carbon as a carrier, load metal palladium salt and metal copper salt by impregnation method, cover with plastic wrap and let stand for 12 hours, remove the plastic wrap and let stand for another 12 hours, put into an oven after the liquid basically disappears, and take out after drying at 120° C. for 12 hours to obtain a catalyst;

[0149] The impregnation method is an equal volume impregnation method;

[0150] The metal palladium salt is palladium chloride;

[0151] The metal copper salt is copper chloride;

[0152] The mass ratio of the loaded metal palladium salt to the sugar-modified activated carbon is 1.7:100;

[0153] The mass ratio of the loaded metal copper salt to the sugar-modified activated carbon is 3.2:100.

[0154] Example 3: Preparation of sugar-modified activated carbon carrier and catalyst

[0155] The following steps are involved:

[0156] Step 1: Preprocessing

[0157] The pretreatment method comprises placing the activated carbon in ultrapure water, controlling the temperature at 100° C., removing the upper black oil film while heating and stirring, and the process lasts for 24 hours, then filtering out the activated carbon, rinsing it with ultrapure water, placing it in an oven, and drying it at 120° C. for 12 hours to obtain the pretreated activated carbon;

[0158] The particle size of the activated carbon is 30 mesh;

[0159] The mass ratio of the activated carbon to the ultrapure water used for pretreatment is 5:500.

[0160] Step 2: Dipping

[0161] The impregnation method comprises dissolving the sugar in ultrapure water, transferring the solution into a volumetric flask to obtain an impregnation solution, placing the pretreated activated carbon into the impregnation solution and covering it with a layer of plastic wrap, removing the plastic wrap after impregnation for 12 hours, standing for 12 hours, placing the solution in an oven after the liquid basically disappears, drying the solution at 120° C. for 12 hours, and taking the solution out to obtain the impregnation-treated activated carbon;

[0162] The sugar is starch;

[0163] The sugar dissolving temperature is 100°C;

[0164] The mass concentration of the impregnation liquid is 5wt%;

[0165] The mass ratio of the pretreated activated carbon to the impregnation liquid is 1:3.3.

[0166] Step 3: Calcination

[0167] The calcination method comprises placing the impregnated activated carbon into a tubular furnace, introducing an inert gas after evacuation, heating to 600° C., keeping the temperature for 8 hours, and then cooling down. After cooling to room temperature, the activated carbon is taken out and sieved to obtain the sugar-modified activated carbon.

[0168] The inert gas is nitrogen;

[0169] The inert gas flow rate is 300 mL / min;

[0170] The heating rate is 2°C / min;

[0171] The cooling rate is 5°C / min;

[0172] The particle size of the sugar-modified activated carbon obtained by screening is 30 mesh, the average internal pore size is 2.7 nanometers, and the specific surface area is 1721m 2 / g.

[0173] Step 4: Load

[0174] The loading is to use sugar-modified activated carbon as a carrier, load metal palladium salt and metal copper salt by impregnation method, cover with plastic wrap and let stand for 12 hours, remove the plastic wrap and let stand for another 12 hours, put into an oven after the liquid basically disappears, and take out after drying at 120° C. for 12 hours to obtain a catalyst;

[0175] The impregnation method is an equal volume impregnation method;

[0176] The metal palladium salt is palladium chloride;

[0177] The metal copper salt is copper chloride;

[0178] The mass ratio of the loaded metal palladium salt to the sugar-modified activated carbon is 1.7:100;

[0179] The mass ratio of the loaded metal copper salt to the sugar-modified activated carbon is 3.2:100. Comparative Example: Preparation of Sugar-Modified Activated Carbon Support and Catalyst

[0180] The following steps are involved:

[0181] Step 1: Preprocessing

[0182] The pretreatment method comprises placing the activated carbon in ultrapure water, controlling the temperature at 100° C., removing the upper black oil film while heating and stirring, and the process lasts for 24 hours, then filtering out the activated carbon, rinsing it with ultrapure water, placing it in an oven, and drying it at 120° C. for 12 hours to obtain the pretreated activated carbon;

[0183] The particle size of the activated carbon is 30 mesh;

[0184] The mass ratio of the activated carbon to the ultrapure water used for pretreatment is 5:500.

[0185] Step 2: Calcination

[0186] The calcination method comprises placing the pretreated activated carbon in a tubular furnace, introducing an inert gas after evacuation, heating to 600° C., keeping the temperature for 8 hours, and then cooling the pretreated activated carbon to room temperature, taking the pretreated activated carbon out, and screening the pretreated activated carbon to obtain the calcined activated carbon.

[0187] The inert gas is nitrogen;

[0188] The inert gas flow rate is 300 mL / min;

[0189] The heating rate is 2°C / min;

[0190] The cooling rate is 5°C / min;

[0191] The calcined activated carbon obtained by screening has a particle size of 30 mesh, an internal average pore diameter of 2.4 nanometers, and a specific surface area of ​​1737 m 2 / g.

[0192] Step 3: Load

[0193] The loading is to use sugar-modified activated carbon as a carrier, load metal palladium salt and metal copper salt by impregnation method, cover with plastic wrap and let stand for 12 hours, remove the plastic wrap and let stand for another 12 hours, put into an oven after the liquid basically disappears, and take out after drying at 120° C. for 12 hours to obtain a catalyst;

[0194] The impregnation method is an equal volume impregnation method;

[0195] The metal palladium salt is palladium chloride;

[0196] The metal copper salt is copper chloride;

[0197] The mass ratio of the loaded metal palladium salt to the sugar-modified activated carbon is 1.7:100;

[0198] The mass ratio of the loaded metal copper salt to the sugar-modified activated carbon is 3.2:100.

[0199] Application Examples

[0200] The catalysts prepared by the above four embodiments were respectively loaded on a continuous flow fixed bed reactor for activity evaluation. The reaction tube length of the reactor was 30 cm, the inner diameter was 8 mm, and the catalyst loading was 200 mg. The reaction used carbon monoxide and methyl nitrite as the reaction raw gases, nitrogen as the buffer gas, the gas ratio was N2:CO:MN=3:1:2, the reaction temperature was 120°C, the reaction was carried out under normal pressure, and the space velocity was 3600 L / (kg·h). The tail gas was analyzed online in real time by a gas chromatograph. The CO conversion rate comparison of the four catalysts after continuous reaction for 10 hours is as follows: Figure 1 As shown in the figure, the space-time yield WTY (g·kg -1 ·h -1 ) For example Figure 2 shown.

[0201] Carbon monoxide conversion rate X CO The calculation method is as follows:

[0202]

[0203] DMC-based selective S DMC / CO The calculation method is as follows:

[0204]

[0205] The space-time yield WTY is calculated as follows:

[0206]

[0207] [CO] in and [CO] out is the CO concentration at the inlet and outlet; [N2] in and [N2] out are the N2 concentrations at the inlet and outlet, respectively.

[0208] n (DMC) and n (DMO) Denote the molar mass of DMC and DMO, respectively. DMC represents the relative molecular mass of DMC (g / mol), WHSV represents the space velocity (L·kg -1 ·h -1 ), Vm is the molar volume of the gas (22.4 L / mol).

[0209] The carriers obtained in Examples 1-3 and Comparative Examples were subjected to nitrogen adsorption and desorption tests, and the results were as follows:

[0210]

[0211] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. Application of a methyl nitrite carbonylation catalyst in the carbonylation of methyl nitrite to prepare dimethyl carbonate, It is characterized in that Under the action of methyl nitrite carbonylation catalyst, methyl nitrite and CO contact reaction; The preparation method of the catalyst comprises the following steps: Sealingly impregnating a mixed solution containing a carrier, a metal palladium salt and a metal copper salt to obtain the catalyst; The carrier is sugar-modified activated carbon; The metal copper salt is selected from copper chloride; The metal palladium salt is selected from palladium chloride; The method for preparing the sugar-modified activated carbon carrier comprises the following steps: S1, heating a mixture containing activated carbon and water to obtain pretreated activated carbon; S2, adding the pretreated activated carbon into a mixture containing sugars and water for sealed immersion to obtain impregnated activated carbon; S3, calcining the impregnated activated carbon to obtain sugar-modified activated carbon; The sugar is selected from starch; The mass concentration of the sugar in the mixed solution is 0.5 wt% to 10 wt%.

2. The use according to claim 1, It is characterized in that In step S1, the particle size of the activated carbon is 10 mesh to 60 mesh; The internal pore size of the activated carbon is 2 nm to 100 nm; The specific surface area of ​​the activated carbon is 500 m 2 / g ~ 3500 m 2 / g.

3. The use according to claim 1, It is characterized in that In step S1, the mass ratio of the activated carbon to water is 2-20:

500.

4. The use according to claim 1, It is characterized in that In step S1, the heating conditions are as follows: Temperature: 90℃ ~ 120℃; The time is 12 h ~ 48 h.

5. The use according to claim 1, It is characterized in that In step S2, the mass ratio of the pretreated activated carbon to the mixed liquid is 1:1 to 20.

6. The use according to claim 1, It is characterized in that In step S2, the immersion time is 12 h to 48 h.

7. The use according to claim 1, It is characterized in that In step S3, the calcination atmosphere is an inert gas.

8. The use according to claim 7, It is characterized in that In step S3, the heating rate is 2°C / min to 10°C / min; the cooling rate is 2°C / min to 10°C / min.

9. The use according to claim 7, It is characterized in that In step S3, the calcination conditions are as follows: Temperature: 400℃ ~ 900℃; The duration is 6 h ~ 18 h; The inert gas is selected from nitrogen, argon and helium.

10. The use according to claim 7, It is characterized in that In step S3, the inert gas flow rate is 40 mL / min to 400 mL / min.

11. The use according to claim 1, It is characterized in that The mass ratio of the metal palladium salt to the carrier is 0.1-20:

100.

12. The use according to claim 1, It is characterized in that The mass ratio of the metal copper salt to the carrier is 0.2-30:

100.

13. The use according to claim 1, It is characterized in that The immersion time is 6 h ~ 24 h.

14. The use according to claim 1, It is characterized in that The contacting process is carried out in a fixed bed reactor or a fluidized bed reactor.

15. The use according to claim 1, It is characterized in that The molar ratio of CO to methyl nitrite is 1:1~10.

16. The use according to claim 1, It is characterized in that The reaction conditions are as follows: Temperature: 90℃ ~ 150℃; Pressure 0 Mpa ~ 3 Mpa; The buffer gas is nitrogen.

17. The use according to claim 1, It is characterized in that The total space velocity of nitrogen, methyl nitrite and CO is 1000 L / (kg·h) ~ 20000 L / (kg·h).