Low-temperature solder paste for brazing copper and aluminum dissimilar metals with high storage stability and preparation method thereof
By using soldering paste composed of metal solder powder and activator composed of Sn, Zn, Bi, and In in the welding of copper and aluminum dissimilar metals, the problems of poor welding performance and poor storage performance are solved, and the soldering of copper and aluminum dissimilar metals is realized. Efficient welding and stable storage.
Patent Information
- Application Number
- CN202211486157.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-11-24
AI Technical Summary
Existing solder pastes used for welding copper and aluminum dissimilar metals have problems with poor welding performance and poor storage performance. This is mainly because the Zn-Al solder generates a brittle intermetallic compound layer on the copper side, resulting in reduced mechanical properties and dense Al2O3 on the aluminum surface. The film hinders the spreading of the solder, resulting in reduced welding quality. At the same time, the reaction between the metal solder powder and the solder during long-term storage leads to deterioration phenomena such as sanding and agglomeration.
It adopts high-quality solder powder (Sn, Zn, Bi, In) and flux paste (activator, active salt, solvent, surfactant, corrosion inhibitor, antioxidant, solder protectant, thixotropic agent). Storage stability copper aluminum Low-temperature solder paste for brazing dissimilar metals uses organic amine fluoroborate as an active agent to remove the aluminum oxide film at the brazing temperature, improves the wettability of the solder and the base metal, and uses corrosion inhibitors and antioxidants to improve the auxiliary properties. Solder paste stability.
It achieves a good combination of copper and aluminum dissimilar metals, with less residue after welding, excellent welding performance, and the solder paste is not easy to sand and agglomerate, has good storage stability, and can achieve brazing of copper and aluminum at 250 to 280°C. soldering, and improves the storage performance of solder paste.
Smart Images

Figure BDA0003962408400000061 
Figure BDA0003962408400000071 
Figure BDA0003962408400000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal brazing materials, specifically to a copper-aluminum dissimilar metal low-temperature solder paste, and in particular to a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability and a preparation method thereof. Background Art
[0002] With the rapid development of my country's industrial technology, energy saving, environmental protection and lightweight have become the themes of contemporary development. Copper-aluminum dissimilar metal connection structures have been widely used in electrical engineering, refrigeration industry and new energy vehicles due to their advantages of light weight, excellent comprehensive performance and relieving the shortage of copper resources. Relevant literature shows that the application of copper-aluminum welding joints will account for 5.8% of all dissimilar metal material joints in the 21st century.
[0003] At present, the welding processes used for copper and aluminum dissimilar metals mainly include pressure welding, friction welding, diffusion welding, brazing, etc. Compared with the previous welding processes that require professional welding equipment and have strict requirements on operators, the brazing process has the advantages of low heating temperature, small workpiece deformation, convenient process operation, etc., and has a wider application field.
[0004] Solder paste is a new type of welding material that came into being with the development of brazing technology. Solder paste is a mixture of metal solder powder and flux paste. The flux paste is mainly composed of activators, active salts, solvents, surfactants and other additives.
[0005] In recent years, more and more types of solder paste have entered the market due to industrial demand. However, there are currently few solder pastes used for copper-aluminum dissimilar metal welding, and there are still problems such as poor welding performance and poor storage performance. There are two main reasons for its poor welding performance: (1) The solder currently used for copper-aluminum joints is mainly Zn-Al solder, which is easy to form a thick CuAl brittle intermetallic compound layer on the copper side of the brazed joint, which will reduce the mechanical properties of the brazed joint; if it comes into contact with a specific corrosive medium, it will also cause intergranular corrosion in the weld. (2) The dense Al2O3 film on the aluminum surface will hinder the spread and wetting of the solder on the base material, thereby reducing the brazing quality of the aluminum side. The main reason for its poor storage performance is that in order to ensure the welding strength of the copper-aluminum joint, a highly corrosive flux is generally used to remove the oxide film on the aluminum side. When the solder paste is stored for a long time, the metal solder powder reacts with the flux and is corroded, resulting in deterioration of the solder paste such as sanding and agglomeration, which reduces the use effect. Summary of the invention
[0006] According to the above technical problems, a low-temperature solder paste with high stability for brazing copper and aluminum dissimilar metals is provided. The solder paste can effectively achieve good bonding between the brazing material and the copper and aluminum dissimilar metals, has less residue after welding, and has good storage stability.
[0007] The technical means adopted by the present invention are as follows:
[0008] A low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability is provided. The solder paste is composed of the following components in percentage by mass: 82% to 87% of metal solder powder and 13% to 18% of flux paste.
[0009] Preferably, the metal solder powder consists of the following components in percentage by mass: 5% to 13% Zn, 0.5% to 3% Bi, 0.1% to 2% In and the balance Sn.
[0010] Preferably, the soldering paste is composed of the following components in percentage by mass: 50% to 65% of an active agent, 3% to 5% of an active salt, 10% to 20% of a solvent, 0.5% to 3% of a surfactant, 0.1% to 2% of a corrosion inhibitor, 0.1% to 2% of an antioxidant, 0.1% to 1% of a solder protectant, and 5% to 10% of a thixotropic agent.
[0011] Preferably, the active agent is an organic amine fluoroborate prepared from an organic amine and fluoroboric acid, and the specific preparation method is as follows: both fluoroboric acid and organic amine are diluted with anhydrous ethanol to 40-50wt%. The diluted fluoroboric acid is slowly added to the diluted organic amine through a funnel to neutralize to a pH of 6.5-7.5. The neutralized solution is placed in an electromagnetic stirring furnace and heated to 90-100° C. to evaporate water, and heating is stopped until there are no bubbles in the solution and white mist is generated. After the solution is slightly cooled, it is transferred to a closed container and cooled to room temperature, thereby obtaining an organic amine fluoroborate.
[0012] Preferably, the organic amine is at least one of ethanolamine, diethanolamine, triethanolamine, hydroxyethylethylenediamine, hydroxypropylethylenediamine and triisopropanolamine.
[0013] Preferably, the active salt is at least one of zinc fluoride, stannous fluoride, ammonium fluoride, lithium fluoride, aluminum fluoride, ammonium bifluoride, zinc fluoroborate, stannous fluoroborate, and ammonium fluoroborate.
[0014] Preferably, the solvent is at least one of ethanol, ethylene glycol, ethylene glycol monobutyl ether, diethylene glycol, terpineol, glycerol, isopropanol, n-butanol, tetrahydrocannabinol, 1,2-propylene glycol, 1,3-propylene glycol, and N-methylpyrrolidone.
[0015] Preferably, the surfactant is at least one of OP-9, OP-10, OP-13, OP-15, oleic acid amide, and acetylene glycol.
[0016] Preferably, the corrosion inhibitor is at least one of BTA and piperazine.
[0017] Preferably, the antioxidant is at least one of hydroquinone, o-tert-butylhydroquinone and ascorbic acid.
[0018] Preferably, the solder protective agent is polyvinyl pyrrolidone.
[0019] Preferably, the thixotropic agent is at least one of hydrogenated castor oil, ethylene bisstearamide, modified rosin, stearic acid, organic bentonite, polyamide wax, and ethyl cellulose.
[0020] The present invention also discloses a method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability, comprising:
[0021] (1) According to the formula ratio, the active agent, active salt, solvent, surfactant, corrosion inhibitor, and antioxidant are put into the corrosion-resistant reactor and stirred until they are completely dissolved into a clear solution. After the solution is heated to 65-80° C., the solder protective agent and thixotropic agent are added thereto and stirred at a high speed and uniformly. After cooling, the solder paste can be obtained;
[0022] (2) Weighing metal solder powder and solder paste according to the formula ratio, and putting them into a blender to mix them evenly, thereby obtaining a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability.
[0023] In the solder paste of the present invention, the metal solder powder component is composed of Sn, Zn, Bi and In, among which Zn and Al have strong mutual diffusion ability; Bi can reduce the melting point of the solder, slightly improve the solder wettability and improve the solder strength; In can reduce the solder melting point and improve the solder wettability; Bi and In can enhance the corrosion resistance of the solder.
[0024] In the solder paste of the present invention, the solder paste is compounded by an activator, an active salt, a solvent, a surfactant, a corrosion inhibitor, an antioxidant and the like. As an activator, an organic amine fluoroborate can decompose hydrogen fluoride and other substances that can effectively remove the oxide film on the surface of aluminum at the soldering temperature, thereby enhancing the wetting of the solder and the aluminum base material. The active salt can react with the metal substrate at the soldering temperature together with the activator, thereby enhancing the removal of the oxide film on the surface of aluminum and further improving the activity of the solder paste. The surfactant can improve the wetting of the solder and the base material, which is beneficial to the metallurgical bonding of the solder and the metal base material. The corrosion inhibitor, the antioxidant and the solder protective agent can improve the storage performance of the solder paste from two aspects, namely, improving the stability of the solder paste and reducing the direct contact between the metal solder powder and the solder paste.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] (1) The present invention uses organic amine fluoroborate as an active agent, which is stable at room temperature and has low corrosiveness to alloy solder powder. At the brazing temperature, it can quickly release substances that remove aluminum oxide film, improve the wettability of the brazing material and the base material, and improve the storage performance of the solder paste while ensuring the brazing quality.
[0027] (2) The solder paste of the present invention is not easy to become sandy or lumpy, and has stable activity.
[0028] (3) The solder paste of the present invention can realize the brazing of dissimilar metals of copper and aluminum at 250-280° C. and has a good welding effect.
[0029] Based on the above reasons, the present invention can be widely promoted in the fields of metal brazing materials and the like. DETAILED DESCRIPTION
[0030] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] A low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability is provided. The solder paste is composed of the following components in percentage by mass: 82% to 87% of metal solder powder and 13% to 18% of flux paste.
[0032] Preferably, the metal solder powder consists of the following components in percentage by mass: 5% to 13% Zn, 0.5% to 3% Bi, 0.1% to 2% In and the balance Sn.
[0033] Preferably, the soldering paste is composed of the following components in percentage by mass: 50% to 65% of an active agent, 3% to 5% of an active salt, 10% to 20% of a solvent, 0.5% to 3% of a surfactant, 0.1% to 2% of a corrosion inhibitor, 0.1% to 2% of an antioxidant, 0.1% to 1% of a solder protectant, and 5% to 10% of a thixotropic agent.
[0034] Preferably, the active agent is an organic amine fluoroborate prepared from an organic amine and fluoroboric acid, and the specific preparation method is as follows: both fluoroboric acid and organic amine are diluted with anhydrous ethanol to 40-50wt%. The diluted fluoroboric acid is slowly added to the diluted organic amine through a funnel to neutralize to a pH of 6.5-7.5. The neutralized solution is placed in an electromagnetic stirring furnace and heated to 90-100° C. to evaporate water, and heating is stopped until there are no bubbles in the solution and white mist is generated. After the solution is slightly cooled, it is transferred to a closed container and cooled to room temperature, thereby obtaining an organic amine fluoroborate.
[0035] Preferably, the organic amine is at least one of ethanolamine, diethanolamine, triethanolamine, hydroxyethylethylenediamine, hydroxypropylethylenediamine and triisopropanolamine.
[0036] Preferably, the active salt is at least one of zinc fluoride, stannous fluoride, ammonium fluoride, lithium fluoride, aluminum fluoride, ammonium bifluoride, zinc fluoroborate, stannous fluoroborate, and ammonium fluoroborate.
[0037] Preferably, the solvent is at least one of ethanol, ethylene glycol, ethylene glycol monobutyl ether, diethylene glycol, terpineol, glycerol, isopropanol, n-butanol, tetrahydrocannabinol, 1,2-propylene glycol, 1,3-propylene glycol, and N-methylpyrrolidone.
[0038] Preferably, the surfactant is at least one of OP-9, OP-10, OP-13, OP-15, oleic acid amide, and acetylene glycol.
[0039] Preferably, the corrosion inhibitor is at least one of BTA and piperazine.
[0040] Preferably, the antioxidant is at least one of hydroquinone, o-tert-butylhydroquinone and ascorbic acid.
[0041] Preferably, the solder protective agent is polyvinyl pyrrolidone.
[0042] Preferably, the thixotropic agent is at least one of hydrogenated castor oil, ethylene bisstearamide, modified rosin, stearic acid, organic bentonite, polyamide wax, and ethyl cellulose.
[0043] A method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability, comprising:
[0044] (1) According to the formula ratio, the active agent, active salt, solvent, surfactant, corrosion inhibitor, and antioxidant are put into the corrosion-resistant reactor and stirred until they are completely dissolved into a clear solution. After the solution is heated to 65-80° C., the solder protective agent and thixotropic agent are added thereto and stirred at a high speed and uniformly. After cooling, the solder paste can be obtained;
[0045] (2) Weighing metal solder powder and solder paste according to the formula ratio, and putting them into a blender to mix them evenly, thereby obtaining a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability.
[0046] The present specific implementation is further described below with reference to specific examples.
[0047] Example 1
[0048] A low-temperature solder paste for brazing copper and aluminum dissimilar metals with high storage stability. The components in the solder paste are as follows, calculated by mass percentage:
[0049]
[0050] The specific preparation method is as follows:
[0051] (1) Fluoboric acid and triethanolamine are diluted to 40wt% with anhydrous ethanol. The diluted fluoboric acid is slowly added to the diluted triethanolamine through a funnel for neutralization until the pH of the acid-amine neutralized solution is 7.0. The neutralized solution is placed in an electromagnetic stirring furnace and heated to 90°C for water evaporation. The heating is stopped until there are no bubbles in the solution and white mist is generated. The solution is slightly cooled and transferred to a closed container and cooled to room temperature, thereby obtaining triethanolamine fluoborate.
[0052] (2) Weigh 9.6 g of triethanolamine fluoroborate, 0.2 g of zinc fluoroborate, 0.2 g of stannous fluoroborate, 0.4 g of ethanol, 0.4 g of ethylene glycol, 1.2 g of diethylene glycol, 0.2 g of OP-10, 0.1 g of BTA, and 0.01 g of hydroquinone, and put them into a corrosion-resistant reactor and stir them to completely dissolve them into a clear solution; then heat the above solution to 70°C, add 0.49 g of polyvinyl pyrrolidone and 0.5 g of hydrogenated castor oil, and stir them at high speed. After cooling, a soldering flux paste can be obtained; finally, 86.7 g of Sn9Zn2.5Bi1.5In alloy solder powder and the prepared soldering flux paste are fully and evenly mixed using a mixer to obtain 100 g of low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability.
[0053] Example 2
[0054] A low-temperature solder paste for brazing copper and aluminum dissimilar metals with high storage stability. The components in the solder paste are as follows, calculated by mass percentage:
[0055]
[0056] The specific preparation method is as follows:
[0057] (1) Fluoroboric acid, diethanolamine and triethanolamine are diluted to 40wt% with anhydrous ethanol. The diluted fluoboric acid is slowly added into a mixed organic amine dilution solution with a mass percentage of 50% of diethanolamine and triethanolamine through a funnel for neutralization titration until the pH of the acid-amine neutralization solution reaches 7.0. The neutralized solution is placed in an electromagnetic stirring furnace and heated to 90°C for water evaporation. The heating is stopped until there are no bubbles in the solution and white mist is generated. The solution is cooled slightly and transferred to a closed container. It is cooled to room temperature to obtain an organic amine fluoroborate.
[0058] (2) Weigh 8.8 g of organic amine fluoroborate, 0.2 g of zinc fluoride, 0.2 g of stannous fluoroborate, 0.3 g of tetrahydrocannabinol, 0.4 g of ethylene glycol, 1.3 g of diethylene glycol, 0.2 g of OP-10, 0.1 g of BTA, and 0.01 g of o-tert-butylhydroquinone, and put them into a corrosion-resistant reactor and stir them to completely dissolve them into a clear solution; then heat the above solution to 80°C, add 0.49 g of polyvinyl pyrrolidone, 0.35 g of hydrogenated castor oil, and 0.15 g of ethylene bisstearamide, and stir them at high speed and evenly, and obtain solder paste after cooling; finally, use a mixer to fully and evenly mix 87.5 g of Sn9Zn2.5Bi1.5In alloy solder powder and the prepared solder paste to obtain 100 g of low-temperature solder paste with high storage stability for copper-aluminum dissimilar metal brazing.
[0059] Example 3
[0060] A low-temperature solder paste for brazing copper and aluminum dissimilar metals with high storage stability. The components in the solder paste are as follows, calculated by mass percentage:
[0061]
[0062]
[0063] The specific preparation method is as follows:
[0064] (1) Fluoroboric acid, diethanolamine and hydroxyethylethylenediamine are diluted with anhydrous ethanol to a mass fraction of 40%. The diluted fluoroboric acid is slowly added into a mixed organic amine diluted solution with a mass percentage of 50% of diethanolamine and hydroxyethylethylenediamine through a funnel for neutralization until the pH of the acid-amine neutralized solution is 7.0. The titrated solution is placed in an electromagnetic stirring furnace and heated to 95° C. to evaporate water. The heating is stopped until there are no bubbles in the solution and white mist is generated. After the solution is slightly cooled, it is transferred to a closed container and cooled to room temperature to obtain an organic amine fluoroborate.
[0065] (2) Weigh 10.1 g of organic amine fluoroborate, 0.2 g of zinc fluoroborate, 0.4 g of stannous fluoride, 0.1 g of ammonium bifluoride, 0.2 g of ethanol, 0.6 g of ethylene glycol monobutyl ether, 1.4 g of diethylene glycol, 0.2 g of OP-13, 0.1 g of BTA, and 0.01 g of hydroquinone, and put them into a corrosion-resistant reactor and stir them to completely dissolve them into a clear solution; then heat the above solution to 80° C., add 0.39 g of polyvinyl pyrrolidone, 0.4 g of hydrogenated castor oil, and 0.2 g of modified rosin thereto, and stir them at high speed and uniformly, and after cooling, a soldering flux paste can be obtained; finally, 85.7 g of Sn9Zn2.5Bi1.5In alloy solder powder and the prepared soldering flux paste are fully and uniformly mixed using a mixer to obtain 100 g of low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability.
[0066] The brazing property, post-welding residual rate and storage time of the low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability prepared in Examples 1 to 3 of the present invention were tested.
[0067] The specific test methods for brazing performance and post-weld residual rate in the embodiments of the present invention are as follows:
[0068] Weigh the solder paste with a mass of m1. The flux ratio of the solder paste in the embodiment is ρ. The solder paste is respectively coated on a copper substrate and a 1060 aluminum substrate with a mass of m2, a thickness of 1 mm, a length and a width of 20 mm, and then the test solder piece is placed on a constant temperature heating table at a temperature of 100°C for preheating for 15 seconds, and then placed in a reflow furnace at a temperature of 260°C. After the solder spreads and forms a solder joint, keep it for 30 seconds before removing the test solder piece, and then directly weigh the test solder piece to obtain its mass m3. The post-welding residual rate f is calculated according to the following formula: f=[m3-m2-(1-ρ)m1] / (ρm1).
[0069] The specific test method for storage time in the embodiment of the present invention is as follows:
[0070] The prepared solder paste is sealed and stored in a container at room temperature, and the deterioration of the solder paste is determined by the fact that the solder paste remains basically unchanged, does not form a crust, and does not become sandy.
[0071] The results are shown in Table 1:
[0072] Table 1 Test results of solderability, post-soldering residual rate and storage time of solder paste
[0073]
[0074] It can be seen from Table 1 that the low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability of the present invention not only has excellent brazing properties, but also has a lower post-welding residue rate on the aluminum substrate than the solder paste invented by Patent Publication No. CN104625483A; the low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability of the present invention has a sealed storage time of more than 30 days at room temperature, and has good storage stability.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability, characterized in that: include: (1) Prepare solder paste. Take materials according to the formula ratio, put the activator, active salt, solvent, surfactant, corrosion inhibitor, and antioxidant into the corrosion-resistant reactor and stir until they are completely dissolved into a clear solution. After heating the solution to 65-80°C, add the solder protective agent and thixotropic agent and stir. After cooling, the solder paste can be obtained. (2) Weighing metal solder powder and solder paste according to the formula ratio, and putting them into a blender to mix them evenly, thereby obtaining a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability; The solder paste is composed of the following components in percentage by mass: 82% to 87% metal solder powder and 13% to 18% flux paste; The metal welding powder is composed of the following components in percentage by mass: 5% to 13% Zn, 0.5% to 3% Bi, 0.1% to 2% In and the balance Sn; The soldering paste is composed of the following components in percentage by mass: 50% to 65% of an active agent, 3% to 5% of an active salt, 10% to 20% of a solvent, 0.5% to 3% of a surfactant, 0.1% to 2% of a corrosion inhibitor, 0.1% to 2% of an antioxidant, 0.1% to 1% of a solder protective agent, and 5% to 10% of a thixotropic agent; The active agent is an organic amine fluoroborate; The active salt is at least one of ammonium fluoride, lithium fluoride, aluminum fluoride, ammonium bifluoride, and ammonium fluoroborate.
2. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 1, characterized in that: The organic amine fluoroborate is prepared from an organic amine and fluoroboric acid, and the preparation method is as follows: the fluoroboric acid and the organic amine are both diluted with anhydrous ethanol to 40-50wt%, the diluted fluoroboric acid is neutralized to a pH of 6.5-7.5 by adding the diluted organic amine, the neutralized solution is placed in an electromagnetic stirring furnace and heated to 90-100° C. to evaporate water, and the heating is stopped until there are no bubbles in the solution and white mist is generated, and the solution is slightly cooled and transferred to a closed container to be cooled to room temperature to obtain the organic amine fluoroborate.
3. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 2, characterized in that: The organic amine is at least one of ethanolamine, diethanolamine, triethanolamine, hydroxyethylethylenediamine, hydroxypropylethylenediamine and triisopropanolamine.
4. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 1, characterized in that: The solvent is at least one of ethanol, ethylene glycol, ethylene glycol monobutyl ether, diethylene glycol, terpineol, glycerol, isopropanol, n-butanol, tetrahydrocannabinol, 1,2-propylene glycol, 1,3-propylene glycol, and N-methylpyrrolidone.
5. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 1, characterized in that: The surfactant is at least one of OP-9, OP-10, OP-13, OP-15, oleic acid amide and acetylene glycol.
6. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 1, characterized in that: The corrosion inhibitor is at least one of BTA and piperazine.
7. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 1, characterized in that: The antioxidant is at least one of hydroquinone, o-tert-butylhydroquinone and ascorbic acid.
8. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 1, characterized in that: The solder protective agent is polyvinyl pyrrolidone.
9. The method for preparing a low-temperature solder paste for copper-aluminum dissimilar metal brazing with high storage stability according to claim 1, characterized in that: The thixotropic agent is at least one of hydrogenated castor oil, ethylene bisstearamide, modified rosin, stearic acid, organic bentonite, polyamide wax, and ethyl cellulose.
Citation Information
Patent Citations
Low-residual and low-corrosivity aluminum soft soldering tin paste and manufacturing method thereof
CN104625483A
Cleaning-free solid-state scaling powder for aluminum low-temperature soldering and preparing method
CN104607826A
Low-residue high-storage stability low-temperature tin paste for aluminium and preparation method thereof
CN107009043A
Novel Sn-Zn-Bi-In series lead-free soldering paste and preparation method thereof
CN114749826A