Aqueous ink, ink cartridge, and inkjet recording method

By using titanium oxide particles coated with alumina and silica and a combination of poly(acrylic acid) and potassium ions in aqueous ink, the problem of sedimentation of titanium oxide particles is solved, and the settlement restorability and fixation restorability of pigments are improved, so as to achieve Stable image performance on transparent recording medium is achieved.

CN115926535BActive Publication Date: 2024-11-12CANON KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211201703.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-09-13
Filing Date
2022-09-29
Publication Date
2024-11-12
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

When the existing aqueous ink is used on a transparent recording medium, the titanium oxide particles tend to settle, resulting in insufficient restoration and fixation restoration of the pigment, which affects the effect of inkjet recording.

Method used

By using titanium oxide particles coated with alumina and silica in aqueous ink and adding poly(acrylic acid) and potassium ions, their mass ratio is controlled to improve the surface charge and electrostatic repulsion of the titanium oxide particles and prevent aggregation , thereby improving the restoration of the pigment and the restoration of the ink.

Benefits of technology

The pigment settlement recovery and fixation recovery of the aqueous ink are significantly improved, ensuring stability and image performance on transparent recording media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115926535B_ABST
    Figure CN115926535B_ABST
Patent Text Reader

Abstract

The present invention relates to an aqueous ink, an ink cartridge and an inkjet recording method. The aqueous ink comprises titanium oxide particles, poly(acrylic acid) and potassium ions, wherein the titanium oxide particles comprise titanium oxide at least a portion of the surface of which is coated with aluminum oxide and silicon dioxide, and the content of poly(acrylic acid) is 0.05 times or more and 0.40 times or less of the content of aluminum oxide in terms of mass ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an aqueous ink, an ink cartridge, and an inkjet recording method. Background Art

[0002] In recent years, inkjet recording apparatuses have been widely used to output advertisements and exhibits using recording media such as paper and resin films. For example, in order to express a vivid color image even on a transparent recording medium, white ink is used in combination with black ink and inks of basic colors (hereinafter, they are sometimes collectively referred to as "color inks"). Specifically, a recording method is adopted in which white ink is applied in advance to a portion of a transparent recording medium including an area where an image is to be recorded for primer treatment, and color inks are applied thereon, or each ink is applied in reverse order (so-called back printing).

[0003] Titanium oxide is widely used as a coloring material for white ink because of its low cost and excellent properties required for white ink such as whiteness and hiding power. In order to stably disperse titanium oxide in aqueous ink, a dispersant is required. However, titanium oxide, as a metal oxide, has a higher specific gravity than coloring materials used for inks of other colors. Therefore, there is a disadvantage that sedimentation cannot be fully suppressed even when a dispersant is used. In this case, emphasis is placed on sedimentation recovery property that titanium oxide is dispersed again even if it is once precipitated, and sticking recovery property that dissolves the settling formed by drying the pigment.

[0004] To date, methods for obtaining the sedimentation recovery of pigments and the fixation recovery of inks through the components of inks have been studied. For example, PCT Japanese Translation Patent Publication No. 2017-521348 discloses a method for producing a dry titanium dioxide product in which a portion of the silane coupling agent is covalently bonded to the surface of the titanium dioxide particles by treating the surface of titanium dioxide particles with silicon dioxide, then further treating the surface of the titanium dioxide particles with a silane coupling agent and drying the obtained titanium dioxide particles. PCT Japanese Translation Patent Publication No. 2021-512077 discloses an ink composition comprising titanium dioxide, a (meth) acrylic acid homopolymer or a salt thereof, and a rheology modifier that has been surface-treated with silicon dioxide and aluminum oxide. Japanese Patent Publication No. 2019-44069 discloses an ink composition comprising a powder having a first charge, an ionic polymer having a second charge different from the first charge, and a pigment having a multivalent ion having a first charge. Summary of the invention

[0005] The present inventors have studied the recovery from sedimentation of pigments and the recovery from fixation of inks in aqueous inks prepared using dried titanium dioxide disclosed in PCT Japanese Translation Patent Publication No. 2017-521348 and aqueous inks prepared using ink compositions disclosed in PCT Japanese Translation Patent Publication No. 2021-512077 and Japanese Patent Publication No. 2019-44069. As a result, it was found that the recovery from sedimentation of pigments and the recovery from fixation of inks were insufficient for the current situation where good performance is required even under the assumption of more severe environmental changes, and therefore, there is room for performance improvement so that users can use the ink smoothly.

[0006] Therefore, the present disclosure provides an aqueous ink containing titanium oxide that is used for inkjet recording and has excellent sedimentation recovery of a pigment and fixation recovery of an ink, an ink cartridge that accommodates the aqueous ink, and an inkjet recording method.

[0007] One aspect of the present disclosure is to provide an aqueous ink for inkjet recording, the aqueous ink comprising titanium oxide particles, poly(acrylic acid) and potassium ions, wherein the titanium oxide particles comprise titanium oxide at least a portion of the surface of which is coated with aluminum oxide and silicon dioxide, and the amount of poly(acrylic acid) contained in the aqueous ink is not less than 0.05 times and not more than 0.40 times the amount of aluminum oxide contained in the titanium oxide particles in terms of mass ratio.

[0008] Further features of the present invention will become apparent from the following description of exemplary embodiments with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 is a cross-sectional view schematically showing an exemplary embodiment of the ink cartridge of the present invention.

[0010] Figure 2A is a perspective view schematically showing an example of a main part of an inkjet recording apparatus used in the inkjet recording method according to the present invention, and Figure 2B It is a perspective view schematically showing an example of a head cartridge used in the inkjet recording method according to the present invention. DETAILED DESCRIPTION

[0011] The present invention will be described in more detail below with reference to preferred exemplary embodiments. In an embodiment of the present invention, when the compound is a salt, the salt is present in the ink in a state of being dissociated into ions, but for convenience it is expressed as "ink contains salt". Titanium oxide and titanium oxide particles may be referred to as "pigment". Aqueous ink for inkjet recording may be referred to as "ink". Unless otherwise specified, the physical property values ​​are all values ​​at room temperature (25°C).

[0012] Inorganic oxides such as titanium oxide react with water molecules contained in the aqueous medium in aqueous ink to form hydroxyl groups (hereinafter sometimes referred to as "surface hydroxyl groups") on the surface of the inorganic oxide. For this reason, in aqueous inks for inkjet recording, in order to further improve the storage stability of the ink while utilizing the formed surface hydroxyl groups, the inorganic oxide is usually used in a state where the inorganic oxide is surface-treated with different inorganic oxides such as aluminum oxide or silicon dioxide. The surface hydroxyl groups of titanium oxide particles have properties inherent to the inorganic oxide corresponding to the inorganic compound used for surface treatment, and the isoelectric point, which is an indicator of acid strength, varies depending on the type of inorganic compound. Therefore, although titanium oxide itself is an inorganic oxide, the surface of the titanium oxide particles exhibits the properties of the inorganic oxide corresponding to the inorganic compound used for surface treatment, and the surface charge of the titanium oxide particles strongly depends on the pH of the aqueous medium, the type of surface treatment agent, and the amount of surface treatment agent used.

[0013] The inventors have studied how to improve the sedimentation recovery of the pigment and the fixation recovery of the ink by using the components contained in the ink. The inventors first studied the factors that deteriorate the sedimentation recovery of the pigment and the fixation recovery of the ink. The distance between the titanium oxide particles is maintained by the dispersant in the ink; however, when the distance between the titanium oxide particles becomes closer, the titanium oxide particles aggregate and these properties deteriorate. It was found that the aggregation is easily promoted by the surface charge of the titanium oxide particles. Under alkaline conditions, which are the usual liquid properties of aqueous inks for inkjet recording, aluminum oxide and silicon dioxide on the surface of the titanium oxide particles form surface hydroxyls. In addition, the surface hydroxyls derived from aluminum oxide are positively charged, while the surface hydroxyls derived from silicon dioxide are negatively charged. Therefore, when the distance between the titanium dioxide particles is reduced, it is believed that the electrostatic effect plays a role in promoting the aggregation of the titanium oxide particles.

[0014] The present inventors have studied the addition of materials to ink to improve the sedimentation recovery performance of the pigment and the fixation recovery of the ink while suppressing the influence of the surface charge of the titanium oxide particles. As a result, the present inventors have found that by using an aqueous ink containing titanium oxide particles subjected to a specific surface treatment and poly(acrylic acid) in a specific mass ratio based on the titanium oxide particles and potassium ions, the sedimentation recovery performance of the pigment and the fixation recovery of the ink can be improved.

[0015] That is, the ink according to the embodiment of the present disclosure has the following characteristics: titanium oxide particles containing titanium oxide whose surface is at least partially coated with aluminum oxide and silicon dioxide are used. The ink further contains poly(acrylic acid) and potassium ions. The content of polyacrylic acid is 0.05 times or more and 0.40 times or less of the amount of aluminum oxide coating the titanium oxide particles in terms of mass ratio. The inventors speculate that the mechanism by which the above-mentioned composition improves the sedimentation recovery of the pigment and the fixation recovery of the ink is as follows.

[0016] The ink contains poly(acrylic acid) and potassium ions. Poly(acrylic acid) has a molecular structure in which multiple carboxylic acid groups are bound to hydrocarbon chains. Potassium ions have a large ionic radius and ionization tendency in alkali metal ions. The presence of potassium ions in the ink promotes the ionization of the carboxylic acid groups of poly(acrylic acid) and the surface hydroxyl groups of titanium oxide particles. The ionized carboxylic acid group is negatively charged and adsorbed to the positively charged surface hydroxyl groups derived from aluminum oxide by electrostatic action. Therefore, the positive charge of the titanium oxide particles can be eliminated to suppress the aggregation of the titanium oxide particles. Therefore, when the dried ink is redissolved, the carboxylic acid group or hydroxyl group can be easily ionized and dissolved, thereby providing excellent ink fixation recovery. When potassium ions are not present in the ink, the ionization of the carboxylic acid group, etc. is not promoted, and electrostatic interaction with the surface hydroxyl groups derived from aluminum oxide of the titanium oxide particles does not occur. In addition, the ionization of the hydroxyl groups derived from silicon dioxide on the titanium oxide surface is not promoted, and the electrostatic repulsion between the titanium oxide particles is not fully obtained. Therefore, it is difficult to redissolve the dried ink, and the fixation recovery of the ink cannot be obtained.

[0017] In addition to the surface hydroxyl groups derived from silicon dioxide, due to the carboxylic acid groups of poly (acrylic acid), the titanium oxide particles adsorbed with poly (acrylic acid) are negatively charged. This further enhances the electrostatic repulsion between the titanium oxide particles, thereby enabling stable dispersion. In addition, even if the distance between the titanium oxide particles is reduced, the spacer function of poly (acrylic acid) can also suppress the particles from approaching more than a certain distance. This can suppress the strong aggregation of titanium oxide particles, thereby improving the sedimentation recovery of the pigment and the fixation recovery of the ink. When the titanium oxide particles are not coated with aluminum oxide, poly (acrylic acid) has no adsorption site. Therefore, the above-mentioned effect that should be obtained by the adsorption of poly (acrylic acid) does not occur, and the sedimentation recovery of the pigment cannot be obtained. In the case where the titanium oxide particles are only coated with aluminum oxide, although poly (acrylic acid) is adsorbed, there is no surface hydroxyl group derived from silicon dioxide. Therefore, the electrostatic repulsion between the titanium oxide particles is not fully obtained, and the sedimentation recovery of the pigment cannot be provided.

[0018] The poly(acrylic acid) content of the ink is more than 0.05 times and less than 0.40 times the content of aluminum oxide in terms of mass ratio. This aluminum oxide coats titanium oxide. When the mass ratio is within the above range, poly(acrylic acid) can be adsorbed to titanium oxide particles, thereby improving the sedimentation recovery of the pigment and the fixation recovery of the ink. When the mass ratio is less than 0.05 times, the adsorption amount of poly(acrylic acid) is insufficient, and the positive charge on the surface of the titanium oxide particles cannot be fully offset, thereby failing to obtain the sedimentation recovery of the pigment or the fixation recovery of the ink. When the mass ratio is greater than 0.40 times, the amount of poly(acrylic acid) present exceeds the amount that can be adsorbed on the titanium oxide particles, and the amount of free poly(acrylic acid) in the ink increases. Free poly(acrylic acid) contributes to the increase in the amount of ions in the ink, destabilizing the dispersion state of the titanium oxide particles, thereby failing to obtain the sedimentation recovery of the pigment.

[0019] In an embodiment of the present disclosure, poly(acrylic acid) can eliminate the positive charge of the surface hydroxyl group derived from aluminum oxide by a composition in which poly(acrylic acid) is adsorbed on titanium oxide particles containing titanium oxide whose surface is coated with aluminum oxide and silicon dioxide. Therefore, even if the distance between the titanium oxide particles is reduced due to sedimentation or drying, the aggregation caused by electrostatic action can also be suppressed, and the spacer function of poly(acrylic acid) prevents the titanium oxide particles from approaching a certain distance, thereby suppressing the aggregation of the titanium oxide particles. In addition, the presence of potassium ions in the ink can promote the ionization of the carboxylic acid groups of the poly(acrylic acid) and the surface hydroxyl groups of the titanium oxide particles. That is, the amount of free poly(acrylic acid) can be reduced. As a result, the instability of the dispersed state of the titanium oxide particles is suppressed, thereby suppressing the aggregation of the titanium oxide particles. In an embodiment of the present disclosure, by satisfying these compositions, the sedimentation recovery of the pigment and the fixation recovery of the ink can be improved.

[0020] Water-based ink

[0021] The ink according to the embodiment of the present disclosure is an aqueous ink for inkjet recording, which contains titanium oxide particles coated with a specific inorganic oxide, poly (acrylic acid) and potassium ions. The ink can be a white ink because titanium oxide is a white pigment. The components contained in the ink of the embodiment of the present disclosure, the physical properties of the ink, etc. are described in detail below.

[0022] Coloring Materials

[0023] The ink contains titanium oxide particles as a coloring material (pigment), and the titanium oxide particles contain titanium oxide surface-treated with a specific inorganic oxide. That is, the ink contains titanium oxide particles containing titanium oxide whose surface is coated with a specific inorganic oxide. The content of titanium oxide particles in the ink is based on the total mass of the ink, preferably 0.10 mass % or more and 20.00 mass % or less. The content of titanium oxide particles in the ink is based on the total mass of the ink, more preferably 1.00 mass % or more and 20.00 mass % or less. The content of titanium oxide particles in the ink is based on the total mass of the ink, particularly preferably 1.00 mass % or more and 15.00 mass % or less.

[0024] Titanium oxide is a white pigment and has three crystal forms: rutile, anatase and brookite. Among them, rutile titanium oxide can be used. Industrial production methods of titanium dioxide include sulfuric acid method and chlorine method. Titanium oxide used in the embodiment of the present invention can be produced by any production method.

[0025] The 50% cumulative particle size based on volume (hereinafter, also referred to as "average particle size") of the titanium oxide particles is preferably 200 nm or more and 500 nm or less. In particular, the 50% cumulative particle size based on volume of the titanium oxide particles is more preferably 200 nm or more and 400 nm or less. The 50% cumulative particle size based on volume of the titanium oxide particles (D 50 ) is the particle size at which the cumulative volume is 50% when integrated from the smaller particle size side based on the total volume of the measured particles in the cumulative particle size curve. D of titanium oxide 50 It can be measured, for example, under the conditions of SetZero: 30 seconds, number of measurements: 3 times, measurement time: 180 seconds, shape: non-spherical, refractive index: 2.60. As a particle size distribution measuring device, a particle size analyzer based on a dynamic light scattering method can be used. Of course, the measurement conditions and the like are not limited to those described above.

[0026] Titanium oxide surface-treated with aluminum oxide and silicon dioxide is used. The surface treatment should suppress photocatalytic activity and improve dispersibility. In this specification, "aluminum oxide" is a general term for aluminum oxides such as aluminum oxide (aluminum oxide). In this specification, "silicon dioxide" is a general term for silicon dioxide and substances composed of silicon dioxide. Most of the aluminum oxide and silicon dioxide coated titanium oxide exist in the form of aluminum oxide and silicon dioxide.

[0027] The proportion of titanium oxide in the titanium oxide particles may be 90.00% by mass or more based on the total mass of the titanium oxide particles. The proportion of titanium oxide in the titanium oxide particles may be 98.50% by mass or less based on the total mass of the titanium oxide particles. The proportion of aluminum oxide in the titanium oxide particles is 0.50 times or more and 1.00 times or less of the proportion of silicon dioxide in terms of mass ratio. A mass ratio of less than 0.50 times results in too small a proportion of aluminum oxide; therefore, poly(acrylic acid) cannot be sufficiently adsorbed in the ink, and the dispersion stability and the like that should be obtained by the adsorption of poly(acrylic acid) cannot be sufficiently obtained. This may result in insufficient recovery from the sedimentation of the pigment. A mass ratio of greater than 1.00 times results in too large a proportion of aluminum oxide; therefore, due to the positive charge of the surface hydroxyl group of aluminum oxide that cannot be eliminated by poly(acrylic acid), aggregation of titanium oxide particles may occur. This may not be able to obtain sufficient recovery from the sedimentation of the pigment or sufficient recovery from the fixation of the ink. The proportion of aluminum oxide in the titanium oxide particles is preferably 0.50% by mass or more and 4.00% by mass or less relative to the total mass of the titanium oxide particles. The proportion of aluminum oxide in the titanium oxide particles is more preferably 1.00 mass % or more and 4.00 mass % or less relative to the total mass of the titanium oxide particles. A proportion of aluminum oxide less than 0.50 mass % will result in insufficient electrostatic action with poly (acrylic acid), and sometimes it is impossible to obtain sufficient recovery of the sedimentation of the pigment or sufficient recovery of the fixation of the ink. When the proportion of aluminum oxide is greater than 4.00 mass %, the aggregation of titanium oxide particles is easy to occur due to the positive charge of the surface hydroxyl groups of aluminum oxide that cannot be eliminated by poly (acrylic acid). This may not be able to obtain sufficient recovery of the sedimentation of the pigment or sufficient recovery of the fixation of the ink. The proportion of silicon dioxide in the titanium oxide particles can be 1.00 mass % or more and 4.00 mass % or less based on the total mass of the titanium oxide particles. When the proportion of silicon dioxide is within the above range, electrostatic repulsion of negative charges caused by surface hydroxyl groups of silicon dioxide can be obtained. In addition, even when using the silane compound described later, the reactivity with the silane compound can be appropriately adjusted, and the aggregation of titanium oxide particles can be further suppressed. This can further improve the recovery from sedimentation of the pigment and the recovery from fixation of the ink.

[0028] As a method for measuring the ratio of aluminum oxide and silicon dioxide in titanium oxide particles, that is, the coating amount of aluminum oxide and silicon dioxide, for example, quantitative analysis of aluminum and silicon elements by inductively coupled plasma (ICP) emission spectroscopy can be performed. In this case, it can be calculated by assuming that all atoms on the coated surface are in the form of oxides and converting the obtained values ​​of aluminum and silicon into their oxides, that is, aluminum oxide and silicon dioxide. The ratio of aluminum element in titanium oxide particles by mass ratio can be more than 0.57 times and less than 1.13 times the ratio of silicon element in titanium oxide particles, which is obtained by inductively coupled plasma emission spectroscopy. When these values ​​are converted based on their oxides, that is, aluminum oxide and silicon dioxide, the ratio of aluminum oxide in titanium oxide particles by mass ratio is more than 0.50 times and less than 1.00 times the ratio of silicon dioxide in titanium oxide particles.

[0029] Examples of methods for treating the surface of titanium oxide include wet treatment and dry treatment. For example, the surface treatment can be performed by dispersing titanium oxide in a liquid medium and then reacting the titanium oxide with a surface treatment agent such as sodium aluminate and sodium silicate. By appropriately changing the ratio of the surface treatment agent, the surface treatment can be adjusted to the desired characteristics. In addition to aluminum oxide and silicon dioxide, inorganic oxides such as zinc oxide and zirconium oxide, and organic substances such as polyols can also be used, as long as the advantageous effects of the present invention are not impaired.

[0030] The ink may contain other pigments other than titanium oxide as long as the advantageous effects of the present invention are not impaired. In this case, color inks other than white ink may also be used. The content of other pigments in the ink is preferably 0.10% by mass or more and 5.00% by mass or less, and more preferably 0.10% by mass or more and 1.00% by mass or less, based on the total mass of the ink.

[0031] Poly(acrylic acid)

[0032] The ink contains poly(acrylic acid). Poly(acrylic acid) has the effect of assisting the dispersion of titanium oxide particles. The poly(acrylic acid) content in the ink is preferably 0.01% by mass or more and 0.50% by mass or less based on the total mass of the ink, more preferably 0.01% by mass or more and 0.20% by mass or less. A poly(acrylic acid) content of less than 0.01% by mass may result in the inability to eliminate the positive charge on the surface of the titanium oxide particles, sometimes resulting in insufficient sedimentation recovery of the pigment, and insufficient fixation recovery of the ink. When the poly(acrylic acid) content is greater than 0.50% by mass, the amount of poly(acrylic acid) present is equal to or greater than the amount adsorbable on the titanium oxide particles. Therefore, salting out is easily caused by free poly(acrylic acid). As a result, it is believed that the dispersion of the titanium oxide particles is unstable, causing aggregation. Therefore, sometimes the sedimentation recovery of the pigment and the fixation recovery of the ink cannot be fully obtained.

[0033] Poly(acrylic acid) is a compound having a structure in which a plurality of carboxylic acid groups are connected to every other carbon atom constituting a hydrocarbon chain. Poly(acrylic acid) can be used appropriately whether it is a commercial product or a synthetic compound. As a synthesis method of poly(acrylic acid), a known synthesis method can be used. Poly(acrylic acid) can be synthesized, for example, by polymerization of acrylic acid. The carboxylic acid group of poly(acrylic acid) can be in acid or salt form. In the case of salt form, examples thereof include salts of alkali metals such as lithium, sodium and potassium, and (organic) ammonium salts. From the viewpoint of storage stability of ink, poly(acrylic acid) can be in the form of an alkali metal salt.

[0034] The weight average molecular weight of poly(acrylic acid) is preferably 1,000 or more and 6,000 or less. The weight average molecular weight of poly(acrylic acid) is more preferably 1,000 or more and 5,000 or less. The weight average molecular weight of poly(acrylic acid) is particularly preferably 1,000 or more and 3,000 or less. When the weight average molecular weight of poly(acrylic acid) is less than 1,000, even if poly(acrylic acid) is adsorbed on titanium oxide particles, due to its too small molecular size, the effect of inhibiting the approach between titanium oxide particles as a spacer is also weak. Therefore, when the titanium oxide particles settle, the titanium oxide particles approach each other to promote aggregation, and sometimes the sedimentation recovery of the pigment cannot be fully obtained. When the weight average molecular weight of poly(acrylic acid) is greater than 6,000, due to the excessive molecular size of poly(acrylic acid), it is believed that the carboxylic acid group is adsorbed on the surface of multiple titanium oxide particles, thereby cross-linking multiple titanium oxide particles with poly(acrylic acid). In this case, due to the cross-linking of poly(acrylic acid), the titanium oxide particles may aggregate and the sedimentation recovery of the pigment and the fixation recovery of the ink cannot be fully obtained.

[0035] Monovalent cations

[0036] The ink contains potassium ions, which are monovalent cations. The term "monovalent cations" used in this specification refers to alkali metal ions, ammonium ions, and organic ammonium ions, and does not include protons (H + ). Potassium ions promote the ionization of the carboxylic acid groups of poly(acrylic acid). In order to effectively promote the ionization of the carboxylic acid groups of poly(acrylic acid), the potassium ion content of the ink may be 300 ppm or more based on the total mass of the ink. When the potassium ion content is less than 300 ppm, the amount of potassium ions in the ink is too small to fully promote the ionization of the carboxylic acid groups of poly(acrylic acid) and the surface hydroxyl groups of the titanium oxide particles. Therefore, the redissolution of the ink composition after drying is not easy to occur, and sometimes the fixation recovery of the ink cannot be fully obtained.

[0037] In order to introduce potassium ions into the ink, for example, a compound that produces potassium ions by ion dissociation can be added to the ink. Examples of such compounds include inorganic potassium salts and organic potassium salts. Examples of inorganic potassium salts include potassium halides, such as potassium fluoride, potassium chloride and potassium bromide; potassium salts of inorganic acids, such as potassium carbonate, potassium sulfate, potassium phosphate, potassium nitrate and potassium borate; potassium hydroxide; and potassium salts of organic acids, such as potassium acetate and potassium benzoate. Any of these salts can be added to the ink. Poly (acrylic acid), which is an essential component of the ink, can be used in the form of a potassium salt. Components other than poly (acrylic acid) can be used in the form of a potassium salt. Potassium ions can be contained in the ink by ion dissociation of any of these potassium salts.

[0038] In addition to potassium ions, the ink may contain monovalent cations other than potassium ions (hereinafter, referred to as "other monovalent cations"). In this case, the potassium ion content may be higher than the other monovalent cation content. The potassium ion content equal to or less than the other monovalent cation content results in an increase in ions with smaller ionic radius and ionization tendency than potassium ions. Therefore, the efficiency of promoting the ionization of the carboxylic acid group of the poly(acrylic acid) is slightly reduced, and sometimes the fixation recovery of the ink cannot be fully obtained.

[0039] The total monovalent cation content in the ink can be 700ppm or more and 1,300ppm or less based on the total mass of the ink. The total monovalent cation content is the sum of potassium ions and other monovalent cations as the basic components of the ink. When the total monovalent cation content is less than 700ppm, the amount of monovalent cations that promote the ionization of the carboxylic acid groups of the poly(acrylic acid) and the surface hydroxyl groups of the titanium oxide particles in the ink is small. This results in insufficient adsorption of the poly(acrylic acid) on the surface of the titanium oxide particles, and a reduction in repulsive forces such as electrostatic repulsion between the titanium oxide particles. Therefore, sometimes the sedimentation recovery of the pigment cannot be fully obtained. When the total monovalent cation content is greater than 1,300ppm, the amount of monovalent cations is too much, resulting in aggregation caused by salting out. Therefore, sometimes the sedimentation recovery of the pigment cannot be fully obtained. When the ink contains cations with a valence of more than 2, the cation content can be less than 10ppm based on the total mass of the ink. The ink does not need to contain cations with a valence of more than 2. The total monovalent cation content in the ink can be measured by, for example, quantitatively containing various monovalent cations by ICP optical emission spectroscopy or ion chromatography.

[0040] Dispersants

[0041] The ink may contain a dispersant for dispersing titanium oxide particles. In particular, the ink may contain a compound represented by the following formula (1). The amount of the compound represented by formula (1) contained in the ink is preferably 0.01% by mass or more and 1.00% by mass or less, and more preferably 0.02% by mass or more and 0.50% by mass or less, based on the total mass of the ink.

[0042] A portion of one or more OR1 groups connected to the silicon atom in the compound represented by formula (1) is partially hydrolyzed in an aqueous medium to form a silanol group. Therefore, the dispersant has an affinity for the surface hydroxyl groups derived from silicon dioxide on the surface of the titanium oxide particles. In addition to the above-mentioned portion capable of forming a silanol group, the compound represented by formula (1) has other portions as repeating units, including n alkylene oxide groups each having 2 to 4 carbon atoms connected by X as a connecting group ((OR4 in formula (1)) n ). Hereinafter, the above part is also referred to as "alkylene oxide chain". Alkylene oxide chain is hydrophilic. Therefore, the alkylene oxide chain extends moderately in the aqueous medium and exhibits repulsive force due to steric hindrance. Therefore, the compound represented by formula (1) is used as a dispersant for titanium oxide particles,

[0043]

[0044] Wherein, in formula (1), R1, R2 and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, each R4 is independently an alkylene group having 2 to 4 carbon atoms, X is a single bond or an alkylene group having 1 to 6 carbon atoms, n is 6 to 24, a is 1 to 3, b is 0 to 2, and a+b=3.

[0045] In formula (1), R1, R2 and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Examples of alkyl groups having 1 to 4 carbon atoms include methyl, ethyl, n-propyl, isopropyl and n-butyl. Among them, from the viewpoint of easy hydrolysis, a methyl group can be used. When each of R1, R2 and R3 is an alkyl group having more than 4 carbon atoms, the compound is not easily hydrolyzed to form a silanol group, so that affinity for titanium oxide particles cannot be obtained. Therefore, titanium oxide particles cannot be stably dispersed, and sometimes the sedimentation recovery of the pigment and the fixation recovery of the ink cannot be fully obtained. Here, a representing the number of R1O is 1 to 3, b representing the number of R2 is 0 to 2, and a+b=3. In particular, a can be 3, b can be 0, that is, all three substituents on the silicon atom can be R1O.

[0046] In formula (1), each R4 is independently an alkylene group having 2 to 4 carbon atoms. Examples of alkylene groups having 2 to 4 carbon atoms include ethylene, n-propylene, isopropylene and n-butylene. In particular, ethylene can be used. The number of OR4, that is, n (average value) representing the number of alkylene oxide groups, is 6 to 24. When n is less than 6, the length of the alkylene oxide chain is too short, and therefore, the repulsive force caused by steric hindrance cannot be fully obtained. Thus, sometimes the sedimentation recovery of the pigment and the fixation recovery of the ink cannot be fully obtained. When n is greater than 24, the length of the alkylene oxide chain is too long, so that the compound has a higher hydrophilicity and is more likely to exist in a free form in an aqueous medium. Therefore, the affinity for the surface hydroxyl group of the titanium oxide particles cannot be fully obtained, and sometimes the aggregation of the titanium oxide particles cannot be effectively suppressed. Therefore, sometimes the sedimentation recovery of the pigment and the fixation recovery of the ink cannot be fully obtained.

[0047] In formula (1), X is a single bond or an alkylene group having 1 to 6 carbon atoms. When X is a single bond, it means that the silicon atom and OR4 are directly bonded to each other. Examples of alkylene groups having 1 to 6 carbon atoms include methylene, ethylene, n-propylene, isopropylene, n-butylene, n-pentylene and n-hexylene. In particular, n-propylene can be used. When X is an alkylene group having more than 6 carbon atoms, the hydrophobicity of the compound represented by formula (1) is too high, and the effect of stabilizing the dispersion of titanium oxide particles is weak; therefore, sometimes the sedimentation recovery of the pigment and the fixation recovery of the ink cannot be fully obtained.

[0048] The compound represented by formula (1) may be a compound represented by the following formula (2). The compound represented by formula (2) has three OR1 groups connected to silicon atoms. Therefore, the compound can be partially hydrolyzed in an aqueous medium to form three hydroxyl groups connected to silicon atoms, thereby increasing the portion having affinity for titanium oxide particles. In addition, the compound represented by the following formula (2) has a repeating unit of an oxyethylene group. Therefore, the oxyethylene chain is appropriately elongated in an aqueous medium, and a repulsive force due to steric hindrance can be obtained,

[0049]

[0050] Wherein, in formula (2), R1 and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and m is 8 to 24.

[0051] The amount of the compound represented by formula (1) contained in the ink in terms of mass ratio may be more than 0.002 times and less than 0.10 times the amount of titanium oxide particles contained in the ink. When the mass ratio is less than 0.002 times, the effect of stabilizing the dispersion of titanium oxide particles is weak. Therefore, in some cases, the sedimentation recovery of the pigment cannot be fully obtained. When the mass ratio is greater than 0.10 times, the proportion of the compound represented by formula (1) is too high; therefore, intermolecular condensation (self-condensation) of the compound represented by formula (1) is prone to occur. Therefore, the compound represented by formula (1) is not consumed as a dispersant. In this case, it is believed that the condensate of the compound represented by formula (1) plays a role in forming a denser aggregate of titanium oxide particles, and sometimes the fixation recovery of the ink cannot be fully obtained.

[0052] Resin

[0053] The ink may contain a resin. Examples of the resin include acrylic resins, polyurethane resins, and urea resins. In particular, acrylic resins may be used. The resin content in the ink is preferably 1.00% by mass or more and 25.00% by mass or less, more preferably 3.00% by mass or more and 15.00% by mass or less, and even more preferably 5.00% by mass or more and 15.00% by mass or less, based on the total mass of the ink.

[0054] In order to improve various characteristics of the recorded image, such as scratch resistance and masking, resin can be included in the ink. Examples of the form of the resin include block copolymers, random copolymers, graft copolymers and combinations of these copolymers. In addition, the resin can be a water-soluble resin soluble in an aqueous medium, or can be resin particles dispersed in an aqueous medium. The resin particles do not need to contain a coloring material.

[0055] In this specification, "water-soluble resin" means that when the resin is neutralized with an amount of alkali equivalent to the acid value of the resin, the resin exists in an aqueous medium in a state where particles whose particle size can be measured by a dynamic light scattering method are not formed. Whether the resin is soluble in water can be determined by the following method: First, a liquid (resin solid content: 10% by mass) containing a resin neutralized with an alkali equivalent to the acid value (e.g., sodium hydroxide or potassium hydroxide) is prepared. The prepared liquid is diluted to 10 times (by volume) with deionized water to prepare a sample solution. Then, when the particle size of the resin in the sample solution is measured by a dynamic light scattering method, if no particles with a particle size are measured, it can be determined that the resin is soluble in water. The measurement conditions at this time can be set as follows: for example, SetZero: 30 seconds, number of measurements: 3 times, and measurement time: 180 seconds. As a particle size distribution measuring device, for example, a particle size analyzer by a dynamic light scattering method (e.g., trade name "UPA-EX150", available from Nikkiso Co., Ltd.) can be used. Of course, the particle size distribution measuring device and the measuring conditions used are not limited to those described above.

[0056] The acid value of the water-soluble resin is preferably 80 mgKOH / g or more and 250 mgKOH / g or less, more preferably 100 mgKOH / g or more and 200 mgKOH / g or less. When resin particles are used, the acid value of the resin particles is preferably 0 mgKOH / g or more and 50 mgKOH / g or less. The weight average molecular weight of the resin is preferably 1,000 or more and 30,000 or less, more preferably 5,000 or more and 15,000 or less. The weight average molecular weight of the resin is a value converted to polystyrene by gel permeation chromatography (GPC).

[0057] Water-based media

[0058] The ink is an aqueous ink containing water as an aqueous medium. The ink may contain water or an aqueous medium as a mixed solvent of water and a water-soluble organic solvent. As water, deionized water (ion exchange water) may be used. The water content in the ink may be 50.00% by mass or more and 95.00% by mass or less based on the total mass of the ink.

[0059] There is no particular limitation on the water-soluble organic solvent as long as it is water-soluble (it can be dissolved in water at any ratio at 25°C). Specific examples of water-soluble organic solvents that can be used include monohydric or polyhydric alcohols, alkylene glycols, glycol ethers, nitrogen-containing polar compounds, and sulfur-containing polar compounds. The content of the water-soluble organic solvent in the ink is preferably 3.00% by mass or more and 50.00% by mass or less, and more preferably 10.00% by mass or more and 40.00% by mass or less, based on the total mass of the ink. When the content of the water-soluble organic solvent is greater than 50.00% by mass, ink supply failure may occur.

[0060] Other additives

[0061] In addition to the above-mentioned additives, the ink may also include various additives such as surfactants, pH regulators, rust inhibitors, preservatives, antifungal agents, antioxidants, reduction inhibitors, evaporation promoters and chelating agents as required. In particular, the ink may include surfactants. These additives may be used to provide an ink containing potassium ions. The surfactant content in the ink is based on the total mass of the ink, preferably 0.10% by mass or more and 5.00% by mass or less, more preferably 0.10% by mass or more and 2.00% by mass or less. Examples of surfactants include anionic surfactants, cationic surfactants and nonionic surfactants. Among them, a nonionic surfactant having low affinity for titanium oxide particles and effective even in a small amount may be used because the surfactant is used to adjust the various physical properties of the ink.

[0062] Physical properties of ink

[0063] The ink is used in an inkjet recording method; therefore, its physical properties can be appropriately controlled. The surface tension of the ink at 25°C is preferably 10mN / m or more and 60mN / m or less, more preferably 20mN / m or more and 40mN / m or less. The surface tension of the ink can be adjusted by appropriately determining the type and amount of the surfactant in the ink. The viscosity of the ink at 25°C can be 1.0mPa·s or more and 10.0mPa·s or less. The pH value of the ink at 25°C can be 7.0 or more and 9.0 or less. The pH of the ink can be measured using a general pH meter equipped with, for example, a glass electrode.

[0064] Uses of ink

[0065] The ink according to the above-mentioned embodiment of the present disclosure contains titanium oxide particles and can therefore be used as white ink. In this case, as described above, in order to show a vivid color image even on a transparent recording medium, a white ink may be applied in advance for primer treatment, and then a color ink may be applied thereon, or each ink may be applied in the reverse order (so-called back printing). The color ink is an ink containing a coloring material different from the titanium oxide particles and presenting a color such as black, cyan, magenta, or yellow. The color ink used in combination with the ink according to the embodiment of the present disclosure (hereinafter also referred to as "white ink") will be described in detail below.

[0066] Color ink

[0067] Coloring Materials

[0068] The color ink contains a coloring material other than titanium oxide particles (hereinafter, also referred to as "color pigment" or simply "pigment" to distinguish it from white). The content of the pigment in the color ink is preferably 0.10 mass % or more and 15.00 mass % or less, and more preferably 1.00 mass % or more and 10.00 mass % or less based on the total mass of the ink.

[0069] Specific examples of the pigment include inorganic pigments such as carbon black, and organic pigments such as azo, phthalocyanine, quinacridone, isoindolinone, imidazolone, diketopyrrolopyrrole, and dioxazine. In particular, carbon black and organic pigments can be used.

[0070] Examples of the dispersion form of the pigment include resin-dispersed pigments using a resin as a dispersant and self-dispersed pigments in which a hydrophilic group is bonded to the particle surface of the pigment. Further examples thereof include resin-bound pigments in which an organic group containing a resin is chemically bonded to the particle surface of the pigment and microcapsule pigments in which the particle surface of the pigment is coated with, for example, a resin. Among them, a resin-dispersed pigment in which a resin as a dispersant is physically adsorbed on the particle surface of the pigment may be used instead of the resin-bound pigment or the microcapsule pigment.

[0071] As a self-dispersing pigment, a pigment in which anionic groups such as carboxylic acid groups, sulfonic acid groups or phosphonic acid groups are directly or via other atomic groups (-R-) bonded to the particle surface of the pigment can be used. The anionic group can be any one of an acid form and a salt form. When the anionic group is in the form of a salt, the anionic group can be in any one of a state in which the anionic group is partially dissociated and a state in which the anionic group is completely dissociated. When the anionic group is in the form of a salt, examples of cations used as counterions include alkali metal cations, ammonium ions and organic ammonium ions. Specific examples of other atomic groups (-R-) include straight or branched alkylene groups having 1 to 12 carbon atoms; arylene groups, such as phenylene or naphthylene groups; carbonyl groups; imino groups; amide groups; sulfonyl groups; ester groups; and ether groups. The group can be a group obtained by combining these groups.

[0072] Monovalent cations

[0073] Color ink may contain monovalent cations. Examples of monovalent cations include alkali metal ions, ammonium ions, and organic ammonium. In particular, potassium ions may be contained. Color ink may contain a variety of monovalent cations. In this case, the monovalent cation content is the total amount of monovalent cations in the color ink. The monovalent cation content in the color ink may be 980 ppm or more and 6,500 ppm or less based on the total mass of the ink. When the monovalent cation content in the color ink is greater than the above range, the storage stability of the color ink may not be obtained due to salting out. When the color ink contains cations with a valence of two or more, the cation content may be 10 ppm or less based on the total mass of the ink. Color ink does not need to contain cations with a valence of two or more. The monovalent cation content in the color ink may be measured, for example, by quantitatively measuring the amount of various monovalent cations contained by ICP emission spectroscopy or ion chromatography.

[0074] In order to introduce monovalent cations into the color ink, for example, a compound that generates monovalent cations by ion dissociation can be added to the ink. Examples of such compounds include alkali metal salts and ammonium salts. Examples of alkali metal salts include alkali metal salts of halogens such as fluorine, chlorine and bromine; alkali metal salts of inorganic acids such as carbonic acid, sulfuric acid, phosphoric acid, nitric acid and boric acid; alkali metal hydroxides; and alkali metal salts of organic acids such as acetic acid and benzoic acid. Examples of ammonium salts include ammonium salts of halogens such as fluorine, chlorine and bromine; ammonium salts of inorganic acids such as carbonic acid, sulfuric acid, phosphoric acid, nitric acid and boric acid; and ammonium salts of organic acids such as acetic acid and benzoic acid.

[0075] The monovalent cation content M2 in the color ink is preferably 1.40 times or more and 5.00 times or less of the monovalent cation content M1 of the white ink in terms of mass ratio (M2 / M1). The ratio is more preferably 3.00 times or less. When the value of M2 / M1 is within the above range, the aggregation of the titanium oxide particles is appropriately regulated, and a secondary color image with excellent color development can be recorded.

[0076] Resin Dispersants

[0077] Color ink can contain resin (resin dispersant) for dispersing pigment. That is, the coloring material in the color ink can be a resin-dispersed pigment. The content of the resin dispersant in the color ink is preferably 1.00 mass % or more and 25.00 mass % or less based on the total mass of the color ink, more preferably 3.00 mass % or more and 15.00 mass % or less. In particular, the content of the resin dispersant is 5.00 mass % or more and 15.00 mass % or less. When the dispersion mode of the pigment is self-dispersed, it is not necessary to include a resin dispersant.

[0078] As resin dispersants, resin dispersants that can disperse pigments in aqueous media through the action of anionic groups can be used. Water-soluble resins can be used as resin dispersants. Examples thereof include acrylic resins, polyurethane resins, urea-formaldehyde resins, polysaccharides and polypeptides. Among them, acrylic resins and polyurethane resins can be used. In particular, acrylic resins containing units derived from (meth) acrylic acid and (meth) acrylate can be used.

[0079] As the acrylic resin, an acrylic resin having a hydrophilic unit and a hydrophobic unit as structural units is preferred. Among them, a resin having a hydrophilic unit derived from (meth) acrylic acid and a hydrophobic unit derived from at least one of a monomer having an aromatic ring and a (meth) acrylic ester is preferred. In particular, a resin having a hydrophilic unit derived from (meth) acrylic acid and a hydrophobic unit derived from at least one of a styrene monomer and an α-methylstyrene monomer is preferred. These resins easily interact with pigments and can therefore be suitably used as a resin dispersant for dispersing pigments.

[0080] The hydrophilic unit is a unit having a hydrophilic group such as an anionic group or an ethylene oxide group. For example, the hydrophilic unit can be formed by polymerizing the hydrophilic monomer with the hydrophilic group. The specific example of the hydrophilic monomer with the hydrophilic group includes acidic monomers with carboxylic acid groups such as (methyl) acrylic acid, itaconic acid, maleic acid and fumaric acid, and anionic monomers such as anhydrides and salts of these acidic monomers. The example of the cation constituting the salt of the acidic monomer includes ions such as lithium ions, sodium ions, potassium ions, ammonium ions and organic ammonium ions. The monovalent cation obtained by the ion dissociation of the salt of the acidic monomer can be included in the color ink.

[0081] The hydrophobic unit is a unit that does not have a hydrophilic group such as an anionic group or an ethylene oxide group. For example, the hydrophobic unit can be formed by polymerizing a hydrophobic monomer that does not have the above-mentioned hydrophilic group. Specific examples of the hydrophobic monomer include aromatic ring-containing monomers such as styrene, α-methylstyrene, and benzyl (meth)acrylate; (meth)acrylate monomers such as methyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0082] The acid value of the resin used as the resin dispersant may be 0 mgKOH / g or more and 250 mgKOH / g or less. The weight average molecular weight of the resin dispersant is preferably 1,000 or more and 30,000 or less, more preferably 5,000 or more and 15,000 or less. The weight average molecular weight of the resin dispersant is a value calculated in terms of polystyrene by gel permeation chromatography (GPC).

[0083] Other resins

[0084] Color ink can contain resin (other resin) different from resin dispersant. The content of other resin in color ink can be more than 0.10 mass % and less than 5.00 mass % based on the total mass of color ink. In order to improve various properties of recorded image, other resin can be included in color ink. Examples of the form of resin include block copolymers, random copolymers, graft copolymers and combinations of these copolymers. In addition, resin can be a water-soluble resin soluble in water-based medium, or can be resin particles dispersed in water-based medium. Resin particles do not need to contain coloring material.

[0085] The acid value of the other resin may be 0 mgKOH / g or more and 250 mgKOH / g or less. The weight average molecular weight of the other resin is preferably 1,000 or more and 30,000 or less, more preferably 5,000 or more and 15,000 or less. The weight average molecular weight of the other resin is a value calculated in terms of polystyrene by gel permeation chromatography (GPC).

[0086] Water-based media

[0087] Color ink is an aqueous ink containing water as an aqueous medium. Color ink may contain water or an aqueous medium as a mixed solvent of water and a water-soluble organic solvent. As water, deionized water (ion exchange water) may be used. The water content in the color ink may be 50.00 mass % or more and 95.00 mass % or less based on the total mass of the ink.

[0088] There is no particular restriction on the water-soluble organic solvent, as long as it is water-soluble (it can be dissolved in water at any ratio at 25°C). Specific examples of water-soluble organic solvents that can be used include monohydric or polyhydric alcohols, alkylene glycols, glycol ethers, nitrogen-containing polar compounds and sulfur-containing polar compounds. The content of water-soluble organic solvent in the color ink is preferably 3.00% by mass or more and 50.00% by mass or less based on the total mass of the color ink, and more preferably 10.00% by mass or more and 40.00% by mass or less. When the content of the water-soluble organic solvent is less than 3.00% by mass, the ink may adhere to the inkjet recording device and may have insufficient adhesion resistance. When the content of the water-soluble organic solvent is greater than 50.00% by mass, the viscosity of the ink is too high, and the fluidity is reduced, which may lead to poor ink supply.

[0089] Other additives

[0090] In addition to the above-mentioned additives, as required, the color ink may also include various additives such as surfactants, pH regulators, rust inhibitors, preservatives, antifungal agents, antioxidants, reduction inhibitors, evaporation promoters and chelating agents. In particular, the color ink may include a surfactant. The surfactant content in the color ink is preferably 0.10% by mass or more and 5.00% by mass or less based on the total mass of the color ink, more preferably 0.10% by mass or more and 2.00% by mass or less. The example of the surfactant includes anionic surfactants, cationic surfactants and nonionic surfactants. Among them, nonionic surfactants are used to adjust the various physical properties of the color ink.

[0091] Physical properties of color ink

[0092] Color ink is used in an inkjet recording method; therefore, its physical properties can be appropriately controlled. The surface tension of the color ink at 25°C is preferably 10 mN / m or more and 60 mN / m or less, more preferably 20 mN / m or more and 40 mN / m or less. The surface tension of the color ink can be adjusted by appropriately determining the type and amount of the surfactant in the color ink. The viscosity of the color ink at 25°C can be 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the color ink at 25°C is preferably 7.0 or more and 11.0 or less, more preferably 7.0 or more and 9.0 or less. The pH of the color ink can be measured with a general-purpose pH meter equipped with, for example, a glass electrode.

[0093] ink cartridge

[0094] The ink cartridge according to the embodiment of the present invention includes ink and an ink storage portion storing the ink. The ink contained in the ink storage portion is the above-mentioned aqueous ink (white ink) according to the embodiment of the present invention. Figure 1 Schematically shows a cross-sectional view of an exemplary embodiment of an ink cartridge of the present invention. Figure 1 As shown, an ink supply port 12 for supplying ink to a recording head is provided on the bottom surface of the ink cartridge. The interior of the ink cartridge is an ink storage portion for storing ink. The ink storage portion includes an ink storage chamber 14 and an absorber storage chamber 16 which are connected to each other through a communication port 18. The absorber storage chamber 16 is connected to the ink supply port 12. The ink storage chamber 14 contains liquid ink 20. The absorber storage chamber 16 receives absorbers 22 and 24 which keep the ink in an impregnated state. The ink storage portion may be configured to include an absorber which maintains the total amount of stored ink without having an ink storage chamber for storing liquid ink. The ink storage portion does not have an absorber and may be configured to store the total amount of liquid ink. In addition, the ink cartridge may be configured to include an ink storage portion and a recording head.

[0095] Inkjet recording method

[0096] The inkjet recording method according to an embodiment of the present invention is a method for recording an image on a recording medium by ejecting the above-mentioned aqueous ink according to an embodiment of the present invention from an inkjet recording head. Examples of methods for ejecting ink include methods for applying mechanical energy to ink and methods for applying thermal energy to ink. In one embodiment of the present invention, a method for ejecting ink by applying thermal energy to ink can be used. In addition to using the ink according to an embodiment of the present invention, the steps included in the inkjet recording method can be the same as the known steps. For example, when recording an image with white ink, a general inkjet recording method can be used as it is. When the color ink is primed with white ink, the image can be recorded by applying a color ink (e.g., black, cyan, magenta or yellow ink) to overlap at least a portion of the area where the white ink is applied. In addition, the primer treatment can also be used for reverse printing of applying white ink in a manner that overlaps at least a portion of the area where the color ink is applied. There is no particular limitation on the recording medium, but since the aqueous ink according to an embodiment of the present invention can be used as white ink, a transparent or colored recording medium can be used. The recording medium can be a poorly absorptive medium (non-absorbent medium), such as a resin film with low liquid medium absorbency.

[0097] Figure 2A is a perspective view schematically showing an example of a main part of an inkjet recording apparatus used in the inkjet recording method according to the present invention, and Figure 2B 1 is a perspective view schematically showing an example of a head box used in the inkjet recording method according to the present invention. The inkjet recording device includes a conveying unit (not shown) configured to convey a recording medium 32; and a carriage shaft 34. A head box 36 can be mounted to the carriage shaft 34. The head box 36 includes recording heads 38 and 40, and is configured in a manner in which an ink cartridge 42 is disposed therein. While the head box 36 is conveyed in the main scanning direction along the carriage shaft 34, ink (not shown) is ejected from the recording heads 38 and 40 toward the recording medium 32. Then, the recording medium 32 is conveyed in the sub-scanning direction by the conveying unit (not shown), thereby recording an image on the recording medium 32.

[0098] Multi-pass recording in which ink is applied to a unit area of ​​a recording medium in multiple relative scans of a recording head and a recording medium may be used. In particular, applying white ink to a unit area and applying color ink thereto may be performed in different relative scans. This allows more time for the inks to contact each other, and is more likely to suppress mixing. The unit area may be set to an arbitrary area, such as one pixel or one band.

[0099] Example

[0100] Hereinafter, the present invention will be described in more detail by way of examples and comparative examples. The present invention is not limited to the following examples as long as it is within the scope of the present invention. With regard to the amounts of the components, "parts" and "%" are based on mass unless otherwise specified. The titanium oxide particle dispersion is referred to as a "pigment dispersion".

[0101] Preparation of titanium oxide

[0102] Commercially available titanium oxide particles that had been surface-treated in advance and titanium oxide particles prepared by surface-treating untreated titanium oxide were used. The volume-based 50% cumulative particle size (D 50 ) was measured by a dynamic light scattering method using a particle size analyzer (trade name: "UPA-EX150", available from Nikkiso Co., Ltd.). Table 1 shows the properties of the titanium oxide particles. In Table 1, TITANIX:JR, JR-403, JR-405, and JR-600A are trade names of rutile titanium oxide available from Tayca Corporation.

[0103] Measurement of the amount of alumina and silica coating

[0104] The ratio of aluminum oxide and silicon dioxide in the titanium oxide particles, that is, the coating amount of aluminum oxide and silicon dioxide is measured as follows: a liquid obtained by adding the prepared titanium oxide particles to nitric acid is used as a sample. Aluminum and silicon elements are quantitatively analyzed using inductively coupled plasma (ICP) emission spectroscopy. At this time, assuming that all atoms on the surface of the titanium oxide coating are in the form of oxides, the obtained aluminum and silicon values ​​are converted to values ​​based on oxides, that is, aluminum oxide and silicon dioxide, and the mass ratio is calculated.

[0105] Titanium oxide particles 1, 3 to 6, 8 and 10

[0106] The surface treatment of titanium oxide is carried out by a wet method to produce each titanium oxide particle. In the surface treatment by a wet method, untreated titanium oxide is contacted with a surface treatment agent (e.g., sodium aluminate and sodium silicate). In the surface treatment, the amount and ratio of the surface treatment agent used are appropriately adjusted to achieve the desired ratio.

[0107] Specifically, 300 parts of unsurface-treated rutile titanium oxide (trade name: "TITANIX JR", available from Tayca Corporation) and 700 parts of deionized water were mixed using a homogenizer. The temperature was raised to 90°C while stirring. Potassium hydroxide (pH adjuster) was added to adjust the pH to 10.5. Sodium silicate was added thereto. Dilute sulfuric acid (pH adjuster) was added within about 1 hour to adjust the pH to 5.0. The reaction was continued for about 1 hour. Then, a small amount of sodium aluminate was added at 90°C. In order to maintain the pH, dilute sulfuric acid was used in combination to keep the pH above 6.0 and below 8.0. After adding sodium aluminate, the reaction was continued for about 1 hour to obtain a dispersion. The dispersion was cooled to 25°C, purified by repeated sedimentation and redispersion in ion exchange water with a centrifugal separator, and dried at 120°C to obtain each titanium oxide particle surface-treated with at least one of aluminum oxide and silicon dioxide. Table 1 shows the properties of each titanium oxide particle.

[0108] Titanium oxide particles 2, 7, 9 and 11

[0109] As titanium oxide particles 2, 7, 9 and 11, commercially available titanium oxide particles (including those preliminarily surface-treated with aluminum oxide and / or silicon dioxide) were used. Table 1 also shows the properties of titanium oxide particles 2, 7, 9 and 11. Some commercially available titanium oxide particles contain inorganic oxides such as zirconium oxide and zinc oxide, and organic compounds such as polyols in addition to aluminum oxide and silicon dioxide, but the proportion thereof is at most about 1.0%. Therefore, for the sake of convenience, these are collectively included in the proportion T (%) of titanium oxide in the titanium oxide particles ("titanium oxide T (%)" in Table 1).

[0110] Table 1: Properties of iron oxide particles

[0111]

[0112] Preparation of the compound represented by formula (1)

[0113] The compound represented by formula (1) is synthesized by the following steps. The synthesis conditions for the compound represented by formula (1) and the comparative compound are given in Table 2, and their structures are given in Table 3. The compound represented by formula (1) can be synthesized by allylation and hydrosilylation of a raw material (e.g., polyalkylene glycol monoalkyl ether).

[0114] The raw materials, alkali and solvent listed in Table 2 are fed into a three-necked flask equipped with a stirring rod and a nitrogen inlet. The mixture is stirred at 25°C for 30 minutes. As "sodium hydride", a 60% dispersion of sodium hydride in paraffin is used. This dispersion is used to reach the amount of sodium hydride given in Table 2. While dripping the bromide described in Table 2, the mixture is stirred at 25°C. After the addition is completed, stirring is continued for an additional 12 hours to prepare a mixture containing the reaction product. After separating unreacted sodium hydride and the neutralization product (sodium bromide) from the mixture containing the reaction product by filtration, THF is removed under reduced pressure to obtain a concentrate. The concentrate is dissolved in 500 parts of deionized water. The aqueous solution is extracted 3 times with 200mL of hexane, and then extracted with 200mL of dichloromethane. The solvent containing the product is dried by magnesium sulfate and evaporated under reduced pressure to obtain each allylated compound (allylation step).

[0115] The allylation raw materials and silane compounds given in Table 2 are fed into a passivated dry round-bottom flask equipped with a stirring rod and an argon inlet. The mixture is stirred at 85°C. Then, 0.54 parts of 65mmol / L solution of chloroplatinic acid monohydrate in isopropanol and water are added thereto. The mixture is heated at 85°C for 5 hours. After the reaction is complete, the mixture is cooled to 25°C. Excess silane compounds are removed under reduced pressure. The residue is purified by column chromatography using silica gel passivated with triethoxysilane as a carrier to obtain each compound (hydrosilylation step). In the purification by column chromatography, an eluent of ethyl acetate / hexane / ethanol=85 / 15 / 5 (based on volume) is used.

[0116] Table 2: Synthesis conditions of the compound represented by formula (1)

[0117]

[0118] Table 3: Structures of the synthesized compounds represented by formula (1)

[0119]

[0120] Preparation of pigment dispersion

[0121] The pigment dispersion was produced by the following steps. The production conditions of the pigment dispersion are given in Table 4.

[0122] Pigment dispersions 1 to 20 and 22 to 24

[0123] 40.00 parts of titanium oxide particles, dispersants, neutralizers and ion exchange water given in Table 4, used in an amount of 100.00 parts in total of each component, were mixed. A preliminary dispersion treatment was performed using a homogenizer. Thereafter, a dispersion treatment (main dispersion treatment) was performed at 25°C for 12 hours using a paint stirrer using 0.5 mm zirconium oxide beads. When a neutralizer is used, the amount of the neutralizer used is appropriately adjusted to achieve a pH of 10.5 for the main dispersion. The pH of the main dispersion is a value measured with a pH meter (trade name: "Portable pH Meter D-74", available from Horiba, Ltd.) at the beginning of the main dispersion treatment. The zirconium oxide beads were separated by filtration. An appropriate amount of ion exchange water was added as needed to prepare each pigment dispersion having a titanium oxide particle content of 40.00%. In Table 4, the "poly (acrylic acid)" of the pigment dispersion 24 was synthesized by the following method, had a weight average molecular weight of 5,000, and was a potassium salt type.

[0124] Pigment dispersion 21

[0125] A pigment dispersion was prepared according to the method for preparing pigment 3k in Example 3 of PCT Japanese Translation Patent Publication No. 2017-521348. Specifically, a pigment dispersion was prepared according to the production method of the above-mentioned dispersion 19. The obtained pigment dispersion was dried by blowing air at 35°C under stirring, and then dried in an oven at 105°C for 4 hours and 15 minutes to obtain a titanium oxide particle powder. The titanium oxide particle powder was redispersed in an appropriate amount of ion exchange water to prepare a pigment dispersion 21 having a titanium oxide particle content of 40.00%.

[0126] Table 4: Production conditions of pigment dispersion

[0127]

[0128] Synthesis of resin particles

[0129] In a four-necked flask equipped with an agitator, a reflux condenser and a nitrogen inlet, 0.2 parts of potassium persulfate and 74.0 parts of ion exchange water were placed. Then, nitrogen was introduced therein. The monomers given in Table 5 and 0.3 parts of an emulsifier (trade name: "NIKKOL BC15", available from Nikko Chemicals Co., Ltd.) were mixed to prepare a mixture. The resulting mixture was added dropwise to a four-necked flask under stirring for 1 hour, and then reacted at 80°C for 2 hours. The reaction mixture was cooled to 25°C. A neutralizer in an amount equal to the acid value of the resin in moles and an appropriate amount of ion exchange water were added to the reaction mixture to prepare an aqueous dispersion of polymer particles 1 to 8 having a resin particle content of 40.0% and a cumulative particle size of 100 nm based on 50% volume. Table 5 gives the acid value of the resin particles. The details of each component in Table 5 are described below.

[0130] ·BMA: Butyl Methacrylate

[0131] MAA: Methacrylic acid

[0132] Table 5: Synthesis conditions and properties of resin particles

[0133]

[0134] Synthesis of poly(acrylic acid)

[0135] Acrylic acid is polymerized in the usual manner to synthesize poly(acrylic acid). The weight average molecular weight is adjusted by adjusting the heating temperature and time during the polymerization. The carboxylic acid groups are converted into sodium, lithium, potassium and ammonium salt forms with sodium hydroxide, lithium hydroxide, potassium hydroxide and ammonia, respectively, which are used in an amount equal to the acid value in moles.

[0136] Preparation of liquid containing alumina particles

[0137] The liquid containing alumina particles was prepared by the following method. Specifically, an alumina particle dispersion containing 10% of amphoteric alumina particles (trade name: "Dispal 23N4-80", dispersed particle size: 90 nm, available from Sasol) was provided. The pH of the alumina particle dispersion was adjusted to 4.0 with a strong acid (1 mol / L hydrochloric acid). The alumina particle dispersion was mixed with a propeller mixer until it became uniform, and pulverized with a bead mill to prepare a liquid containing alumina particles (alumina particle content: 10%).

[0138] Ink preparation

[0139] The components of the types and amounts given in the upper rows of Tables 6 to 9 are mixed and stirred. Acetylenol E60 (trade name) is a nonionic surfactant available from Kawaken Fine Chemicals Co., Ltd. Proxel GXL (S) (trade name) is a preservative available from LONZA. Thereafter, pressure filtration is performed using a membrane filter having a pore size of 5.0 μm (available from Sartorius) to prepare each ink. In Tables 6 to 9, the weight average molecular weight and salt form of the poly (acrylic acid) are recorded together. For example, the record of "poly (acrylic acid) (Mw: 1,500, sodium salt)" indicates that the weight average molecular weight is 1500 and the poly (acrylic acid) is in the form of a sodium salt.

[0140] Calculation of total monovalent cation content in ink

[0141] The total monovalent cation content in the ink is measured by ICP optical emission spectroscopy. Specifically, each prepared ink is diluted with ion exchange water so that the pigment content is 0.04%. The amount of various monovalent cations contained in the ink is quantified using an ICP optical emission spectrometer (trade name: "SPS5100 ICP-OES", available from Dionex). Among the monovalent cations, the ammonium ion concentration is measured using an ion chromatograph (trade name: "DX-320", available from Dionex). The total monovalent cation content (ppm) in the case of the titanium oxide particle content in the ink before dilution is calculated from the quantitative monovalent cation content. Tables 6 to 9 collectively show the properties of each ink in the lower part, the potassium ion content, and the total monovalent cation content.

[0142] Table 6: Ink composition and properties

[0143]

[0144] Table 7: Ink composition and properties

[0145]

[0146] Table 8: Ink composition and properties

[0147]

[0148] Table 9: Ink composition and properties

[0149]

[0150] evaluate

[0151] Each ink obtained above was evaluated for the following items. In the examples of the present disclosure, in the evaluation criteria of each item described below, "A" and "B" are defined as acceptable levels, and "C" is defined as an unacceptable level. Table 10 shows the evaluation results.

[0152] Sedimentation recovery

[0153] First, 8.0g of each ink obtained above is placed in a 10mL centrifuge tube made of polytetrafluoroethylene. A portion of the liquid in the area extending from the upper surface of the liquid to a depth of about 1cm is sampled. The absorbance at 550nm (called "absorbance before oscillation") is measured. A spectrophotometer (trade name: "U-3011", available from Hitachi High-Tech Science Corporation) is used for absorbance measurement. The ink is stored at 25°C for 6 days, and then, it is vibrated at 180rpm for 5 minutes with an oscillator (trade name: "Labo Shaker Wide SR-5", available from As One Corp.) to disperse the titanium oxide particles again. After oscillation, a portion of the liquid in the area extending from the upper surface of the liquid to a depth of about 1cm is sampled. The absorbance at 550nm (called "absorbance after oscillation") is measured in the same way. The absorbance recovery rate is calculated based on the following formula: absorbance recovery rate = 100 × ("absorbance after oscillation") / ("absorbance before oscillation"). The sedimentation recovery property of the pigment was evaluated according to the following evaluation criteria.

[0154] A: The absorbance recovery rate is 90% or more.

[0155] B: The absorbance recovery rate is 85% or more and less than 90%.

[0156] C: The absorbance recovery rate is less than 85%.

[0157] Fixation recovery

[0158] In an open system container, place 5.0 g of each ink obtained above. Dry the ink for 1 day in an environment with a temperature of 30°C and a relative humidity of 10%. Measure the mass of the ink residue in the container (referred to as the "mass of the initial residue"). Add 3.0 g of the same ink to the ink residue. Stir the mixture. Afterwards, filter the ink containing the residue, and measure the mass of the residue again (referred to as the "mass of the residue after redissolution"). The "residual rate after redissolution" is calculated based on the formula 100×("mass of the residue after redissolution") / ("mass of the initial residue"), and evaluate the ink fixation recovery according to the following evaluation criteria. The lower the residual rate after redissolution, the easier it is to remove the fixed matter of the ink dried in the recording head, that is, the better the ink fixation recovery.

[0159] A: The residual rate after redissolution is less than 20%.

[0160] B: The residual rate after re-dissolution is 20% or more and less than 50%.

[0161] C: The residual rate after re-dissolution is 50% or more.

[0162] Table 10: Evaluation results

[0163]

[0164] Color rendering of secondary color images

[0165] After forming an undercoat layer with the ink of Example 1, a color ink prepared as described below was applied to obtain a secondary color image, and the color developability of the secondary color image was evaluated.

[0166] Preparation of color pigment dispersion

[0167] Color Pigment Dispersion 1 to 4

[0168] The pigment and dispersant of the type and amount given in Table 11 are mixed with ion exchange water used in an amount such that the total amount of each component is 100.00%. A homogenizer is used for preliminary dispersion treatment. As a dispersant, a copolymer having a group having affinity for the pigment is used (trade name: "DISPERBYK-199", available from BYK Japan KK). After that, a dispersion treatment (main dispersion) is carried out at 25° C. for 12 hours using a paint stirrer using 0.5 mm zirconium oxide beads. The zirconium oxide beads are separated by filtration. An appropriate amount of ion exchange water is added thereto as needed. Thus, color pigment dispersions 1 to 4 are prepared.

[0169] Color Pigment Dispersion 5

[0170] As color pigment dispersion 5, a pigment dispersion prepared by mixing a commercially available pigment dispersion (trade name: "Cab-O-Jet 400", available from Cabot Corporation, pigment content: 15.00%) with ion exchange water to adjust the pigment content to 14.00% was used. The pigment dispersion contains a self-dispersible pigment in which a phosphonic acid group is connected to the particle surface of a pigment (carbon black) through other atomic groups.

[0171] Table 11: Preparation conditions and properties of color pigment dispersions

[0172]

[0173] Preparation of color ink

[0174] The components of the kind and amount given in the upper part of Table 12 were mixed and stirred. Vinyblan 2685 (trade name) is the trade name of an acrylic emulsion (acrylic resin particle content: 30%) available from Nissin Chemical Industry Co., Ltd. Ion-exchanged water containing potassium hydroxide is ion-exchanged water to which potassium hydroxide is added so as to have the monovalent cation content given in the lower part of Table 12. The ion-exchanged water containing potassium hydroxide was added in such a manner that the sum of the components was 100.0%. Thereafter, filter pressing was performed using a membrane filter having a pore size of 5.0 μm (available from Sartorius). Thus, color inks 33 to 41 were prepared. The pH of each color ink was measured with a pH meter (trade name: "Portable pH Meter D-74", available from Horiba, Ltd). The pH of each color ink was in the range of 7.0 to 11.0.

[0175] Color rendering

[0176] The ink of Example 1 and each color ink prepared as described above are filled into the ink cartridge. The ink cartridge is set in an inkjet recording device (trade name: "PIXUS PRO10-S", available from CANONKABUSHIKI KAISHA) equipped with a recording head that ejects ink by thermal energy. The device prints in a serial manner and includes a plurality of ejection port arrays arranged in a sub-scanning direction (recording medium conveying direction) perpendicular to the main scanning direction of the recording head. The ink cartridge filled with the ink of Example 1 and the ink cartridge filled with color ink are arranged in the device in a manner such that their ejection port arrays are adjacent to each other. In this example, an image recorded under the condition that 4 ink droplets each weighing 3.8ng are applied to a unit area (1 pixel) of 1 / 600 inch × 1 / 600 inch is defined as a 100% recording task. Under these conditions, an evaluation image as described below is recorded by multi-pass recording (the application of ink to a unit area of ​​the recording medium is performed in multiple relative scans between the recording head and the recording medium).

[0177] Specifically, an evaluation image was recorded under the condition that the ink of Example 1 and the color ink were applied in an overlapping manner with different numbers of recording passes. The ink of Example 1 was set so as to be ejected from the ejection ports corresponding to 1 / 2 of the ejection port array located upstream in the sub-scanning direction. The color ink was set so as to be ejected from the ejection ports corresponding to 1 / 2 of the ejection port array located downstream in the sub-scanning direction. A solid image in which the recording duty of the color ink was 100% was recorded so as to overlap with a solid image in which the recording duty of the white ink was 100%. The resulting recorded matter was dried in an oven at 120° C. for 10 minutes to obtain an evaluation image.

[0178] For the secondary color image in the evaluation image obtained above, L*, a*, and b* in the Lab color system were measured using a fluorescence spectrophotometer (trade name: "FD-7", available from Konica Minolta Japan, Inc.). Based on the equation C*={(L*) 2 +(a*) 2 +(b*) 2} 1 / 2 Calculate the chromaticity C*. The color rendering of the secondary color image was evaluated according to the following evaluation criteria. The higher the chromaticity C* value of the image means the better the color rendering of the image.

[0179] A: The chromaticity C* value of the image is 35 or more.

[0180] B: The chromaticity C* value of the image is less than 35.

[0181] The color development properties of the secondary color images in Examples 40 and 41 were "B", which was the same as that in Example 39. However, the secondary color image in Example 39 showed excellent color development properties.

[0182] Table 12: Composition, properties and evaluation results of color inks

[0183]

[0184] According to an embodiment of the present disclosure, it is possible to provide an aqueous ink containing titanium oxide that is used for inkjet recording and has excellent sedimentation recovery of a pigment and fixation recovery of an ink, an ink cartridge that accommodates the aqueous ink, and an inkjet recording method.

[0185] While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments.The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.

Claims

1. A water-based ink for inkjet recording, comprising: Titanium oxide particles; Poly(acrylic acid); and Potassium ions, It is characterized in that The titanium oxide particles include titanium oxide at least a portion of the surface of which is coated with aluminum oxide and silicon dioxide, and An amount of the poly(acrylic acid) contained in the aqueous ink is 0.05 times or more and 0.40 times or less the amount of the aluminum oxide contained in the titanium oxide particles in terms of mass ratio.

2. The aqueous ink according to claim 1, further comprising a monovalent cation different from the potassium ion, The amount of the potassium ions is greater than the amount of monovalent cations other than the potassium ions in terms of mass ratio. 3 . The aqueous ink according to claim 1 , wherein a ratio of the aluminum oxide in the titanium oxide particles is 0.50 times or more and 1.00 times or less of a ratio of the silicon dioxide in the titanium oxide particles in terms of mass ratio. 4 . The aqueous ink according to claim 1 , wherein a ratio of the titanium oxide in the titanium oxide particles is 90.00% by mass or more based on the total mass of the titanium oxide particles. 5 . The aqueous ink according to claim 1 , wherein a ratio of the titanium oxide in the titanium oxide particles is 98.50% by mass or less based on the total mass of the titanium oxide particles. 6 . The aqueous ink according to claim 1 , wherein a ratio of the aluminum oxide in the titanium oxide particles is 0.50% by mass or more and 4.00% by mass or less based on the total mass of the titanium oxide particles. 7 . The aqueous ink according to claim 1 , wherein a ratio of the silicon dioxide in the titanium oxide particles is 1.00% by mass or more and 4.00% by mass or less based on the total mass of the titanium oxide particles.

8. The water-based ink according to claim 1, wherein: The ratio of the aluminum element in the titanium oxide particles is 0.57 times or more and 1.13 times or less of the ratio of the silicon element in the titanium oxide in terms of mass ratio, and the ratio is obtained by inductively coupled plasma emission spectrometry.

9. The water-based ink according to claim 1, wherein: The titanium oxide particles have a 50% cumulative particle size based on volume of 200 nm or more and 400 nm or less. 10 . The aqueous ink according to claim 1 , wherein an amount of the titanium oxide particles contained in the aqueous ink is 1.00% by mass or more and 20.00% by mass or less based on the total mass of the ink.

11. The water-based ink according to claim 1, wherein: The weight average molecular weight of the poly(acrylic acid) is 1,000 or more and 6,000 or less.

12. The water-based ink according to claim 1, wherein: The weight average molecular weight of the poly(acrylic acid) is 1,000 or more and 3,000 or less.

13. The water-based ink according to claim 1, wherein: The amount of the poly(acrylic acid) is 0.01% by mass or more and 0.50% by mass or less based on the total mass of the ink.

14. The water-based ink according to claim 1, wherein: The potassium ion content in the aqueous ink is 300 ppm or more based on the total mass of the ink.

15. The water-based ink according to claim 1, wherein: The total monovalent cation content in the aqueous ink is 700 ppm or more and 1,300 ppm or less based on the total mass of the ink.

16. The aqueous ink according to claim 1, further comprising a compound represented by the following formula (1): in, In formula (1), R1, R2 and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, each R4 is independently an alkylene group having 2 to 4 carbon atoms, X is a single bond or an alkylene group having 1 to 6 carbon atoms, n is 6 to 24, a is 1 to 3, b is 0 to 2, and a+b=3.

17. The aqueous ink according to claim 16, wherein: The amount of the compound represented by formula (1) contained in the aqueous ink is 0.002 times or more and 0.10 times or less the amount of the titanium oxide particles contained in the aqueous ink in terms of mass ratio. 18 . The aqueous ink according to claim 1 , wherein the pH of the aqueous ink is 7.0 or more and 9.0 or less.

19. An ink cartridge comprising ink; and an ink storage portion storing the ink, It is characterized in that The ink includes the aqueous ink according to claim 1 .

20. An inkjet recording method for recording an image on a recording medium by ejecting ink from an inkjet recording head, It is characterized in that The ink includes the aqueous ink according to claim 1 .