A method for comprehensive utilization of ferrotitanium elements in titanium concentrate

By adding a solid carbonaceous reducing agent to the titanium concentrate and using NH3 for reduction, nitriding, roasting and rusting reactions, the problems of titanium-iron separation efficiency and environmental pollution are solved, and the preparation of high-quality titanium-rich materials and the separation of red mud are achieved. , reduces production costs and waste liquid emissions, and is suitable for industrial applications.

CN115927880BActive Publication Date: 2024-10-18CHONGQING UNIV

Patent Information

Application Number
CN202211713539.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-18
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

In the existing technology, high-calcium magnesium-type ilmenite has low titanium recovery rate, high production cost, serious environmental pollution, and poor titanium-iron separation efficiency and quality, making it difficult to achieve effective comprehensive utilization.

Method used

Low-grade titanium concentrate with a particle size of 100~200 μm is mixed with a solid carbonaceous reducing agent. Through reduction nitriding roasting and rust reaction, NH3 is used as the reducing agent and nitriding agent to prepare loose and porous granular TiNxOy. Then acid leaching is performed to remove impurities and separate high-quality titanium-rich materials and red mud.

Benefits of technology

It improves the separation efficiency and quality of ferrotitanium, reduces production costs, reduces waste liquid discharge, realizes the feasibility of industrial production, simplifies the process, and improves the cleanliness and efficiency of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115927880B_ABST
    Figure CN115927880B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for comprehensively utilizing titanium iron elements in titanium concentrate. The method uses NH3 as the main reducing agent and nitriding agent, uses low-grade titanium concentrate as raw material, and combines the use of solid carbonaceous reducing agent to improve the reduction and nitridation efficiency. The titanium concentrate and the solid carbonaceous reducing agent are mixed and then placed in a rotary tube furnace for roasting. After roasting, the product is treated by a rusting method, and the titanium-rich material and red mud are effectively separated by screening, and then the titanium-rich material is further purified by acid leaching to obtain high-quality TiN x O y . Among them, the raw materials of the roasting process are powdered, eliminating the steps of ball making or briquetting. At the same time, the addition of solid carbonaceous reducing agent greatly improves the reaction efficiency, reduces the amount of NH3 used, lowers the roasting temperature, and shortens the reaction time. The loose and porous granular structure of the roasted product also improves the efficiency of the corrosion reaction. Compared with other traditional methods, the present invention can improve the reaction efficiency and efficiently and cleanly prepare high-quality TiN x O y .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and mainly relates to a method for comprehensively utilizing ferro-titanium elements in titanium concentrate. Technical Background

[0002] my country's titanium resources are mainly high-calcium-magnesium ilmenite in the Panzhihua area. For the comprehensive utilization of this type of ilmenite, the titanium recovery rate of the existing process is only 25%, and there are problems such as difficult selection and smelting, low product quality, and low comprehensive utilization rate. The titanium concentrate separated from the ilmenite is mainly the main raw material for the production of titanium dioxide and sponge titanium. In the current production process, whether it is the sulfuric acid method to produce titanium dioxide or the chlorination method to produce titanium dioxide, this type of natural rutile, artificial rutile or high-titanium slag high-grade titanium-containing raw materials are required. However, the high-calcium-magnesium ilmenite has a low grade and cannot be applied to these methods, so it needs to be prepared into titanium-rich materials first. In the preparation process of titanium-rich materials, the acid leaching method requires a large amount of acid, which will produce a large amount of waste liquid, waste acid and waste acid "three wastes". The "three wastes" will pollute the environment. How to reuse the "three wastes" limits the development of this method. For example, Chinese patents CN104828864A, CN102786082A and CN102146523B are all based on acid leaching as the main method to extract artificial rutile. No matter how to improve the process, a large amount of waste acid is generated. In addition, the electric furnace smelting method has problems such as large energy consumption, large electrode consumption, and serious lining erosion due to the need for smelting reaction at a high temperature of more than 1600 ° C, resulting in high production costs. At the same time, since impurities such as calcium and magnesium cannot be effectively removed, the quality of the titanium-rich material produced is relatively low. In the reaction process of the selective chlorination method, due to the high temperature, impurities such as calcium and magnesium are easily chlorinated, and CaCl2 and MgCl2 cannot be effectively processed in the furnace bottom enriched material, causing boiling deterioration phenomenon to hinder the chlorination reaction from proceeding, resulting in the dead bed phenomenon.

[0003] At present, for the comprehensive utilization process of high-calcium-magnesium ilmenite, the "high-temperature carbonization-low-temperature chlorination" process has industrial prospects and can effectively deal with the problem of the presence of impurities such as calcium and magnesium. Chinese patent CN201811411238.8 discloses that by high-temperature carbonization, the titanium-containing phase is transformed into titanium carbide or titanium carbonitride, so that it can be chlorinated at low temperature, and impurities such as calcium and magnesium will not be chlorinated, which effectively solves the problem of impurities destroying the fluidized state. Therefore, the key to low-temperature selective chlorination lies in the preparation of titanium carbide / carbonitride. However, high-temperature carbonization has problems such as high temperature and high energy consumption, and there is carbon dioxide emission, which is not in line with the development direction of low-carbon smelting. The Chinese invention patent with application number CN202110428145.1 discloses a method for preparing low-temperature titanium chloride slag using low-grade titanium concentrate. The method innovatively proposes that ammonia gas can be used as the main reducing agent and nitriding agent to prepare a main phase of TiN at a temperature of 800~1100 ℃.x O y Low-temperature titanium chloride slag. However, the problem with this method is that the gas-solid reaction efficiency is affected by the density and porosity of the raw materials, and the product is easily sintered at high temperatures, resulting in a decrease in the reaction rate. At the same time, magnetic separation cannot effectively separate titanium iron, which affects the subsequent chlorination.

[0004] The reduction corrosion method can effectively separate titanium iron, and has the characteristics of low cost and low pollution. The Chinese invention patent with application number CN200510032102.2 discloses a method for preparing artificial rutile by reduction-corrosion method using high calcium magnesium type titanium concentrate as raw material, and the grade of TiO2 of the obtained artificial rutile is about 85%. However, the reaction efficiency of the corrosion method is related to the metallization rate of the reduced product and the density and porosity of the structure. The above method has a metallization rate of about 93% for the reduced product, a relatively dense structure, and a low porosity, resulting in low reaction efficiency and a long reaction time during the corrosion process. Summary of the invention

[0005] In view of the above problems existing in the prior art, the technical problem to be solved by the present invention is: how to achieve efficient and low-cost reduction and effective separation of ferrotitanium.

[0006] The present invention provides a method for comprehensively utilizing ferrotitanium in titanium concentrate, comprising the following steps:

[0007] S1: Mix low-grade titanium concentrate with a particle size of 100-200 μm with a solid carbonaceous reducing agent, place it in a rotary atmosphere tubular furnace, and introduce ammonia for reduction nitriding roasting, wherein the molar ratio of solid carbonaceous reducing agent to titanium concentrate is 2-4, the roasting temperature is 1000-1200 ℃, and the roasting time is 0.5-3 h; this step uses NH3 as the main reducing agent and nitriding agent, uses low-grade titanium concentrate as raw material, and combines the use of solid carbonaceous reducing agent to improve the reduction nitriding efficiency. The particle size of titanium concentrate is 100-200 μm, which is conducive to the roasting reaction and the subsequent separation of titanium-rich material and red mud. The product of reduction nitriding is a loose and porous granular structure, which does not require ball milling and other processes and can be directly used for corrosion reaction.

[0008] S2: The cooled reduction nitridation product is subjected to corrosion reaction, the corrosion temperature is 50~70 ℃, the corrosion agent concentration is 1~1.6% NH4Cl, the liquid-solid ratio is 5~10, the stirring rate is 200~400 r / min, and the air flow rate is 1~2 L·min -1 ·m -3 , the corrosion time is 3~6 h;

[0009] S3: After the rusting reaction is finished, the rusting liquid is separated and returned to the rusting reaction; the lower layer material after the rusting reaction is filtered, and the titanium-rich material and red mud are separated using a 400-600 mesh screen, the screened material is the titanium-rich material, and the screened material is the red mud. By using high-calcium-magnesium type low-grade titanium concentrate, high-quality titanium-rich material for low-temperature chlorination is prepared, which can be used as a raw material for low-temperature chlorination, and the separated iron-containing red mud can be used as pigment-grade iron red.

[0010] Specifically, S4: the titanium-rich material obtained by rust separation is subjected to acid leaching to remove the residual trace red mud and calcium and magnesium impurities. The acid leaching uses 5% to 10% HCl, a stirring rate of 100 to 200 r / min, a liquid-solid ratio of 5 to 10, a leaching time of 10 to 30 min, and a leaching temperature of 70 to 90 °C. The main components of the titanium-rich material are TiN x O y After acid leaching, the residual trace red mud and impurities such as calcium and magnesium in the titanium-rich material can be effectively removed to increase TiN x O y The purity of the material makes it suitable for use as a coating or structural material.

[0011] Specifically, the solid carbonaceous reducing agent includes graphite, coke powder, coal powder or biochar.

[0012] Compared with the prior art, the present invention uses NH3 as a reducing agent and a nitriding agent, and the added solid carbonaceous reducing agent can participate in a partial reduction reaction, coupling the reduction reaction into a gas-solid reaction and a solid-solid reaction, which has at least the following beneficial effects:

[0013] 1) Solid carbonaceous reducing agents can participate in the reduction of iron oxides, effectively reducing the amount of NH3 used; the heat released by the solid carbonaceous reducing agent can provide energy for subsequent reactions; the solid carbonaceous reducing agent improves the ability of NH3 to penetrate the material layer, which is beneficial to the mass transfer of the reaction gas. This is because the iron-containing phase generated at high temperature will not undergo serious sintering due to the presence of a large amount of solid carbonaceous reducing agents, maintaining the porosity of the product material layer, which is beneficial to the mass transfer of the reaction gas and further shortening the reaction time.

[0014] 2) The raw materials in the reduction nitriding process do not need to be added with additives and binders, eliminating the processes such as ball making / briquetting and the subsequent crushing and ball milling processes, simplifying the production process and reducing costs.

[0015] 3) The product prepared by reduction nitridation has a loose and porous granular structure, which is conducive to the corrosion reaction. Among the products after corrosion, the phase with larger particle size that cannot pass through the sieve is TiN x O y The smaller particle size, that is, the red mud that passes through the screen, can be separated by simple screening.

[0016] 4) Compared with other publicly patented methods, this method is a method that can be realized in industrial production, with the remarkable characteristics of high reaction efficiency, clean and efficient production process, low waste liquid discharge, etc., and the process flow is simple and has few steps. At the same time, the coordination of the entire process flow greatly reduces the production cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The figure is a simplified flow chart of the method of the present invention. DETAILED DESCRIPTION

[0018] The present invention provides a method for comprehensively utilizing ferrotitanium in titanium concentrate, which specifically comprises the following steps:

[0019] 1) High calcium and magnesium type low-grade titanium concentrate with a particle size of 100-200 μm is mixed with a solid carbonaceous reducing agent, placed in a rotary atmosphere tubular furnace, and ammonia is introduced for reduction nitriding roasting. The roasting temperature is 1000-1200 °C, the roasting time is 0.5-3 h, and the molar ratio of the solid carbonaceous reducing agent to the titanium concentrate is 2-4.

[0020] In specific implementation, the calcination temperature can be 1000°C, 1050°C, 1080°C, 1100°C, 1120°C, 1150°C or 1200°C; the calcination time can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h or 3 h; the molar ratio of the solid carbonaceous reducing agent to the titanium concentrate can be 2, 2.5, 3, 3.5 or 4; the solid carbonaceous reducing agent includes various solid carbonaceous reducing agents such as graphite, coke powder, coal powder or biochar.

[0021] 2) The cooled reduced nitridation product was subjected to corrosion reaction, the corrosion temperature was 50~70 ℃, the corrosion agent concentration was 1~1.6% NH4Cl, the liquid-solid ratio was 5~10, the stirring rate was 200~400 r / min, and the air flow rate was 1~2 L·min -1 ·m -3 , the corrosion time is 3~6 h. After the corrosion reaction is completed, the lower layer of materials after corrosion is filtered, and the titanium-rich material and red mud are separated using a 400~600 mesh sieve. The obtained titanium-rich material can be used as a raw material for low-temperature chlorination, and the red mud can be used as a pigment-grade iron red.

[0022] In a specific implementation, the corrosion temperature can be 50 ℃, 55 ℃, 60 ℃, 65 ℃ or 70 ℃; the concentration of NH4Cl can be 1%, 1.2%, 14% or 1.6%; the liquid-solid ratio can be 5, 6, 7, 8, 9 or 10; the stirring rate can be 200 r / min, 250 r / min, 300 r / min, 350 r / min or 400 r / min; the air flow rate can be 1 L·min -1 ·m -3 、1.5 L·min -1 ·m -3 or 2 L min -1 ·m -3 ; The corrosion time can be 3 h, 4 h, 5 h or 6 h; The screen can be 400 mesh, 500 mesh or 600 mesh.

[0023] 3) The titanium-rich material separated by rust is subjected to acid leaching to remove the residual trace red mud and impurities such as calcium and magnesium. The acid leaching uses HCl with a concentration of 5%~10%, a stirring rate of 100~200 r / min, a liquid-solid ratio of 5~10, a leaching time of 10-30 min, and a leaching temperature of 70~90 ℃.

[0024] In a specific implementation, the concentration of HCl can be 5%, 6%, 7%, 8%, 9% or 10%; the stirring rate can be 100 r / min, 150 r / min or 200 r / min; the liquid-solid ratio can be 5, 6, 7, 8, 9 or 10; the leaching time can be 10 min, 20 min or 30 min; and the leaching temperature can be 70 °C, 80 °C or 90 °C.

[0025] The present invention will be further described below in conjunction with the embodiments.

[0026] Example 1: Panzhihua low-grade titanium concentrate was used as raw material, and its main chemical components are shown in Table 1.

[0027] Table 1 Main chemical components of titanium concentrate

[0028] <![CDATA[TiO2]]> FeO <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO MnO <![CDATA[V2O5]]> S P other 46.82 34.52 6.10 5.66 3.23 1.00 0.84 0.635 0.058 0.14 <0.005 0.99

[0029] This embodiment adopts a method for comprehensive utilization of ferro-titanium in titanium concentrate defined in the present invention, and the specific steps are as follows:

[0030] Low-grade titanium concentrate with a particle size of 100-200 μm was mixed with graphite, placed in a rotary atmosphere tubular furnace, and ammonia was introduced for reduction nitridation roasting. The molar ratio of graphite to titanium concentrate was 3. The roasting temperature was 1200 °C and the roasting time was 3 h.

[0031] The cooled reduced nitridation product was subjected to corrosion reaction at a corrosion temperature of 70 °C, a corrosion agent concentration of 1.6% NH4Cl, a liquid-to-solid ratio of 10, a stirring rate of 400 r / min, and an air flow rate of 2 L·min -1 ·m -3 , the corrosion time is 6 h. After the corrosion reaction is completed, the lower layer of materials after the corrosion reaction is filtered, and the titanium-rich material and red mud are separated using a 400-mesh sieve. Table 2 shows the main chemical components of the titanium-rich material after corrosion separation, and Table 3 shows the main chemical components of the red mud.

[0032] Table 2 Main chemical composition of titanium-rich material after rust separation

[0033] <![CDATA[TiN x THE y ]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 84.40 5.39 4.69 2.36 1.11 1.20 0.85

[0034] Table 3 Main chemical components of red mud

[0035] <![CDATA[TiN x Ltd.]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 3.69 94.63 0.88 0.13 0.28 0.18 0.21

[0036] The titanium-rich material separated by rust was acid-leached to remove the residual trace red mud and impurities such as calcium and magnesium. The acid leaching used 10% HCl, a stirring rate of 200 r / min, a liquid-solid ratio of 10, a leaching time of 30 min, and a leaching temperature of 90 °C. Finally, the TiN obtained was filtered, washed, and dried. x O y The purity is 97.21%.

[0037] Example 2

[0038] This embodiment provides a method for comprehensively utilizing ferro-titanium in titanium concentrate, using the Panzhihua low-grade titanium concentrate described in Example 1 as a raw material, and the specific steps are as follows:

[0039] Low-grade titanium concentrate with a particle size of 100-200 μm was mixed with coke powder, placed in a rotary atmosphere tubular furnace, and ammonia was introduced for reduction nitridation roasting. The molar ratio of coke powder to titanium concentrate was 4. The roasting temperature was 1150 °C and the roasting time was 2 h.

[0040] The cooled reduced nitridation product was subjected to corrosion reaction at a corrosion temperature of 60 °C, a corrosion agent concentration of 1.6% NH4Cl, a liquid-to-solid ratio of 5, a stirring rate of 300 r / min, and an air flow rate of 1.5 L·min -1 ·m -3 , the corrosion time is 5 h. After the corrosion reaction is completed, the lower layer of materials after corrosion is filtered, and the titanium-rich material and red mud are separated using a 400-mesh sieve. Table 4 shows the main chemical components of the titanium-rich material after corrosion separation, and Table 5 shows the main chemical components of the red mud.

[0041] Table 4 Main chemical composition of titanium-rich material after rust separation

[0042] <![CDATA[TiN x Ltd.]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 83.39 5.74 4.83 3.12 1.02 0.98 0.92

[0043] Table 5 Main chemical components of red mud

[0044] <![CDATA[TiN x Ltd.]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 3.83 93.97 0.93 0.17 0.32 0.21 0.57

[0045] The titanium-rich material separated by rust was acid-leached to remove the residual trace red mud and impurities such as calcium and magnesium. The acid leaching used 5% HCl, a stirring rate of 150 r / min, a liquid-solid ratio of 5, a leaching time of 20 min, and a leaching temperature of 80 °C. Finally, the TiN obtained by filtration, washing, and drying x O y The purity is 96.37%.

[0046] Example 3

[0047] This embodiment provides a method for comprehensively utilizing ferro-titanium in titanium concentrate, using the Panzhihua low-grade titanium concentrate described in Example 1 as a raw material, and the specific steps are as follows:

[0048] Low-grade titanium concentrate with a particle size of 100-200 μm was mixed with coal powder, placed in a rotary atmosphere tubular furnace, and ammonia was introduced for reduction nitridation roasting. The molar ratio of coal powder to titanium concentrate was 2.5. The roasting temperature was 1100 °C and the roasting time was 3 h.

[0049] The cooled reduced nitridation product was subjected to corrosion reaction at a corrosion temperature of 50 °C, a corrosion agent concentration of 1.6% NH4Cl, a liquid-to-solid ratio of 8, a stirring rate of 200 r / min, and an air flow rate of 1 L·min -1 ·m -3 , the corrosion time is 4 h. After the corrosion reaction is completed, the lower layer of materials after corrosion is filtered, and the titanium-rich material and red mud are separated using a 600-mesh sieve. Table 6 shows the main chemical components of the titanium-rich material after corrosion separation, and Table 7 shows the main chemical components of the red mud.

[0050] Table 6 Main chemical composition of titanium-rich material after rust separation

[0051] <![CDATA[TiN x Ltd.]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 83.37 5.93 4.73 2.94 1.05 0.98 1.00

[0052] Table 7 Main chemical components of red mud

[0053] <![CDATA[TiN x Ltd.]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 2.98 94.48 0.87 0.21 0.34 0.24 0.88

[0054] The titanium-rich material separated by rust was acid-leached to remove the residual trace red mud and impurities such as calcium and magnesium. The acid leaching used 8% HCl, a stirring rate of 100 r / min, a liquid-solid ratio of 5, a leaching time of 15 min, and a leaching temperature of 75 °C. Finally, the TiN obtained was filtered, washed, and dried. x O y The purity is 96.72%.

[0055] Example 4

[0056] This embodiment provides a method for comprehensively utilizing ferro-titanium in titanium concentrate, using the Panzhihua low-grade titanium concentrate described in Example 1 as a raw material, and the specific steps are as follows:

[0057] Low-grade titanium concentrate with a particle size of 100-200 μm was mixed with biochar, placed in a rotary atmosphere tubular furnace, and ammonia was introduced for reduction nitridation roasting. The molar ratio of biochar to titanium concentrate was 3. The roasting temperature was 1150 °C and the roasting time was 2 h.

[0058] The cooled reduced nitridation product was subjected to corrosion reaction at a corrosion temperature of 65 °C, a corrosion agent concentration of 1.2% NH4Cl, a liquid-solid ratio of 5, a stirring rate of 300 r / min, and an air flow rate of 1.5 L·min -1 ·m -3 , the corrosion time is 3 h. After the corrosion reaction is completed, the lower layer of materials after corrosion is filtered, and the titanium-rich material and red mud are separated using a 600-mesh sieve. Table 8 shows the main chemical components of the titanium-rich material after corrosion separation, and Table 9 shows the main chemical components of the red mud.

[0059] Table 8 Main chemical composition of titanium-rich material after rust separation

[0060] <![CDATA[TiN x Ltd.]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 82.41 6.37 5.13 2.48 1.23 1.12 1.26

[0061] Table 9 Main chemical components of red mud

[0062] <![CDATA[TiN x Ltd.]]> <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO other 2.34 95.41 0.97 0.26 0.31 0.29 0.42

[0063] The titanium-rich material separated by rust was acid-leached to remove the residual trace red mud and impurities such as calcium and magnesium. The acid leaching used 10% HCl, a stirring rate of 150 r / min, a liquid-solid ratio of 5, a leaching time of 20 min, and a leaching temperature of 80 °C. Finally, the TiN obtained by filtration, washing, and drying x O y The purity is 97.13%.

Claims

1. A method for comprehensive utilization of ferrotitanium in titanium concentrate, Features: The low-grade titanium concentrate with a particle size of 100 to 200 μm is mixed with a solid carbonaceous reducing agent, placed in a rotary atmosphere tubular furnace, and ammonia gas is introduced for reduction nitridation roasting, wherein the molar ratio of the solid carbonaceous reducing agent to the titanium concentrate is 2 to 4, the roasting temperature is 1000 to 1200° C., and the roasting time is 0.5 to 3 hours; The cooled reduced nitrided product is subjected to corrosion reaction at a temperature of 50-70°C and a corrosion agent concentration of 1-1.6% NH 4 Cl, liquid-to-solid ratio is 5-10, stirring rate is 200-400r / min, air flow rate is 1-2L·min -1 ·m -3 , the corrosion time is 3 to 6 hours; After the corrosion reaction is completed, the corrosion liquid is separated and returned to the corrosion reaction; the lower layer material after the corrosion reaction is filtered, and the titanium-rich material and the red mud are separated by a 400-600 mesh sieve, the material on the sieve is the titanium-rich material, and the material under the sieve is the red mud; The titanium-rich material obtained by rust separation is subjected to acid leaching to remove residual trace red mud and calcium and magnesium impurities. The acid leaching uses HCl with a concentration of 5% to 10%, a stirring rate of 100 to 200 r / min, a liquid-to-solid ratio of 5 to 10, a leaching time of 10 to 30 minutes, and a leaching temperature of 70 to 90°C.

2. The method for comprehensive utilization of ferrotitanium in titanium concentrate according to claim 1, Features: The solid carbonaceous reducing agent includes graphite, coke powder, coal powder or biochar.

Citation Information

Patent Citations

  • Method for preparing titanium dioxide and ferric oxide from ilmenite

    CN102146523B

  • Method for preparing artificial rutile

    CN102786082A

  • Titanium carbonitride preparing method

    CN109399585A

  • A method for preparing low-temperature titanium chloride slag from low-grade titanium concentrate

    CN113088683B

  • Method of preparing synthetic rutile from ore type ilmenite concentrate

    CN1923703A

Cited By

  • Method for reducing and nitriding carbon-ammonia synergistically reinforced low-grade titanium concentrate

    CN121700200A