Ultra-thin ultra-low density films for EUV lithography
Through the interconnection network structure formed by multiple carbon nanofibers, the problem of difficult to take into account the transmittance and robustness of the EUV protective layer at high temperature and high mechanical strength is solved, and the combination of high EUV transmittance and mechanical robustness is achieved, satisfying the Technical requirements for EUV lithography.
Patent Information
- Application Number
- CN202180047759.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-16
- Filing Date
- 2021-09-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-09-15
AI Technical Summary
The existing EUV protective layer is difficult to take into account both high transmittance and mechanical robustness under the requirements of high temperature and high mechanical strength. The poor structural structure of the carbon nanotube film leads to the transmission ratio not meeting industry standards.
Using multiple carbon nanofibers to form a planar-oriented interconnection network structure, including at least 50% double-walled carbon nanofibers, ultra-thin ultra-low density nanostructure membranes are prepared by filtration to achieve the combination of high EUV transmittance and mechanical strength. .
The EUV transmittance is achieved above 92% or 98%, and it also has temperature tolerance and low deflection above 600℃, meeting the mechanical robustness requirements of EUV lithography.
Smart Images

Figure CN115943346B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates generally to thin films and thin film devices used in semiconductor microchip fabrication, and more particularly to ultra-thin ultra-low density nanostructured free-standing pellicle films for extreme ultraviolet (EUV) lithography. Background Art
[0002] A protective covering is a protective covering that covers a photomask and is used in semiconductor microchip manufacturing. A photomask may refer to an opaque plate with holes or transparent portions that allow light to pass through in a defined pattern. Such photomasks are commonly used in the production of photolithography and integrated circuits. A photomask is used as a master template to create a pattern on a substrate, which is typically a thin slice of silicon, known as a wafer in the case of semiconductor chip manufacturing.
[0003] Particle contamination can be a serious problem in semiconductor manufacturing. The photomask is protected from particles by a sheath, which is a thin transparent film stretched over a frame attached over the patterned side of the photomask. The sheath is close to the mask, but far enough away that medium to small sized particles that land on the sheath will be too far out of focus to be printed. Recently, the microchip manufacturing industry has realized that the sheath can also protect the photomask from damage from causes other than particles and contaminants.
[0004] Extreme ultraviolet lithography is an advanced optical lithography technology that uses a certain range of EUV wavelengths (more specifically, 13.5nm wavelengths). It enables semiconductor microchip manufacturers to pattern the most sophisticated features at 7nm resolution and greater, and place more transistors without increasing the size of the required space. The working principle of the EUV photomask is to reflect light, and the reflection of light is achieved by using multiple alternating layers of molybdenum and silicon. When the EUV light source is turned on, the EUV light first illuminates the protective layer, passes through the protective layer, and then reflects back from under the photomask, illuminates the protective layer again, and then continues to print out the microchip. Some energy is absorbed during this process and heat can be generated, absorbed and accumulated. The temperature of the protective layer can be raised to any temperature from 600°C to 1000°C or above 1000°C.
[0005] While heat resistance is important, the overcoat must also be very transparent to EUV to ensure that reflected light and the light pattern from the photomask pass through.
[0006] After decades of research and efforts, a polysilicon-based EUV overlay was developed in 2016, where a simulated relatively low-power 175-watt EUV source had only 78% EUV transmission. As transistor density requirements increase, stringent requirements have placed EUV overlay developers under more technical challenges, such as higher transmittance, lower transmittance variation, higher temperature tolerance, and strong mechanical strength.
[0007] Although efforts have been made to achieve higher light transmittance by deploying high content of single-walled carbon nanotubes (e.g., up to 98% by mass) in carbon nanotube sheets, these efforts have resulted in poor product structure, which in turn leads to reduced mechanical strength and / or durability. Therefore, such carbon nanotube-based films must have a certain degree of thickness to support their structural integrity. Therefore, the EUV transmittance of such carbon nanotube-based films still does not meet industry standards. Therefore, conventional technology has limited further development of the transmittance of EUV light and the thickness of the protective layer film. Summary of the invention
[0008] According to one aspect of the present disclosure, a nanostructured film of a special structure is disclosed, wherein the nanostructured film comprises a plurality of carbon nanofibers, wherein the plurality of carbon nanofibers are randomly crossed to form an interconnected network structure oriented in a plane, wherein the interconnected network structure has a thickness ranging from a lower limit of 3 nm to an upper limit of 100 nm and a minimum EUV transmittance of 92% or higher, wherein the plurality of carbon nanofibers comprises at least 50% double-walled carbon nanofibers.
[0009] According to another aspect of the present disclosure, in some embodiments, the thickness is within the range of the lower limit of 3 nm to the upper limit of 40 nm.
[0010] According to another aspect of the present disclosure, in some embodiments, the thickness is within the range of the lower limit of 3 nm to the upper limit of 20 nm.
[0011] According to yet another aspect of the present disclosure, in some embodiments, the average thickness of the interconnected network structure is 11 nm.
[0012] According to further aspects of the present disclosure, in some embodiments, EUV transmittance rises above 95%.
[0013] According to yet another aspect of the present disclosure, in some embodiments, EUV transmittance rises above 98%.
[0014] According to another aspect of the present disclosure, the plurality of carbon nanofibers further include single-walled carbon nanotubes and multi-walled carbon nanotubes, and the number of walls of the single-walled carbon nanotubes is one, the number of walls of the double-walled carbon nanotubes is two, and the number of walls of the multi-walled carbon nanotubes is three or more.
[0015] According to another aspect of the present disclosure, the percentage of single-walled carbon nanotubes to all carbon nanotubes is between 20% and 40%, the percentage of double-walled carbon nanotubes to all carbon nanotubes is 50% or more, and the remaining carbon nanotubes are multi-walled carbon nanotubes.
[0016] According to another aspect of the present disclosure, the single-walled carbon nanotubes account for more than 20% but less than 50% of all carbon nanotubes, the double-walled carbon nanotubes account for more than 75% of all carbon nanotubes, and the remaining carbon nanotubes are multi-walled carbon nanotubes accounting for the remaining percentage of all carbon nanotubes.
[0017] According to another aspect of the present disclosure, the difference between any two EUV transmission measurements from the same nanostructure film at any focal region is less than 5%.
[0018] According to another aspect of the present disclosure, the difference between any two EUV transmission measurements from the same nanostructure film at any focal region is less than 2%.
[0019] According to another aspect of the present disclosure, the difference between any two EUV transmission measurements from the same nanostructure film at any focal region is less than 0.4%.
[0020] According to another aspect of the present disclosure, the network has a deflection of less than 3.5 mm at a constant 2Pa pressure, at a flow rate of 10sccm, at a flow rate of 8sccm, at 3.5mbar (millibar) / second or under any scanner conditions, particularly when used in EUV lithography applications or lithography scanners.
[0021] According to another aspect of the present disclosure, the deflection is less than 0.6 mm at a constant 2 Pa pressure, at a flow rate of 10 sccm, at a flow rate of 8 sccm, at 3.5 mbar / sec, or under any scanner conditions.
[0022] According to another aspect of the present disclosure, for a full size EUV shield (approximately 110x144mm, with a gap of 2.5mm with the mask in the scanner), the network has a deflection of less than 0.1mm when subjected to an evacuation speed of 3.5mbar / sec, particularly when used in EUV lithography applications or lithography scanners.
[0023] According to another aspect of the present disclosure, the network has a deflection of less than 0.1 mm at a flow rate of 3.5 mbar / sec.
[0024] According to another aspect of the present disclosure, the network produces less than 0.3% scattering under EUV radiation.
[0025] According to another aspect of the present disclosure, the nanofibers are conformally coated with a metal, metal oxide, or nitride, the metal being selected from boron, ruthenium, zirconium, niobium, molybdenum, rubidium, yttrium, strontium, or rhodium.
[0026] According to another aspect of the present disclosure, the nanostructured film has a viscosity of about 0.2 μg / cm 2 To about 6.0μg / cm 2 Surface density.
[0027] According to one aspect of the present disclosure, a sheath is disclosed. The sheath comprises: a sheath boundary, the sheath boundary defining an orifice; and at least one nanostructure film, the at least one nanostructure film disposed to the sheath boundary and covering the orifice.
[0028] According to another aspect of the present disclosure, a method of performing EU lithography is disclosed. The method includes transmitting EUV radiation through a protective layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The present disclosure is further described by way of non-limiting examples of preferred embodiments thereof in the following detailed description with reference to the several drawings wherein like characters represent like elements throughout the several views of the drawings.
[0030] Figure 1 A filtration method for forming a sheath membrane according to an exemplary embodiment is shown.
[0031] Figure 2 Different types of CNT compositions and their mechanical properties in Samples A to I according to exemplary embodiments are shown.
[0032] FIG. 3(A) shows a scanning electron microscope (SEM) image of a microstructure of a DWCNT film according to an exemplary embodiment.
[0033] FIG. 3(B) illustrates areal density according to an exemplary embodiment.
[0034] FIG. 4(A) shows the transparency and absorbance of DWCNT films having different areal densities at 550 nm according to example embodiments.
[0035] FIG. 4(B) shows the effect of areal density on the deflection and permeability of a DWCNT film of size 25×25 mm at 2 Pa and at fracture, according to an exemplary embodiment.
[0036] FIG4(C) shows the DWCNT / MWCNT ratio for 25x25 mm and areal density of 2.9 to 3.0 μg / cm 2 Effect of the film deflection of the CNT film at 2 Pa and at fracture.
[0037] FIG. 4(D) shows a 110×140 mm and areal density of 0.65 μg / cm during evacuation at a maximum rate of 3.5 mbar / sec according to an exemplary embodiment. 2 The deflection of the membrane.
[0038] FIG. 4(E) shows the effect of various DWCNT / MWCNT ratios on the fracture pressure of CNT films.
[0039] FIG. 5(A) shows a 1×1 cm 2 Two 0.6μg / cm 2 Linear plot of the EUV transparency of the film.
[0040] FIG. 5(B) shows a 1×1 cm 2 Two 0.6μg / cm 2 Linear plot of the EUV reflectivity of the film.
[0041] FIG. 6(A) shows a set of bar graphs indicating CNT bundle diameters for different samples of films where DWCNTs are the predominant constituent, according to an exemplary embodiment.
[0042] FIG. 6(B) shows a set of bar graphs indicating the major pore axes of different samples of membranes where DWCNTs are the major constituent, according to an exemplary embodiment. DETAILED DESCRIPTION
[0043] The embodiments and / or specific features or subcomponents of the present disclosure are intended to bring about one or more of the advantages specifically described above and pointed out below, through one or more of the various aspects of the present disclosure.
[0044] A protective layer may refer to a thin transparent membrane that protects a photomask during the production of a semiconductor microchip. The protective layer may be used as a dust cover to prevent particles and contaminants from falling onto the photomask during production. However, the protective layer must be transparent enough to allow light to be transmitted to perform photolithography. A higher degree of light transmission is desired to make photolithography more effective.
[0045] Furthermore, overcoats for EUV lithography require large (e.g., greater than 110x140 mm), freestanding thin film materials with extremely unique properties. In addition to high transparency to EUV radiation, the overcoat needs to withstand temperatures above 600°C and be mechanically robust to survive handling, transport, evacuation, and exhaust during the lithography process. It is also desirable to be gas permeable but have the ability to retain micron-sized particles. Given the high level of properties required, it is generally difficult to produce effective EUV overcoats.
[0046] In this regard, carbon nanotubes have been proposed as possible starting materials to form overcoats for such EUV overcoat applications due to their excellent thermal and mechanical properties and ability to form porous films.
[0047] Carbon nanotubes and carbon nanotube films
[0048] Carbon nanotubes (CNTs) generally have several different types, including but not limited to single-walled CNTs (SWCNTs), double-walled CNTs (DWCNTs), multi-walled CNTs (MWCNTs) and coaxial nanotubes. These carbon nanotubes can exist essentially in one type alone or often in combination with other types. A single CNT can intersect with several other CNTs. Many CNTs can form a network of independent microstructured films together. Although such formation is possible, it is not guaranteed that every trial will be successful, especially when making ultra-thin films with high EUV transparency. As the name implies, SWCNTs have one or a single wall, DWCNTs have two walls and MWCNTs have three or more walls.
[0049] Furthermore, among several possible methods for making stand-alone films, a filtration-based approach is utilized to produce films ranging from small-sized films to sufficiently large and uniform films for EUV shields. This filtration-based approach allows for rapid production of not only CNT films, but also other high-aspect-ratio nanoparticle and nanofiber films, such as boron nitride nanotubes (BNNTs) or silver nanowires (AgNWs). Since this approach separates the nanoparticle synthesis process from the film fabrication process, various types of nanotubes produced by almost any method can be used. Different types of nanotubes can be mixed in any desired ratio. Filtration is also a promising candidate for producing very uniform films, since filtration is a self-leveling process in the sense that non-uniformities in film thickness are automatically corrected by changes in local permeability during the filtration process and is therefore a very desirable film formation process.
[0050] Figure 1 A filtration method for forming a sheath membrane according to an exemplary embodiment is shown.
[0051] like Figure 1 As shown in , a stand-alone carbon nanotube-based sheath membrane can be produced via a filtration-based method. In operation 101, a catalyst is removed from carbon nanotubes (CNTs) that will be used to form a water-based suspension. In an example, the CNTs can be chemically purified to reduce the concentration of catalyst particles to less than 1% or preferably less than 0.5% by weight (as measured by thermogravimetric analysis) before being dispersed into the suspension. The removal of the catalyst is not limited to any particular process or procedure, so that any suitable process can be used to achieve the desired results.
[0052] In operation 102, a water-based suspension is prepared using purified CNTs so that the purified CNTs are uniformly dispersed in the water-based suspension. When preparing one or more CNT suspensions, the carbon nanotube material can be mixed with a selected solvent to uniformly distribute the nanotubes in the final solution as a suspension. Mixing can include mechanical mixing (e.g., using a magnetic stirring bar and a stirring plate), ultrasonic agitation (e.g., using an immersion ultrasonic probe) or other methods. In some examples, the solvent can be a proton or aproton polar solvent, such as water, isopropyl alcohol (IPA) and a water-containing alcohol mixture, such as 60%, 70%, 80%, 90%, 95% IPA, N-methyl-2-pyrrolidone (NMP), dimethyl sulfide (DMS) and combinations thereof. In an example, a surfactant may also be included to help disperse the carbon nanofibers uniformly in the solvent. Examples of surfactants include, but are not limited to, anionic surfactants.
[0053] The carbon nanofiber membrane is usually formed from one of MWCNTs, DWCNTs or SWCNTs. The carbon nanofiber membrane may also contain a mixture of different types of CNTs (ie, SWCNTs, DWCNTs and / or MWCNTs), wherein the ratio between the different types of CNTs is variable.
[0054] Each of the three different types of carbon nanotubes (MWCNT, DWCNT, and SWCNT) has different properties. In one example, single-walled carbon nanotubes can be more conveniently dispersed in a solvent (i.e., most of the nanotubes are suspended individually and do not adsorb to other nanotubes) to subsequently form a sheet of randomly oriented carbon nanotubes. This ability to evenly disperse individual nanotubes in a solvent can in turn produce a more planar, uniform nanotube film formed by removing solvent from the suspended nanofibers. This physical uniformity can also improve the uniformity of properties (e.g., transparency to radiation) throughout the film.
[0055] As used herein, the term "nanofiber" means a fiber having a diameter of less than 1 μm. As used herein, the terms "nanofiber" and "nanotube" are used interchangeably and encompass single-walled carbon nanotubes, double-walled carbon nanotubes, and / or multi-walled carbon nanotubes in which carbon atoms are linked together to form a cylindrical structure.
[0056] In an example, the water-based CNT suspension initially formed in operation 102 may have a SWCNT purity of at least greater than 85%. The remainder may be a mixture of DWCNT, MWCNT, and / or catalyst. In other examples, dispersed CNT suspensions having various ratios of different types of CNTs may be prepared, such as about 20% / 75% DWCNT / SWCNT, about 50% / 45% DWCNT / SWCNT, about 70% / 20% DWCNT / SWCNT, with MWCNT accounting for the remainder. In an example, an anionic surfactant may be used as a catalyst in the suspension.
[0057] In operation 103, the CNT suspension is then further purified to remove polymerized or bonded CNTs from the initial mixture. In an example, different forms of CNTs, whether undispersed or polymerized CNTs or fully dispersed CNTs, can be separated from the suspension via centrifugation. Centrifugation of the carbon nanotubes suspended by the surfactant can help reduce the turbidity of the suspension solution and ensure that the carbon nanotubes are fully dispersed in the final suspension solution before entering the next filtration step. However, aspects of the present disclosure are not limited thereto, such that other separation methods or processes can be utilized.
[0058] In operation 104, the CNT supernatant from operation 103 is then filtered through a filtration membrane to form a CNT mesh, which is a continuous film of interdigitated CNTs.
[0059] In an example, a technique for making a CNT membrane uses water or other fluids to deposit nanotubes in a random pattern on a filter. A mixture containing uniformly dispersed CNTs is allowed to pass or forced through the filter, leaving a nanotube structure layer on the surface of the filter. The size and shape of the resulting membrane are determined by the size and shape of the desired filtration area of the filter, while the thickness and density of the membrane are determined by the amount of nanotube material utilized during the process and the permeability of the filter membrane to the components of the input material, because the permeable components are captured on the surface of the filter. If the concentration of the nanotubes dispersed in the fluid is known, the mass of the nanotubes deposited on the filter can be determined based on the amount of fluid passing through the filter, and the surface density of the membrane is determined by dividing the mass of the nanotubes by the total filtration area. The selected filter is usually impermeable to any CNTs.
[0060] The CNT membrane formed by filtration can be a combination of SWCNTs, DWCNTs and / or MWCNTs in different compositions.
[0061] The CNT film is then detached from the filter membrane in operation 105. More specifically, the carbon nanofibers may randomly cross to form an interconnected network structure in a planar orientation to form a thin CNT film.
[0062] In operation 106, the raised CNT film is then harvested using a harvester frame, and the CNT film is then directly transferred and placed on almost any solid substrate, such as a sheath boundary with a defined orifice. The CNT film can be placed on the sheath boundary and cover the orifice to form a sheath. A transfer film placed on a metal frame or silicon frame with an opening as small as 1x1 cm may be useful. Larger size films are very desirable for actual EUV scanners. CNT film characterization, such as its mechanical strength, deflection testing, permeability testing, deflection under constant pressure or during evacuation conditions, can be performed. Full-size sheaths for EUV lithography scanning may require ultra-thin stand-alone films, which are typically larger than 110x140mm based on current industry standards.
[0063] Exemplary embodiments of the present disclosure encompass filtered CNT sheath films having compositions different from known prior art while exhibiting properties that meet or exceed EUV lithography requirements including, but not limited to, EUV transmittance (EUVT), EUVT uniformity, low deflection, and mechanical strength under pressure changes.
[0064] This composition of the cover film provides an ultra-thin cover film that allows for very high EUVT (e.g., greater than 92%, 95%, or even 98%) while being extremely temperature resistant (e.g., withstanding temperatures greater than 600° C.) and mechanically robust. In an example, the minimum EUVT may be a value of 92% or greater.
[0065] Although the above noted disclosure is provided with reference to CNTs and aqueous solutions, aspects of the present disclosure are not so limited, such that different nanotubes, such as boron nitride nanotubes (BNNTs), may be utilized according to the same principles.
[0066] The above-mentioned thin film can also be conformally coated by various methods, including but not limited to electron beam, chemical vapor deposition, atomic layer deposition, spin coating, dip coating, spray coating, sputtering, DC sputtering and RF sputtering. The material can be a metallic element, including any of the following: silicon, SiO2, SiON, boron, ruthenium, boron, zirconium, niobium, molybdenum, rubidium, yttrium, YN, Y2O3, strontium and / or rhodium. The material can also be any of a metal, a metal oxide or a nitride. However, aspects of the present disclosure are not limited thereto, so that a combination of materials can be used when coating.
[0067] CNT sheath microstructure
[0068] In order to analyze the microstructure of the CNT sheath film, a carbon nanotube film sample was prepared according to the standard transmission electron microscope (TEM) sample preparation guide. The resulting high-resolution transmission electron micrograph (HRTEM) was analyzed. A typical image with a 700K magnification can show one CNT to eight CNTs. The DiameterJ plug-in tool of the National Institute of Standards and Technology or a similar analysis tool is used to study the HRTEM image. The number of walls of each CNT is counted. Exemplary results and other measurements are presented in Table 1 provided below.
[0069] Table 1
[0070] wall# Sample 1 Sample 2 Sample 3 Sample 4 1 25.0% 38.0% 40.0% 21.6% 2 73.0% 57.0% 51.0% 76.5% ≥3 2.0% 5.0% 9.0% 1.0%
[0071] As shown above, each of the CNT sheath film samples exhibited a DWCNT composition of about 51% or more, with the remainder being formed by a combination of SWCNTs and MWCNTs. The average percentage of DWCNTs for all four samples was equal to a value greater than 60%.
[0072] In another test, the CNT sheath film exhibited more than 20% SWCNTs, more than 75% DWCNTs, with the remainder formed by MWCNTs.
[0073] In addition to the above, it should be noted that the percentage of SWCNTs may be 20% to 40% of all CNTs included in the CNT sheath film, and the percentages of DWCNTs and MWCNTs are more than 50% and less than 10% of all carbon nanotubes, respectively.
[0074] Exemplary analysis results of samples A to G ( Figure 2 ) indicates that DWCNTs have the best mechanical strength when they account for more than 50% of the total CNT content. More specifically, Figure 2 Samples A to G show the mechanical property values of CNT sheath films dominated by DWCNTs.
[0075] like Figure 2 As shown in , the DWCNT-dominated CNT sheath film provides significantly higher fracture pressure values than the SWCNT sheath film (see Sample H). More specifically, the DWCNT-dominated CNT sheath film includes fracture pressure values ranging from about 136.0 Pa to 203.6 Pa, while the SWCNT sheath film has a fracture pressure of 66.6 Pa, which is less than half of the lowest fracture pressure value of the DWCNT-dominated CNT sheath film.
[0076] In addition, Figure 2It can also be seen in the graphs that the DWCNT-dominated CNT sheath film exhibits significantly lower deflection values at a pressure of 2 Pa. In one case, the deflection value of the DWCNT-dominated CNT sheath film sample (0.047 mm) is almost half of the deflection value of the SWCNT sheath film (0.097 mm). The lower deflection value allows the CNT sheath film to fit within the allowable space of the EUV lithography scanner.
[0077] Finally, Figure 6(A) (200K magnification) shows a set of bar graphs indicating the diameters of different samples of membranes with DWCNTs as the main constituent, according to an exemplary embodiment. Figure 6(B) (100K magnification) shows a set of bar graphs indicating the main pore axes of different samples of membranes with DWCNTs as the main constituent, according to an exemplary embodiment.
[0078] Figures 6(A) and 6(B) show exemplary distributions of various CNT bundle diameters and pore diameters of various DWCNT-based membrane samples based on SEM image analysis. As shown in Figure 6(A), the average bundle diameters of the three individual samples were 18.7±10.5nm, 12.8±6.9nm, and 12.1±7.5nm, respectively. In addition, as shown in Figure 6(B), the average pore diameters of the three individual samples were 38.911±35.011nm, 42.286±36.826nm, and 40.535±35.906nm, respectively.
[0079] Film thickness
[0080] The exemplary embodiments of the present disclosure were further analyzed to learn their thickness, which is critical to determining and ensuring high EUVT. More specifically, the Dimension Icon AFM instrument was first calibrated against a National Institute of Standards and Technology (NIST) traceable standard. A CNT sheath film with an area of approximately 90μm x 90μm was selected for AFM 2D and 3D height imaging. Step height analysis was performed to measure film thickness. Three measurements were taken on three carbon nanotube film samples, with readings of 11.8nm, 10.6nm, and 11.4nm, respectively. The average thickness of the test object was approximately 11.3±0.6nm.
[0081] Furthermore, based on further measurement sets, thickness values in the ranges of 3 nm to 100 nm, 3 nm to 40 nm and 3 nm to 20 nm are provided.
[0082] In addition, in other samples, the thickness value may also be within the range of 3nm to 100nm, 3nm to 40nm, and 3nm to 20nm. However, aspects of the present application are not limited thereto, such that the range may have a lower limit of 3nm to 5nm and an upper limit of 20nm to 100nm.
[0083] Given that DWCNT-dominated CNT sheath films exhibit higher mechanical strength, DWCNT-dominated CNT sheath films can be constructed to be extremely thin, allowing for higher EUVT values for use in EUV scanners without sacrificing mechanical strength or integrity.
[0084] Visible and EUV transmittance
[0085] The EUV transmittance of the sample is measured at the current industry standard of 13.5 nm wavelength. An EUVT map is formed based on the EUV scan results to show and measure the variation and / or uniformity of the transmittance.
[0086] EUV transmittance measurement and protective layer lifetime test were performed on the samples under high-intensity EUV radiation. EUV radiation was performed at a radiation intensity of 5.1W / cm 2 The above radiation intensity is equivalent to the intensity of a 250W light source acting on an EUV mask. The total EUV dose in this test is 73kJ / cm 2 , this dose is approximately equivalent to processing 14,000 wafers.
[0087] The CNT sheath film formed by filtration exhibits a high EUV transmittance of approximately above 92%, with results in some instances being above 95% or exceeding 98%. For example, see Figure 5(A). For example, a cross-sample scan of a full-size sheath film (approximately 110mm x 144mm) exhibits an average transmittance of 96.69±0.15%, while scanning a central area of 1.5mm x 1.5mm produces an average transmittance of 96.75±0.03%. Extremely strict criteria for evaluating EUVT uniformity are used to calculate the difference between any two EUVT measurements from the same nanostructure film at any focal area. This requirement may be less than 5%, less than 2%, or even less than 1.0% or lower. For the full-size sheath of this exemplary embodiment, the multi-point EUVT uniformity test results (100 point measurements per sample) exhibit some slight variations of less than 1.5%, less than 0.9%, 0.6%, or less than 0.4%.
[0088] FIG. 5 shows EUV transparency, reflectivity, and scattering of a CNT sheath film formed by filtration according to an exemplary embodiment. More specifically, FIG. 5(A) shows a 1x1 cm 2 Two 0.6μg / cm2 FIG5(B) shows a linear graph of EUV transparency of a film of size 1x1 cm according to an exemplary embodiment. 2 Two 0.6μg / cm 2 Linear plot of the EUV reflectivity of the film.
[0089] As shown in FIG. 5 , the filtered CNT sheath film has an EUV transparency of more than 97%, with an exceptionally low reflectivity and scattering level of only 0.21%. More specifically, FIG. 5(A) shows EUVT values for both samples A and B ranging from 97% to 99%, with most EUVT values being between 98% and 99%. As shown in FIG. 5(A), the CNT sheath film provided in the present disclosure provides very high EUVT values that were previously impossible to achieve. In view of the high EUVT values, it can be seen in FIG. 5(B) that the CNT sheath film has very low reflectance values, with most values being below 0.00005 mm and almost all values being below 0.00010 mm. Based on the above, it can be seen that the CNT sheath film with DWCNTs as the main component (at least 50%) allows almost all EUV radiation to be transmitted through, given the very high EUVT values and very low reflectance values.
[0090] Furthermore, the areal density of the CNT sheath film has an influence on visible light transmittance and visible light absorbance. In this regard, FIG. 4(A) shows the transparency and absorbance of DWCNT films having different areal densities at 550 nm (eg, visible light) according to an exemplary embodiment.
[0091] As shown in Figure 4(A)(I), there is an inverse relationship between the surface density and the transmittance at 550 nm. The inverse relationship is shown in Figure 4(A)(II). At one end, the surface density is 0.62 μg / cm 2 The average 550nm wavelength transmittance value is 93.833%. On the opposite end, the surface density is 3.11μg / cm 2 The average transmittance value at 550nm wavelength is 72.900%.
[0092] On the other hand, there is a symmetric relationship between the surface density and the absorbance. The symmetric relationship is exemplarily shown in Figure 4(A)(III). At one end, the surface density is 0.62 μg / cm 2 The average absorbance value is 0.028. At the opposite end, the surface density is 3.11 μg / cm 2 The absorbance value was 0.137.
[0093] Mechanical properties of CNT sheaths for EUV
[0094] Exemplary embodiments of the present application provide a CNT sheath having sufficient and satisfactory mechanical strength to cope with product transportation and handling. The sheath can withstand any required pressure changes around its environment (including but not limited to EUV lithography scanner environment).
[0095] A commonly used mechanical characterization is the bulge test. For example, the diaphragm used for the test can be attached to a flat surface of the boundary, and the baseline of the diaphragm can be established. Then, an initial inert gas flow can be applied to the central area of the diaphragm vertically at a low stable pressure to raise the local surface. The air pressure continues to increase incrementally to further deform the diaphragm until the pressure reaches a predetermined value, which is 2 Pa in terms of the 2Pa deflection test. This value can also be at a flow rate of about 10sccm, at 3.5mbar / second, or under any scanner evacuation conditions. The distance between the highest tip of the deformed diaphragm and its baseline can be measured. The result can be recorded as the deflection at 2Pa. The deflection test can be performed at different pressures other than 2Pa.
[0096] Increasing this gas flow pressure can eventually break the diaphragm apart. This pressure can be recorded as the rupture pressure, and the deflection of the diaphragm just before the diaphragm ruptures can be called the rupture deflection.
[0097] Additionally, film deflection may be intentionally adjusted by a variety of methods including, but not limited to, tension adjustment by physical or chemical means.
[0098] FIG4(B) shows the effect of areal density on the deflection of a DWCNT-dominated film of size 10x10 mm under a constant pressure of 2 Pa and at fracture according to an exemplary embodiment. FIG4(C) shows the effect of MWCNT concentration on the deflection of a DWCNT-dominated film of size 10x10 mm and with an areal density of 2.9 to 3.0 μg / cm 2 FIG4(D) shows a DWCNT film of 110×140 mm and with an areal density of 0.65 μg / cm during evacuation at a maximum rate of 3.5 mbar / sec according to an exemplary embodiment. 2 FIG4(E) shows the fracture pressure of membranes with different DWCNT / MWCNT ratios, which provides evidence supporting the current embodiment.
[0099] The structure of the membrane may be very porous. For example, see Figure 3 (A) and Figure 3 (B). The structure of the membrane can also be greatly dependent on the surface density. More specifically, since the membrane may be very porous, the surface density (μg / cm 2) rather than the film thickness. This change in microstructure also greatly affects the mechanical properties of the film (Figure 4(B)). In addition, visible light absorption is also affected. When measured over a range, these films appear to follow the Beer-Lambert law quite well. For example, see Figure 4(A). In the example, the CNT sheath film, including the full-scale film, can have a CNT sheath of about 0.2 μg / cm 2 To about 6.0μg / cm 2 Surface density.
[0100] Based on deflection testing of full-scale CNT sheaths according to exemplary embodiments, the CNT network forming the CNT film may have a deflection of less than 4.0 mm, less than 3.0 mm, 1.5 mm, or 0.6 mm at a constant 2 Pa pressure.
[0101] Various sizes of membranes ranging from 1 cm x 1 cm to 12 cm x 15 cm have been tested. However, aspects of the present disclosure are not so limited, such that testing of other sizes not specified herein may be performed.
[0102] The microstructure of BNNT films is very similar to that of CNT films, but BNNT films have a lower aspect ratio and contain more impurities due to the characteristics and low purity of the available raw materials.
[0103] Although low areal density CNT films can be manufactured to achieve high EUV transmittance, this may also make the film very susceptible to external pressure changes. By increasing the areal density of the CNT film, the deflection of the film under constant pressure can be greatly reduced and the elongation at the breaking point can be slightly increased. For example, see Figure 4(B).
[0104] As exemplarily shown in Fig. 4(B)(I), a lower surface density of 0.62 μg / cm2 results in an average deflection value of 0.098 mm at a pressure of 2 Pa, while a higher surface density of 3.11 μg / cm2 results in an average deflection value of 0.012 mm at a pressure of 2 Pa. The inverse relationship between the surface density and the deflection value at 2 Pa is exemplarily shown in Fig. 4(B)(II).
[0105] FIG. 4(B)(I) also indicates a generally equidirectional relationship between the surface density value and the deflection value at the fracture point of the CNT film. For example, a lower surface density of 0.62 μg / cm2 results in an average deflection value of 0.289 mm at fracture, while a higher surface density of 3.11 μg / cm2 results in an average deflection value of 0.380 mm at fracture. FIG. 4(B)(III) exemplarily shows the relationship between the surface density and the deflection value at fracture.
[0106] However, the relationship may affect the basic EUV transparency capability, ultimately rendering the high areal density films unsuitable for EUV lithography.
[0107] The effect of the type of CNT used (i.e., MWCNT) is shown in FIG4(C). The MWCNT film exhibits a higher deflection than the DWCNT film at the same pressure, indicating that the film material has a lower Young's modulus (softer); and the MWCNT film exhibits a lower deflection at break, indicating a lower elongation at break (more brittle). An explanation for this may be that, at the same surface density, a film made of MWCNT will contain less total nanotube length per unit area than a film made of DWNCT. This means that there are fewer contact points between the nanotubes and may result in a weaker material.
[0108] More specifically, FIG. 4(C)(I) shows the average deflection values and maximum deflection values of various CNT film samples having different DWCNT to MWCNT composition ratios at a pressure of 2Pa. As provided in FIG. 4(C)(I), the CNT film composed of 100% DWCNTs has an average deflection value of 0.030 mm and a maximum deflection value of 0.379 mm at a pressure of 2Pa. In addition, the CNT film composed of 75% DWCNT and 25% MWCNT has an average deflection value of 0.029 mm and a maximum deflection value of 0.345 mm at a pressure of 2Pa. The CNT film composed of 50% DWCNT and 50% MWCNT has an average deflection value of 0.052 mm and a maximum deflection value of 0.336 mm at a pressure of 2Pa. The CNT film composed of 25% DWCNT and 75% MWCNT has an average deflection value of 0.072 mm and a maximum deflection value of 0.307 mm at a pressure of 2Pa. Finally, the CNT film composed of 100% MWCNTs has an average deflection value of 0.066 mm and a maximum deflection value of 0.300 mm at a pressure of 2 Pa. As shown in Figure 4(C)(I), 100% MWCNTs have a deflection value (i.e., 0.066 mm) at a pressure of 2 Pa that is more than twice the deflection value (i.e., 0.030 mm) of 100% DWCNTs at a pressure of 2 Pa. The unidirectional relationship between the deflection value at a pressure of 2 Pa and the MWCNT composition ratio is shown in Figure 4(C)(II). The inverse relationship between the maximum deflection value and the MWCNT composition ratio is shown in Figure 4(C)(III).
[0109] Basically, pure DWCNT films showed higher mechanical strength. Figure 4(E) shows the fracture pressure (Pa) at different DWCNT to MWCNT ratios. All films have similar surface density and transparency. DWCNT is significantly stronger than MWCNT.
[0110] Figure 2 It is shown that a CNT film mainly composed of single-walled carbon nanotubes has a value very different from that of a CNT film mainly composed of double-walled carbon nanotubes. Figure 2It is also shown that the average deflection value of the DWCNT-dominated CNT film was measured at 2Pa to be 0.0967mm, which is about twice the lower limit of 0.0473mm for the SWCNT film. In addition, the SWCNT film exhibited a lower average fracture pressure of 66.61Pa. Finally, the average fracture deflection of the DWCNT-dominated CNT film was 0.498mm, while that of the SWCNT film was 0.097mm. And at Figure 2 In the results, the composite MWCNT films with similar size again showed their weaknesses in fracture pressure and deflection compared with the DWCNT-dominated CNT films.
[0111] like Figure 2 As exemplarily shown in , a CNT film composed primarily of DWCNTs (eg, at least 50%) has significantly lower deflection and higher transmittance as well as significantly higher fracture resistance, which indicates higher structural strength.
[0112] Life test
[0113] Exemplary life test of CNT sheath membrane formed by filtration according to exemplary embodiments. 1x1cm 2 The CNT sheath remained intact after EVU irradiation. 2 Exposure to 73 kJ / cm 2 dosage.
[0114] In addition, at 20W / cm 2 The power is equivalent to 90kJ / cm 2 Four hours of EUV irradiation testing of a full-size CNT sheath at a dose of 1000 W (equivalent to a 600 W energy source) showed an unbroken CNT film. This test dose is equivalent to the total irradiation required to process approximately 32,000 wafers.
[0115] As described above, the inventors have demonstrated the ability to produce freestanding nanoparticle films of sufficient size to be used as EUV sheaths in EUV scanner environments. When made from sufficiently thin monolayers of CNT material, these films have high EUV transparency (e.g., greater than 92%), low scatter (e.g., less than 0.3%), and retain sufficient mechanical stability and porosity to withstand the shipping, handling, and evacuation operations of full-size EVU sheaths (e.g., less than 0.1 mm deflection when evacuated at 3.5 mbar / sec).
[0116] Furthermore, the film withstands EUV radiation equivalent in dose and power to a 250W to 600W EUV scanner.
[0117] The illustrations of the embodiments described herein are intended to provide a general understanding of the various embodiments. The illustrations are not intended to be a complete description of all elements and features of the products and methods forming the products or methods described herein. Those skilled in the art will understand many other embodiments after reviewing this disclosure. Other embodiments may be utilized and derived from this disclosure so that structural and logical substitutions and changes may be made without departing from the scope of this disclosure. In addition, the illustrations are only representative and may not be drawn to scale. Certain ratios within the illustrations may be exaggerated, while other ratios may be minimized. Therefore, this disclosure and the accompanying drawings should be considered illustrative and not restrictive.
[0118] One or more embodiments of the present disclosure may be referred to herein individually and / or collectively by the term "invention", which is for convenience only and is not intended to limit the scope of the present application to any particular invention or inventive concept. In addition, although specific embodiments have been shown and described herein, it should be understood that any subsequent arrangements designed to achieve the same or similar purposes may replace the specific embodiments shown. The present disclosure is intended to cover any and all subsequent changes or variations of the various embodiments. Those skilled in the art will understand the combination of the above embodiments and other embodiments not specifically described herein after reviewing the description.
[0119] The abstract of the present disclosure is submitted with the understanding that it will not be used to interpret or limit the scope or meaning of the claims. In addition, in the foregoing detailed description, various features may be grouped together or described in a single embodiment to achieve the purpose of streamlining the present disclosure. The present disclosure should not be interpreted as reflecting the intention that the claimed embodiment requires more features than the features explicitly set forth in each claim. Rather, as reflected in the appended claims, the subject matter of the invention may not be all the features of any one of the disclosed embodiments. Therefore, the appended claims are incorporated into the specific embodiments, wherein each claim independently and individually defines the claimed subject matter.
[0120] The subject matter disclosed above should be considered illustrative rather than restrictive, and the appended claims are intended to cover all such modifications, enhancements, and other embodiments that are within the true spirit and scope of the disclosure. Therefore, to the maximum extent allowed by law, the scope of the present disclosure is determined by the broadest permissible interpretation of the appended claims and their equivalents, and shall not be restricted or limited by the foregoing detailed description.
Claims
1. A nanostructured film, the nanostructured film include: A plurality of carbon nanotubes, the plurality of carbon nanotubes randomly crossing to form an interconnected network structure in a planar orientation, the interconnected network structure having a thickness ranging from a lower limit of 3 nm to an upper limit of 100 nm and a minimum EUV transmittance of 92%, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, multi-walled carbon nanotubes and at least 50% double-walled carbon nanotubes, The number of walls of the single-walled carbon nanotube is one, the number of walls of the double-walled carbon nanotube is two, and the number of walls of the multi-walled carbon nanotube is three or more. 2 . The nanostructured film according to claim 1 , wherein the thickness is within the range of the lower limit of 3 nm to the upper limit of 40 nm. The nanostructured film according to claim 1 , wherein the thickness is within the range of the lower limit of 3 nm to the upper limit of 20 nm. The nanostructure film according to claim 1 , wherein the average thickness of the interconnected network structure is 11 nm. The nanostructured film of claim 1 , wherein the EUV transmittance is greater than 95%. The nanostructured film of claim 1 , wherein the EUV transmittance is greater than 98%.
7. The nanostructured film of claim 1, wherein the percentage of single-walled carbon nanotubes to all carbon nanotubes is between 20% and 40%, the percentage of double-walled carbon nanotubes to all carbon nanotubes is 50% or more, and the remaining carbon nanotubes are multi-walled carbon nanotubes.
8. The nanostructured film of claim 1, wherein the single-walled carbon nanotubes account for more than 20% of all carbon nanotubes, the double-walled carbon nanotubes account for more than 75% of all carbon nanotubes, and the remaining carbon nanotubes are multi-walled carbon nanotubes accounting for the remaining percentage of all carbon nanotubes.
9. The nanostructure film of claim 7, wherein the difference between any two EUV transmission measurements from the same nanostructure film at any focal region is less than 5%.
10. The nanostructure film of claim 9, wherein the difference between any two EUV transmission measurements from the same nanostructure film at any focal region is less than 2%.
11. The nanostructure film of claim 10, wherein the difference between any two EUV transmission measurements from the same nanostructure film at any focal region is less than 0.4%.
12. The nanostructured film of claim 1, wherein the interconnected network structure has a deflection of less than 3.5 mm at a flow rate of 10 seem.
13. The nanostructured film of claim 12, wherein the deflection is less than 0.6 mm at a flow rate of 10 seem.
14. The nanostructured film of claim 1, wherein the interconnected network structure has a deflection of less than 0.1 mm at a flow rate of 3.5 mbar / sec.
15. The nanostructure film of claim 1, wherein the interconnected network structure produces less than 0.3% scattering under EUV radiation.
16. The nanostructured film of claim 1, wherein the nanoparticles are conformally coated with boron, a metal, a metal oxide or a nitride, the metal being selected from ruthenium, zirconium, niobium, molybdenum, rubidium, yttrium, strontium or rhodium.
17. The nanostructured film according to claim 5, wherein the nanostructured film has a carbon content of 0.2 μg / cm 2 To 6.0μg / cm 2 Surface density.
18. The nanostructured film of claim 1, wherein the interconnected network structure has a deflection of less than 3.5 mm at a flow rate of 3.5 mbar / sec.
19. The nanostructured film of claim 18, wherein the interconnected network structure has a deflection of less than 4.0 mm under a 2 Pa deflection test.
20. A protective layer, the protective layer include: a sheath boundary defining an aperture, and at least one nanostructured film disposed to the boundary of the sheath and covering the aperture, Wherein, the at least one nanostructured film comprises: A plurality of carbon nanotubes, the plurality of carbon nanotubes randomly crossing to form an interconnected network structure in a planar orientation, the interconnected network structure having a thickness ranging from a lower limit of 3 nm to an upper limit of 100 nm and a minimum EUV transmittance of 92%, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, multi-walled carbon nanotubes and at least 50% double-walled carbon nanotubes, The number of walls of the single-walled carbon nanotube is one, the number of walls of the double-walled carbon nanotube is two, and the number of walls of the multi-walled carbon nanotube is three or more.
21. The covering of claim 20, wherein the at least one nanostructured film has a deflection of less than 3.5 mm at a flow rate of 3.5 mbar / second.
22. The covering of claim 21 wherein the at least one nanostructured film has a deflection of less than 4.0 mm under a 2 Pa deflection test.
23. A method of performing EUV lithography, the method comprising transmitting EUV radiation through a protective layer, The protective layer include: a sheath boundary defining an aperture, and at least one nanostructured film disposed to the boundary of the sheath and covering the aperture, Wherein, the at least one nanostructured film comprises: A plurality of carbon nanotubes, the plurality of carbon nanotubes randomly crossing to form an interconnected network structure in a planar orientation, the interconnected network structure having a thickness ranging from a lower limit of 3 nm to an upper limit of 100 nm and a minimum EUV transmittance of 92%, wherein the plurality of carbon nanotubes include single-walled carbon nanotubes, multi-walled carbon nanotubes and at least 50% double-walled carbon nanotubes, The number of walls of the single-walled carbon nanotube is one, the number of walls of the double-walled carbon nanotube is two, and the number of walls of the multi-walled carbon nanotube is three or more.