Porous lanthanum zirconium phosphate defluorination material and preparation method and application thereof

By preparing porous zirconium lanthanum phosphate defluoridation materials, the problem of difficulty in reducing the concentration of fluorine-containing wastewater and material regeneration in the existing fluoride removal process has been solved. Efficient and stable fluoride ion adsorption and recycling have been achieved, and the fluoride removal efficiency and materials have been improved. specific surface area.

CN115945160BActive Publication Date: 2024-10-22WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310064193.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-12
Publication Date
2024-10-22
Estimated Expiration
2043-01-12

AI Technical Summary

Technical Problem

The existing fluoride removal process is difficult to reduce the concentration of fluorine-containing wastewater below 1.5 mg/L, and it cannot be recycled and reused. The adsorption materials have low efficiency and small specific surface area.

Method used

Porous zirconium lanthanum phosphate defluoridation materials are prepared by using raw materials such as zirconium oxychloride, lanthanum nitrate and diammonium hydrogen phosphate through high-temperature precipitation, filtration and washing, drying and roasting. It has a high specific surface area and mesoporous structure, and can be used as a high-efficiency defluoridation agent. Cetyltrimethylammonium bromide was used as a template to improve the adsorption capacity of the material.

Benefits of technology

It achieves high-efficiency removal of fluoride ions, and the material has good chemical stability and cycle regeneration performance. It can still ensure a removal rate of 78% in a fluorine-containing solution with an initial concentration of 5 mg/L for 6 times, and the maximum specific surface area is 455.15m2/ g, adsorption can reach equilibrium within 50 minutes, is low-cost and meets environmental requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115945160B_ABST
    Figure CN115945160B_ABST
Patent Text Reader

Abstract

The present invention discloses a porous zirconium lanthanum phosphate defluorination material and a preparation method and application thereof. The porous zirconium lanthanum phosphate defluorination material comprises the following raw material components: zirconium oxychloride, lanthanum nitrate, diammonium hydrogen phosphate, ammonium carbonate and a template agent. The addition amounts of the zirconium oxychloride and the lanthanum nitrate are represented by a molar ratio of Zr 4+ :La 3+ =1:(0.3-3). The method mainly uses zirconium oxychloride as a zirconium source, lanthanum nitrate as a lanthanum source, diammonium hydrogen phosphate as a phosphorus source, and hexadecyltrimethylammonium bromide as a template agent, and prepares a high specific surface area porous zirconium lanthanum phosphate defluorination material through high temperature precipitation, filtration washing, drying and roasting. The mesoporous structure is stable and the specific surface area is high, and it can be used as an efficient defluorination agent. The porous zirconium lanthanum phosphate defluorination material obtained by the method has uniform element distribution, high specific surface area, many active sites, and strong adsorption capacity. It has a high adsorption capacity for fluoride ions and can be recycled, showing great application value in the field of purifying fluoride-containing water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic functional material synthesis, and specifically relates to a porous lanthanum zirconium phosphate defluorination material and a preparation method and application thereof. Background Art

[0002] With the large amount of wastewater generated by the aluminum processing industry, semiconductor industry, phosphating industry and fertilizer industry, as well as the geological characteristics of underground rock minerals and the weathering and leaching of certain fluorine-containing minerals such as amphibole, apatite, mica and fluorite, the fluoride concentration in groundwater is relatively high. The World Health Organization (WHO) stipulates that the optimal concentration of fluoride in drinking water is 0.5-1.5 mg / L. Intake of trace fluoride is beneficial to the healthy growth of human bones and teeth, but too high fluoride can cause various diseases such as thyroid disease, nervous system disease, dental fluorosis and skeletal fluorosis.

[0003] At present, the commonly used defluorination methods mainly include chemical precipitation, adsorption, ion exchange, etc. The traditional defluorination process is mainly based on limestone precipitation, which mainly uses Ca 2+ With F - Calcium fluoride precipitate is generated to reduce the fluoride ion concentration, but CaF2 will wrap around the surface of Ca(OH)2 and reduce the precipitation efficiency, making it difficult to reduce the fluoride-containing wastewater concentration to less than 1.5 mg / L.

[0004] In recent years, studies have shown that some metal oxides, hydroxides and phosphates have high anion adsorption capacity. The main target of treatment is H2AsO4 - ,HAsO4 2- 、H2PO4 - 、H2PO4 2- 、F - Ions, among which zirconium and lanthanum oxides have better effects on fluorine removal. Zirconium salts are gradually being developed and utilized in adsorption because of their large specific surface area, high thermal stability, water resistance and easy precipitation. Lanthanum salts are usually used as active substances for adsorbing fluoride ions. This is because the lanthanum metal atom has a low potential and high alkalinity, which makes hydrated lanthanum oxide positively charged and has a strong ability to adsorb anions. However, pure hydrated lanthanum oxide is difficult to regenerate and has the defect of lanthanum ion dissolution.

[0005] Based on this, the present invention combines zirconium and lanthanum metals with phosphate ions to prepare porous zirconium lanthanum phosphate defluorination material adsorption material which not only has high defluorination efficiency but also has good chemical stability and recycling regeneration performance. Summary of the invention

[0006] In order to overcome the shortcomings of the above-mentioned existing background technology, the present invention provides a porous zirconium lanthanum phosphate defluorination material and its preparation method and application. The method mainly uses zirconium oxychloride as a zirconium source, lanthanum nitrate as a lanthanum source, diammonium hydrogen phosphate as a phosphorus source, and hexadecyltrimethylammonium bromide as a template agent. After high-temperature precipitation, filtration and washing, drying and roasting, a high specific surface area porous zirconium lanthanum phosphate defluorination material is prepared. The mesoporous structure is stable and the specific surface area is high, and it can be used as a high-efficiency defluorination agent. The porous zirconium lanthanum phosphate defluorination material obtained by this method has uniform element distribution, high specific surface area, many active sites, strong adsorption capacity, high adsorption capacity for fluoride ions, and can be recycled, showing great application value in the field of purifying fluoride-containing water.

[0007] To achieve the above object, the present invention is implemented by the following technical solutions:

[0008] On the one hand, the present invention provides a porous zirconium lanthanum phosphate defluorination material, the porous zirconium lanthanum phosphate defluorination material comprises the following raw material components: zirconium oxychloride, lanthanum nitrate, diammonium hydrogen phosphate, ammonium carbonate and a template, the addition amount of the zirconium oxychloride and the lanthanum nitrate is denoted by molar ratio: Zr 4+ :La 3+ =1:(0.3-3).

[0009] Preferably, the amount of zirconium oxychloride and lanthanum nitrate added is represented by a molar ratio of Zr 4+ :La 3+ =2:1.

[0010] Preferably, the specific surface area of ​​the porous lanthanum zirconium phosphate defluorination material is 450 to 455 m 2 / g, pore volume is 0.078cm 3 / g, average pore size 1.5~2.0nm.

[0011] Preferably, the template is selected from hexadecyltrimethylammonium bromide.

[0012] On the other hand, the present invention provides a method for preparing a porous lanthanum zirconium phosphate defluorination material, comprising the following steps:

[0013] (1) dissolving zirconium oxychloride and ammonium carbonate in deionized water to prepare solution A, dissolving diammonium hydrogen phosphate in deionized water to prepare solution B, and dissolving lanthanum nitrate in deionized water to prepare solution C;

[0014] (2) Slowly drop solution B into solution A, stir for 10 to 30 minutes, then drop solution C, stir for 10 to 30 minutes until the solution becomes clear; then add the template, stir for 1 to 2 hours to obtain a mixed solution D;

[0015] (3) Pour the mixed solution D into a sealed polyethylene bottle and place it at 80-90° C. for precipitation for 72-84 hours. After complete precipitation, filter, wash and dry the product. After calcining at 500-600° C. for 3-5 hours, a porous zirconium lanthanum phosphate defluorination material with a high specific surface area is obtained.

[0016] Preferably, in step (3), the temperature of the heating precipitation is 85° C., and the insulation reaction time is 72 h.

[0017] Preferably, in step (3), the high temperature calcination temperature is 550° C. and the calcination time is 3 h.

[0018] In another aspect, the present invention provides an application of a porous lanthanum zirconium phosphate defluorination material in treating fluoride ions in water, comprising: adding the porous lanthanum zirconium phosphate defluorination material to a fluoride-containing aqueous solution, placing it on a constant temperature shaker for shaking, and removing fluoride ions.

[0019] Preferably, a constant temperature and humidity air bath shaker is used for shaking, with a shaking frequency of 160-180 rpm, a shaking time of 2 h, and a shaking temperature of 25°C.

[0020] Preferably, the fluorine-containing aqueous solution is an acidic or neutral system, and the dosage of the porous lanthanum zirconium phosphate defluorination material is 0.2-2.0 g / L. Furthermore, the optimal dosage of the porous lanthanum zirconium phosphate defluorination material is 0.85 g / L.

[0021] Preferably, the porous zirconium lanthanum phosphate defluorination material that is saturated with adsorption after use is added with a 0.01-0.5 mol / L NaOH solution, shaken at room temperature, and regenerated after 24 hours of desorption reaction. After desorption, it is washed with deionized water to neutrality, and the porous zirconium lanthanum phosphate defluorination material after desorption can be recycled.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. At present, it is difficult for the traditional defluorination process to reduce the concentration of fluorine-containing wastewater to less than 1.5 mg / L, and it cannot be recycled. The porous zirconium lanthanum phosphate defluorination material prepared by the present invention has good regeneration and recycling performance. In a fluorine-containing solution with an initial concentration of 5 mg / L, 6 cycles of adsorption can still ensure a removal rate of 78%.

[0024] 2. The current defluorination adsorption materials have low adsorption efficiency and small specific surface area. The porous zirconium lanthanum phosphate defluorination material prepared by the present invention has a large specific surface area, a uniform and stable mesoporous structure, and a maximum specific surface area of ​​455.15m 2 / g, the maximum adsorption capacity of the prepared porous lanthanum zirconium phosphate defluorination material is 95.15 mg / g, and equilibrium can be reached after 50 minutes of adsorption.

[0025] 3. The preparation method of the present invention has simple process, low cost and meets environmental requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope photo and element mapping diagram of the porous lanthanum zirconium phosphate defluorination material in Example 2 of the present invention; wherein, Figure 1 a is a scanning electron microscope photo, Figure 1 b is the element mapping diagram;

[0027] Figure 2 This is a transmission electron microscope of the porous lanthanum zirconium phosphate defluorination material in Example 2 of the present invention;

[0028] Figure 3 This is a graph showing the fluorine removal performance of porous lanthanum zirconium phosphate fluorine removal materials with different ratios in Example 3 of the present invention;

[0029] Figure 4 This is a test diagram of the effect of contact time on the defluorination performance of the porous lanthanum zirconium phosphate defluorination material in Example 4 of the present invention;

[0030] Figure 5 This is a test diagram of the effect of initial concentration on the defluorination performance of the porous lanthanum zirconium phosphate defluorination material in Example 5 of the present invention;

[0031] Figure 6 This is a test diagram of the regeneration cycle performance of the porous lanthanum zirconium phosphate defluorination material in Example 6 of the present invention; wherein, Figure 6 a is the effect of using different concentrations of NaOH solution as the analytical solution on the adsorption efficiency of porous zirconium phosphate lanthanum defluorination material. Figure 6 b is the effect of different recycling times on the adsorption efficiency of porous zirconium lanthanum phosphate defluorination material;

[0032] Figure 7 This is a diagram showing the application results of the porous lanthanum zirconium phosphate defluorination material in Application Example 1 of the present invention in actual fluoride-containing water. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments, but it should not be understood as limiting the present invention and is only used as an example.

[0034] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0035] Example 1

[0036] A method for preparing a high specific surface area porous lanthanum zirconium phosphate defluorination material adsorbent:

[0037] Weigh 1.79g zirconium oxychloride and 3.78g ammonium carbonate and dissolve them in 40ml deionized water, then weigh 1.47g diammonium hydrogen phosphate and dissolve them in 30ml deionized water, and then weigh a certain amount of lanthanum nitrate and dissolve them in 30ml deionized water. Stir them on a constant temperature magnetic stirrer for 20min until they are clear, then mix and stir the above solutions until they are clear, add 0.61g hexadecyltrimethylammonium bromide and continue stirring for 2h until they are completely dissolved. The content of zirconium oxychloride and lanthanum nitrate is recorded in molar ratio as Zr 4+ :La 3+ =1:0.3, 1:0.5, 1:1, 1:2, 1:3. The resulting solution was covered and placed in an oven at 85°C for 72 hours to completely precipitate and cool, filtered, washed with deionized water, dried, and then calcined at 550°C for 3 hours to obtain a porous zirconium lanthanum phosphate defluorination material.

[0038] The porous lanthanum zirconium phosphate defluorination material prepared according to the above method was subjected to BET specific surface area analysis, and the obtained parameters are shown in Table 1.

[0039] Example 2

[0040] Structure and properties of porous lanthanum zirconium phosphate defluorination material:

[0041] On the basis of zirconium phosphate, porous zirconium lanthanum phosphate defluorination materials with different specific surface areas can be obtained by changing the dosage of lanthanum nitrate, so as to further obtain the best ratio and achieve better adsorption effect. 4+ :La 3+ When the ratio is 2:1, the prepared porous zirconium lanthanum phosphate defluorination material has the largest specific surface area, reaching 455.15m 2 / g. The scanning electron microscope image of the porous zirconium lanthanum phosphate defluorination material is shown in Figure 1 , transmission electron microscopy images are shown in Figure 2 It can be seen that the porous zirconium lanthanum phosphate defluorination material is spherical, with a rough surface and gaps. Obviously, the porous structure can provide more adsorption sites, which is more conducive to the adsorption of F - Combined with the porous lanthanum zirconium phosphate to enhance the defluorination of F - adsorption efficiency and adsorption capacity.

[0042] Example 3

[0043] Fluoride removal performance of porous zirconium lanthanum phosphate defluoride materials with different ratios:

[0044] Weigh different proportions of porous zirconium lanthanum phosphate defluorination materials (Zr 4+ :La 3+=3:1, 2:1, 1:1, 1:2, 1:3) 0.01g each, added to 50ml of sodium fluoride prepared pH = 3, concentration of 5mg / L fluoride ion solution, constant temperature oscillation at 25℃, adsorption for 2h, calculate the adsorption amount according to formula (1):

[0045]

[0046] Among them, q t is the equilibrium adsorption amount per unit mass of adsorbent in time t, mg / g; C0 is the initial fluoride ion concentration, mg / L; C t is the fluoride ion concentration after adsorption time t, mg / L; V is the volume of the fluoride ion solution, mL; m is the mass of the porous zirconium lanthanum phosphate defluoridation material, g.

[0047] The calculation results are shown in Figure 3 As can be seen from the figure, in Zr 4+ :La 3+ When the ratio is 2:1, the adsorption capacity reaches the maximum, which may be due to the 4+ and La 3+ It forms a stable structural framework with phosphate ions, but with La 3+ The increase in the content of non-framework La 3+ Excess affects the formation of its porous structure.

[0048] Example 4

[0049] Effect of contact time on the fluorine removal performance of porous zirconium lanthanum phosphate fluorine removal material:

[0050] 0.3 g of porous lanthanum zirconium phosphate defluorination material (Zr 4+ :La 3+ The ratio of 2:1) was added to 500 ml of fluoride ion solution with pH = 3 and different initial concentrations (5 and 10 mg / L), and the mixture was kept at a constant temperature of 25 °C. 30 mL of sample was taken out every 10 min, and the adsorption amount was determined according to formula (1). The results are shown in Figure 4 As can be seen from the figure, the adsorption capacity gradually increases with time until equilibrium. When the initial concentration is 5 and 10 mg / L, the equilibrium time of the porous zirconium lanthanum phosphate defluorination material is about 50 min and 80 min, and the corresponding adsorption amounts are 7.14 and 13.88 mg / g, respectively.

[0051] Example 5

[0052] Effect of initial concentration on the defluorination performance of porous lanthanum zirconium phosphate defluorination material:

[0053] In order to investigate the effect of different fluoride ion concentrations on the adsorption performance of porous lanthanum zirconium phosphate defluorination materials, 0.03 g lanthanum zirconium phosphate (Zr4+ :La 3+ The ratio of the mixture was 2:1), and the mixture was put into 50 ml of a fluoride ion solution with a pH of 3 and a concentration of 2, 4, 5, 6, 8, 10, 20, 30, 40, 50, and 100 mg / L. The mixture was kept at a constant temperature of 25°C and the adsorption capacity was determined after 2 hours of adsorption according to formula (1). The results are shown in Table 1. Figure 5 It can be seen from the figure that as the initial fluoride ion concentration increases, the adsorption capacity of the porous zirconium lanthanum phosphate defluoridation material also increases. This is because the higher the concentration of fluoride ions, the higher the efficiency of binding with the porous zirconium lanthanum phosphate defluoridation material, and the higher the adsorption efficiency.

[0054] Example 6

[0055] Regeneration cycle performance of porous zirconium lanthanum phosphate defluorination material:

[0056] Using NaOH solutions of different concentrations of 0.01, 0.05, 0.1, 0.2, and 0.5 mol / L as analytical solutions, the adsorption saturated porous zirconium lanthanum phosphate defluorination material (Zr 4+ :La 3+ The ratio of 2:1) was soaked for 12 hours, washed with deionized water, filtered and dried, and then put into 50mL of fluoride ion solution with pH = 3 and concentration of 5mg / L for another adsorption experiment. The adsorption was carried out at a constant temperature of 25°C. After adsorption for 2 hours, the calculation was performed according to formula (1), and then the above experiment was repeated. The regeneration cycle performance of porous zirconium lanthanum phosphate defluorination material is shown in Figure 6 As can be seen from the figure, the adsorption performance remains basically unchanged, and even after 6 cycles, the adsorption efficiency can still be maintained at 78%.

[0057] Comparative Example 1

[0058] Table 2 compares the performance of zirconium-based oxides in adsorbing fluoride ions in water. It can be seen from the table that the prepared porous zirconium lanthanum phosphate defluoridation material has a relatively high adsorption performance for fluoride ions in water, which may be due to the fact that Zr 4+ and La 3+ It has a strong affinity for fluoride ions, and the internal porous structure also provides more adsorption sites for fluoride ions, thereby improving the adsorption performance of porous zirconium lanthanum phosphate defluorination materials for fluorine.

[0059] Application Example 1

[0060] In order to test the application of adsorption materials in actual fluoride-containing water, a well in the high-fluoride area of ​​Phosphorus Mine Town, Zhongxiang City, Jingmen City, Hubei Province was selected. The fluoride-containing groundwater was analyzed by ICP-MS, showing the fluoride concentration in the groundwater sample (initial pH value was 7.6, fluoride concentration was 2.94 mg / L), and the groundwater quality indicators are shown in Table 3. Different doses of 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, and 0.15 g of porous zirconium lanthanum phosphate defluoridation material (Zr 4+ :La 3+ The ratio is 2:1) and 50 mL of actual fluoride-containing water is added. The mixture is kept at a constant temperature of 25 °C and shaken. After adsorption for 2 h, the adsorption amount is measured according to formula (1). The results are shown in Figure 7 . As the adsorbent dosage increased, the fluoride concentration decreased, and the residual fluoride concentration after adsorption equilibrium dropped from 2.94 mg / L to 0.33 mg / L. When the adsorbent dosage was 0.05 g, the residual fluoride concentration after adsorption equilibrium was 0.74 mg / L, which could effectively reduce the fluoride ion concentration to below 1.0 mg / L, providing evidence for the applicability and feasibility of porous zirconium lanthanum phosphate defluoridation materials in removing fluoride from water.

[0061] The BET analysis and specific surface area parameters of the porous zirconium lanthanum phosphate defluorination materials with different zirconium and lanthanum ratios prepared according to the above method are shown in Table 1.

[0062] Table 1

[0063]

[0064] Table 2

[0065]

[0066]

[0067] Table 3

[0068]

[0069] It should be noted that the above-described embodiments are only preferred embodiments of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above-described exemplary embodiments, and the present invention can be implemented in any other specific form without departing from the spirit or basic features of the present invention. Therefore, this embodiment is merely an exemplary case and is non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and is intended to include all changes within the meaning and scope of the equivalent elements of the claims. Any reference numerals in the claims should not be considered as limiting the claims involved.

Claims

1. A porous lanthanum zirconium phosphate defluorination material, characterized in that: The porous zirconium lanthanum phosphate defluorination material comprises the following raw material components: zirconium oxychloride, lanthanum nitrate, diammonium hydrogen phosphate, ammonium carbonate and a template agent. The addition amounts of the zirconium oxychloride and the lanthanum nitrate are denoted by molar ratio: Zr 4+ :La 3+ =2:1, the specific surface area of ​​the porous zirconium lanthanum phosphate defluorination material is 450-455m 2 / g, pore volume is 0.078cm 3 / g, average pore size 1.5~2.0nm; The method for preparing a porous lanthanum zirconium phosphate defluorination material comprises the following steps: (1) dissolving zirconium oxychloride and ammonium carbonate in deionized water to prepare solution A, dissolving diammonium hydrogen phosphate in deionized water to prepare solution B, and dissolving lanthanum nitrate in deionized water to prepare solution C; (2) Slowly drop solution B into solution A, stir for 10 to 30 minutes, then drop solution C, stir for 10 to 30 minutes until the solution becomes clear; then add the template, stir for 1 to 2 hours to obtain a mixed solution D; (3) Pour the mixed solution D into a sealed polyethylene bottle and place it at 80-90° C. for precipitation for 72-84 hours. After complete precipitation, filter, wash and dry the product. After calcining at 500-600° C. for 3-5 hours, a porous zirconium lanthanum phosphate defluorination material with a high specific surface area is obtained.

2. The porous lanthanum zirconium phosphate defluorination material according to claim 1, characterized in that: The template agent is selected from hexadecyltrimethylammonium bromide.

3. The porous lanthanum zirconium phosphate defluorination material according to claim 1, characterized in that: In step (3), the temperature of the heating precipitation is 85° C., and the insulation reaction time is 72 h.

4. The porous lanthanum zirconium phosphate defluorination material according to claim 1, characterized in that: In step (3), the high temperature calcination temperature is 550° C. and the calcination time is 3 h.

5. Use of the porous lanthanum zirconium phosphate defluoridation material according to any one of claims 1 to 4 in treating fluoride ions in water, characterized in that: include: The porous lanthanum zirconium phosphate defluorination material is added to the fluorine-containing aqueous solution and placed on a constant temperature shaker to remove fluoride ions.

6. The use according to claim 5, characterized in that: The fluorine-containing aqueous solution is an acidic or neutral system, and the dosage of the porous lanthanum zirconium phosphate defluorination material is 0.2-2.0 g / L.

7. The use according to claim 5, characterized in that: The porous lanthanum zirconium phosphate defluorination material that is saturated with adsorption after use is added with a 0.01-0.5 mol / L NaOH solution, shaken at room temperature, and regenerated after 24 hours of desorption reaction. After desorption, it is washed with deionized water to neutrality. The porous lanthanum zirconium phosphate defluorination material after desorption can be recycled.