Air purification material and preparation method thereof
Through the preparation technology of cobalt-doped manganese oxide fiber membrane, combined with the growth of metal organic framework materials, the problem of existing air filter materials being unable to adsorb PM2.5 and formaldehyde at the same time has been solved, achieving efficient adsorption and improving stability, and providing a A reusable air purification material.
Patent Information
- Application Number
- CN202211610126.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-12
AI Technical Summary
Existing air filter materials cannot efficiently adsorb indoor PM2.5, PM10 and other tiny particles and formaldehyde at the same time. Harmful substances are easily desorbed, resulting in secondary pollution, and the material stability is poor.
The cobalt-doped manganese oxide fiber membrane is prepared by electrospinning technology, impregnated with 2-methylimidazole and then annealed to form an air purification material with a three-dimensional network structure. Metal-organic framework materials are used to grow on the surface of the fiber to improve the adsorption effect.
It achieves efficient adsorption of formaldehyde, PM2.5, and PM10. The adsorbed materials are not easy to desorb. The material has good reusability and air purification performance.
Smart Images

Figure BDA0003993464240000091 
Figure BDA0003993464240000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of air purification, and in particular to an air purification material and a preparation method thereof. Background Art
[0002] In recent years, the rapid economic development has improved people's living standards, and most daily activities and work have been transferred from outdoor to indoor. Studies have shown that people now spend more than 85% of their daily life and work in indoor spaces, so indoor air quality is crucial. According to statistics from indoor air testing departments, 80% of indoor environments have pollutant levels that exceed national standards, causing harm to public health. Air pollution is mainly divided into tiny particles and volatile organic compounds. Tiny particles mainly include PM2.5, PM10, etc. and pathogenic bacteria, and volatile organic compounds mainly include formaldehyde, benzene, toluene and other harmful substances. Formaldehyde released from interior decoration materials and PM2.5 tiny particles suspended indoors are the most urgent indoor pollution problems to be solved. The current air filter materials have a single function, mainly targeting tiny particles PM2.5, and cannot simultaneously take into account the adsorption of harmful substances such as formaldehyde.
[0003] Activated carbon is the most common adsorption material at present. Its small adsorption capacity requires constant replacement of materials, and the adsorbed pollutants may also desorb and cause secondary pollution. Manganese dioxide (MnO2) can be used as a catalyst to deeply oxidize formaldehyde in the air through the surface lattice, but MnO2 materials have the problems of low catalytic efficiency and poor stability at room temperature. Metal organic framework materials (MOFs) have excellent characteristics such as large specific surface area, high porosity, structural and functional diversity. They have been widely studied by scientific researchers in the fields of gas adsorption and separation, storage, catalysis, biomedicine, luminescence and sensing. However, most MOFs materials are powdered materials, which limits their practical applications.
[0004] Therefore, developing a new type of material that can efficiently purify indoor air environment has good application prospects. Summary of the invention
[0005] The purpose of the present invention is to provide an air purification material and a preparation method thereof, which can improve the adsorption effect on formaldehyde and tiny particles such as PM2.5 and PM10, and the adsorbed pollutants are not easy to desorb and can be reused.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] The invention provides a method for preparing an air purification material. After a cobalt-doped manganese oxide fiber membrane is prepared, the membrane is immersed in 2-methylimidazole and annealed to obtain the air purification material.
[0008] Furthermore, the method for preparing manganese oxide fiber membrane comprises the following steps: adding manganese acetate and copper acetate to isopropanol, stirring evenly to obtain a sol, adjusting the pH to acidic, adding an isopropanol solution of polyvinyl pyrrolidone to obtain a precursor solution, and performing electrospinning to obtain a manganese oxide fiber membrane.
[0009] Furthermore, the mass ratio of manganese acetate to copper acetate is (45-50):(8-10).
[0010] Further, the pH was adjusted to 5-6.
[0011] Furthermore, the molecular weight of polyvinyl pyrrolidone is 15000-30000. During the electrospinning process, the viscosity of the spinning solution affects the morphology and performance of the final product. The spinning solution can be better stretched by the electric field force to form fibers within a suitable viscosity range. In the present invention, whether the fibers can be smoothly formed during the preparation process of the cobalt-doped manganese oxide fiber membrane is greatly affected by the molecular weight of polyvinyl pyrrolidone. When the molecular weight of polyvinyl pyrrolidone is too large, it will cause excessive and dense entanglement of the molecular chains, restrict the free movement of the polymer molecular chains, and cause instability during the jet, making it difficult to complete the spinning process; when the molecular weight of polyvinyl pyrrolidone is too small, the spinning solution is difficult to form a normal jet, and spinning is difficult, and only droplets can be formed in the end. The fibers in the cobalt-doped manganese oxide fiber membrane obtained by the present invention are uniform in thickness, smooth in surface, good in fiber structure morphology, and no beads appear.
[0012] Furthermore, the parameters of electrospinning are: voltage of 15-20 V, injection speed of 0.06-0.08 mm / min, syringe tilt angle of 30° to the horizontal plane, receiving distance of 18-20 cm, receiving roller speed of 140-160 rpm, temperature of 25±2° C., humidity of 25±2° C., and receiving time of 30 h.
[0013] Furthermore, the immersion temperature is 35-45°C, and the immersion time is 10-15h.
[0014] Furthermore, the annealing temperature is 400-500°C and the annealing time is 1-3h. The diameter of the fiber directly affects the adsorption efficiency of the air purification material, and the fineness and uniformity of the fiber diameter are conducive to the subsequent growth of the metal organic framework on its surface. The average fiber diameter of the cobalt-doped manganese oxide fiber membrane is 330-360nm. In order to obtain MOFs material on the surface of the cobalt-doped manganese oxide fiber membrane, the manganese oxide fiber membrane is immersed in an anhydrous ethanol solution of 2-MI. Under heating, Co 2+It undergoes a coordination reaction with 2-MI in the solution, and ZIF-6 crystals grow along the surface of the manganese oxide fiber. The cobalt-doped manganese oxide fiber membrane remains intact after impregnation, and the growth of the metal organic framework material will not destroy the fiber morphology or block the internal pores of the fiber membrane. The ZIF-6 crystals are densely arranged on the fiber surface, and a rough structure appears on the fiber surface. The fiber diameter increases slightly, and the average diameter is 350-375nm. After annealing, the PVP skeleton is vaporized to obtain an air purification material with a three-dimensional network structure, which has a good adsorption effect on formaldehyde and tiny particles such as PM2.5 and PM10, and is not easy to desorb.
[0015] The invention provides an air purification material prepared by the preparation method.
[0016] The present invention discloses the following technical effects:
[0017] The present invention provides an air purification material with a three-dimensional network structure, which has the characteristics of large specific surface area, small pore size and high porosity, has good adsorption effect on formaldehyde and tiny particles such as PM2.5 and PM10, and can be used in the field of air purification. DETAILED DESCRIPTION
[0018] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0019] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0020] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0021] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0022] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0023] The molecular weight of polyvinyl pyrrolidone in the embodiment of the present invention is 15000-30000.
[0024] The room temperature in the embodiments of the present invention refers to 25±2°C.
[0025] The commercial activated carbon used in the formaldehyde adsorption performance test of the present invention is coconut shell activated carbon purchased from Suzhou Hongda Environmental Protection Technology Co., Ltd.
[0026] Example 1
[0027] In a glove box, 4.5 g of Mn(CH3COO)2·2H2O and 0.8 g of Co(CH3COO)2 were added to 6 mL of isopropanol and stirred for 5 h to obtain a sol. Ammonia water was added to adjust the pH of the sol to 6. 4 mL of isopropanol solution in which 0.3 g of polyvinyl pyrrolidone (molecular weight 15000) was dissolved was added and stirred for 1 h to obtain a precursor solution, which was poured into a syringe for electrospinning. 2 The non-woven fabric was used as the receiving substrate, and the electrospinning process parameters were as follows: voltage of 15 V, injection speed of 0.08 mm / min, syringe inclination angle of 30° to the horizontal plane, receiving distance of 20 cm, receiving roller speed of 140 rpm, temperature of 25±2°C, humidity of 25±2°C, and receiving time of 30 h to obtain a cobalt-doped manganese oxide fiber membrane; 2 g of 2-methylimidazole (2-MI) was dissolved in 100 mL of anhydrous ethanol to obtain an anhydrous ethanol solution of 2-MI, and the prepared cobalt-doped manganese oxide fiber membrane was immersed in the anhydrous ethanol solution of 2-MI at 35°C for 12 h, then rinsed with anhydrous ethanol and deionized water, dried in an oven at 80°C, and then annealed in a muffle furnace at 400°C for 3 h to obtain an air purification material.
[0028] The average diameter of the fibers constituting the cobalt-doped manganese oxide fiber membrane in this embodiment is 330 nm, and the fibers are uniform in thickness, smooth in surface, good in fiber structure morphology, and free of beads. The cobalt-doped manganese oxide fiber membrane is immersed in a 2-MI anhydrous ethanol solution and heated. 2+A coordination reaction occurs with 2-MI in the solution, and ZIF-6 crystals grow along the surface of the manganese oxide fiber. The cobalt-doped manganese oxide fiber membrane remains intact after impregnation, and the growth of the metal organic framework material does not destroy the morphology of the fiber and does not block the internal pores of the fiber membrane. The ZIF-6 crystals are densely arranged on the fiber surface, and a rough structure appears on the fiber surface. The fiber diameter increases slightly, and the average diameter is 352nm. After annealing, the PVP skeleton is vaporized to obtain an air purification material with a three-dimensional network structure.
[0029] The BET specific surface area of the air purification material in this embodiment is 2596 m 2 / g, porosity is 92.3%, pore volume is 2.61cm 3 / g, and the pore size distribution is 1.3-1.6nm.
[0030] Example 2
[0031] In a glove box, 5.0 g of Mn(CH3COO)2·2H2O and 1.0 g of Co(CH3COO)2 were added to 6 mL of isopropanol and stirred for 5 h to obtain a sol. Ammonia water was added to adjust the pH of the sol to 5. 4 mL of isopropanol solution in which 0.3 g of polyvinyl pyrrolidone (molecular weight 20,000) was dissolved was added and stirred for 1 h to obtain a precursor solution, which was poured into a syringe for electrospinning. 2 The non-woven fabric was used as the receiving substrate, and the electrospinning process parameters were as follows: voltage of 20 V, injection speed of 0.08 mm / min, syringe inclination angle of 30° to the horizontal plane, receiving distance of 20 cm, receiving roller speed of 140 rpm, temperature of 25±2°C, humidity of 25±2°C, and receiving time of 30 h to obtain a cobalt-doped manganese oxide fiber membrane; 2 g of 2-MI was dissolved in 100 mL of anhydrous ethanol to obtain an anhydrous ethanol solution of 2-MI, and the prepared cobalt-doped manganese oxide fiber membrane was immersed in the anhydrous ethanol solution of 2-MI at 35°C for 12 h, then rinsed with anhydrous ethanol and deionized water, dried in an oven at 80°C, and then annealed in a muffle furnace at 450°C for 2 h to obtain an air purification material.
[0032] The average fiber diameter of the cobalt-doped manganese oxide fiber membrane in this embodiment is 345 nm, and the fiber thickness is uniform, the surface is smooth, the fiber structure morphology is good, and no beads appear. After ZIF-6 crystals grow along the surface of the manganese oxide fiber, the fiber diameter increases slightly, and the average diameter is 361 nm. After annealing, the PVP skeleton is gasified to obtain an air purification material with a three-dimensional network structure.
[0033] The BET specific surface area of the air purification material in this embodiment is 2601m 2 / g, porosity is 93.7%, pore volume is 2.65cm3 / g, and the pore size distribution is 1.3-1.6nm.
[0034] Example 3
[0035] In a glove box, 4.5 g of Mn(CH3COO)2·2H2O and 0.8 g of Co(CH3COO)2 were added to 6 mL of isopropanol and stirred for 5 h to obtain a sol. Ammonia water was added to adjust the pH of the sol to 6. 4 mL of isopropanol solution in which 0.3 g of polyvinyl pyrrolidone (molecular weight 30,000) was dissolved was added and stirred for 1 h to obtain a precursor solution, which was poured into a syringe for electrospinning. 2 The non-woven fabric was used as the receiving substrate, and the electrospinning process parameters were as follows: voltage of 20 V, injection speed of 0.08 mm / min, syringe inclination angle of 30° to the horizontal plane, receiving distance of 20 cm, receiving roller speed of 140 rpm, temperature of 25±2°C, humidity of 25±2°C, and receiving time of 30 h to obtain a cobalt-doped manganese oxide fiber membrane; 2 g of 2-MI was dissolved in 100 mL of anhydrous ethanol to obtain an anhydrous ethanol solution of 2-MI, and the prepared cobalt-doped manganese oxide fiber membrane was immersed in the anhydrous ethanol solution of 2-MI at 35°C for 12 h, then rinsed with anhydrous ethanol and deionized water, dried in an oven at 80°C, and then annealed in a muffle furnace at 500°C for 1 h to obtain an air purification material.
[0036] The average fiber diameter of the cobalt-doped manganese oxide fiber membrane in this embodiment is 360 nm, and the fiber thickness is uniform, the surface is smooth, the fiber structure morphology is good, and no beads appear. After ZIF-6 crystals grow along the surface of the manganese oxide fiber, the fiber diameter increases slightly, and the average diameter is 375 nm. After annealing, the PVP skeleton is gasified to obtain an air purification material with a three-dimensional network structure.
[0037] The BET specific surface area of the air purification material in this embodiment is 2675 m 2 / g, porosity is 94.1%, pore volume is 2.63cm 3 / g, and the pore size distribution is 1.3-1.6nm.
[0038] Example 4
[0039] In a glove box, 4.5 g of Mn(CH3COO)2·2H2O and 0.8 g of Co(CH3COO)2 were added to 6 mL of isopropanol and stirred for 5 h to obtain a sol. Ammonia water was added to adjust the pH of the sol to 5. 4 mL of isopropanol solution in which 0.3 g of polyvinyl pyrrolidone (molecular weight 25000) was dissolved was added and stirred for 1 h to obtain a precursor solution, which was poured into a syringe for electrospinning. 2The non-woven fabric was used as the receiving substrate, and the electrospinning process parameters were as follows: voltage of 15 V, injection speed of 0.08 mm / min, syringe inclination angle of 30° to the horizontal plane, receiving distance of 20 cm, receiving roller speed of 140 rpm, temperature of 25±2°C, humidity of 25±2°C, and receiving time of 30 h to obtain a cobalt-doped manganese oxide fiber membrane; 2 g of 2-MI was dissolved in 100 mL of anhydrous ethanol to obtain an anhydrous ethanol solution of 2-MI, and the prepared cobalt-doped manganese oxide fiber membrane was immersed in the anhydrous ethanol solution of 2-MI at 35°C for 12 h, then rinsed with anhydrous ethanol and deionized water, dried in an oven at 80°C, and then annealed in a muffle furnace at 500°C for 1 h to obtain an air purification material.
[0040] The fibers of the cobalt-doped manganese oxide fiber membrane in this embodiment are uniform in thickness, smooth in surface, good in fiber structure morphology, and no beads appear. After ZIF-6 crystals grow along the surface of the manganese oxide fiber, the fiber diameter increases slightly. After annealing, the PVP skeleton is gasified to obtain an air purification material with a three-dimensional network structure.
[0041] The BET specific surface area of the air purification material in this embodiment is 2624 m 2 / g, porosity is 93.7%, pore volume is 2.62cm 3 / g, and the pore size distribution is 1.3-1.6nm.
[0042] Comparative Example 1
[0043] The same as Example 3, except that the annealing treatment was not performed, and the air purification material was obtained after washing with anhydrous ethanol and deionized water and drying in an oven at 80°C.
[0044] The BET specific surface area of the air purification material in this comparative example is 1527 m 2 / g, porosity of 75.1%, pore volume of 2.50cm 3 / g, and the pore size distribution is 1.3-1.9nm.
[0045] Comparative Example 2
[0046] The same as Example 3, except that the molecular weight of polyvinyl pyrrolidone is 10000, the jet is unstable during the electrospinning process, and it is difficult to complete the spinning process, and the subsequent preparation and performance testing process is not carried out.
[0047] Comparative Example 3
[0048] Same as Example 3, except that the molecular weight of polyvinyl pyrrolidone is 40000, beads appear in the fiber, the average fiber diameter is 190nm, and the fiber thickness is uneven. After the ZIF-6 crystals are grown, the crystals are sparsely distributed and unevenly distributed, and clear crystals cannot be observed on the fiber surface by scanning electron microscopy.
[0049] Formaldehyde adsorption performance test:
[0050] A closed space was built at room temperature, and the formaldehyde solution was diluted with deionized water at a volume ratio of 1:50 and then sprayed. A formaldehyde tester (MEF500) was used to observe the formaldehyde data changes in the closed space in real time. When the formaldehyde tester detection data tended to be stable, the air purification materials of each embodiment and comparative example were placed in the closed space to test the formaldehyde adsorption performance. The formaldehyde removal rate calculation formula is as follows:
[0051] Q=(C0-C1) / C0×100%
[0052] Where, Q represents the formaldehyde removal rate (%), C0 represents the initial formaldehyde concentration (mg / m 3 ), C1 represents the final concentration of formaldehyde (mg / m 3 ).
[0053] The initial formaldehyde concentration in the confined space is controlled at 2 mg / m 3 , weigh 0.1g / m 3 The air purification materials of various embodiments and comparative examples were placed in a closed space for testing. The formaldehyde removal rate results after different time periods are shown in Table 1.
[0054] Table 1
[0055]
[0056]
[0057] It can be seen from Table 1 that the air purification material prepared in the embodiment of the present invention can achieve the effect of quickly purifying formaldehyde due to its three-dimensional network structure and large specific surface area, and has a good removal effect on formaldehyde.
[0058] The air purification materials prepared in Example 3 and Comparative Examples 1 and 3 were tested for filtration performance at an air flow rate of 32 L / min using a TSI8130A automatic filter material detector. The filtration efficiency of the air purification material in Example 3 was 96.7%, and the quality factor was 0.0513 Pa. -1 The filtration efficiency of the air purification material in Comparative Example 1 is 55.1%, and the quality factor is 0.0264Pa -1 The filtration efficiency of the air purification material in comparative example 3 is 67.1%, and the quality factor is 0.0357Pa -1Therefore, the air purification material prepared in the embodiment of the present invention has good filtering performance.
[0059] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing an air purification material, characterized in that: In a glove box, 4.5 g of Mn(CH3COO)2·2H2O and 0.8 g of Co(CH3COO)2 were added to 6 mL of isopropanol and stirred for 5 h to obtain a sol. Ammonia water was added to adjust the pH of the sol to 6. 4 mL of an isopropanol solution containing 0.3 g of polyvinyl pyrrolidone with a molecular weight of 15,000 was added and stirred for 1 h to obtain a precursor solution, which was poured into a syringe for electrospinning. 2 The non-woven fabric was used as the receiving substrate, and the electrospinning process parameters were as follows: voltage of 15 V, injection speed of 0.08 mm / min, syringe tilt angle of 30° to the horizontal plane, receiving distance of 20 cm, receiving roller speed of 140 rpm, temperature of 25±2°C, humidity of 25±2°C, receiving time of 30 h, and a cobalt-doped manganese oxide fiber membrane was obtained; 2 g of 2-methylimidazole was dissolved in 100 mL of anhydrous ethanol to obtain an anhydrous ethanol solution of 2-methylimidazole, and the prepared cobalt-doped manganese oxide fiber membrane was immersed in the anhydrous ethanol solution of 2-methylimidazole at 35°C for 12 h, then rinsed with anhydrous ethanol and deionized water, and dried in an oven at 80°C. Under heating, Co 2+ The ZIF-6 crystals were grown along the surface of the manganese oxide fiber after coordination reaction with 2-methylimidazole in the solution. The cobalt-doped manganese oxide fiber membrane was still intact after impregnation, and the growth of the metal organic framework material did not destroy the morphology of the fiber and did not block the internal pores of the fiber membrane. The ZIF-6 crystals were densely arranged on the fiber surface, and a rough structure appeared on the fiber surface. The fiber diameter increased slightly, and the average diameter was 352nm. Then, the fiber was annealed at 400℃ for 3h in a muffle furnace, and the PVP skeleton was gasified to obtain an air purification material with a three-dimensional network structure. The BET specific surface area of the air purification material is 2596 m 2 / g, porosity is 92.3%, pore volume is 2.61cm 3 / g, and the pore size distribution is 1.3-1.6nm.