An optical item with high light transmittance

By adopting a multi-layer coating structure on optical items, the transmittance of blue light is improved, the problem of color deviation caused by the low transmittance of blue light in existing optical items is solved, and the imaging effect is significantly improved.

CN115961247BActive Publication Date: 2024-10-11FUJIAN DAYOPTICS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211727919.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-31
Publication Date
2024-10-11
Estimated Expiration
2042-12-31

Smart Images

  • Figure CN115961247B_ABST
    Figure CN115961247B_ABST
Patent Text Reader

Abstract

An optical article with high light transmittance includes a base layer, a first coating layer disposed on one side of the base layer, and a second coating layer disposed on one side of the base layer, wherein the first coating layer is (MgF2 / TiO2)xMgF2, and the second coating layer is (SiO2 / Ta2O5)xSiO2. In the present invention, by setting the first coating layer to be (MgF2 / TiO2)xMgF2 and the second coating layer to be (SiO2 / Ta2O5)xSiO2, the transmittance of blue light in the optical article is increased, the imaging effect of the optical article is improved, and the color deviation of the object is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of optical articles, in particular to an optical article with high light transmittance. Background Art

[0002] In existing optical products, a transparent film is coated on the surface of the base layer, and the interference phenomenon between the film medium and the specific wavelength is used to effectively reduce the transmittance or reflection of the wavelength of blue light of 400nm to 470nm. Alternatively, a specific color is dyed on the surface of the base layer, and the RGB primary colors are used to produce complementary colors, which are defined in physical vision as the relationship between colored light and object reflection, so that the wavelength of blue light of 400nm to 470nm can effectively reduce the light intensity, absorb or change the wavelength.

[0003] Using a spectrometer to scan and inspect existing optical items, the transmittance of lens sample 1 at a cutoff wavelength of 383nm reached 2%, the transmittance of lens sample 2 at a cutoff wavelength of 384nm reached 2%, and the transmittance of lens sample 3 at a cutoff wavelength of 390nm reached 2%. In addition, the three samples had a transmittance of 93% at a blue light wavelength of 450nm, 97% at a green light wavelength of 550nm, and 99.3% at a red light wavelength of 650nm.

[0004] At present, if optical objects block too much blue light, the objects will appear too dark, causing color deviation and reducing the penetration of blue light. Summary of the invention

[0005] The present invention provides an optical article with high light transmittance, the main purpose of which is to overcome the defect that the blue light transmittance in the existing optical articles is low, making the object look too dark and causing color deviation of the object.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] An optical article with high light transmittance, comprising a base layer, a first coating layer coated on one side of the base layer, and a second coating layer coated on the other side of the base layer, wherein the first coating layer is (MgF2 / TiO2) x MgF2, the second coating layer is (SiO2 / Ta2O5) x SiO2.

[0008] Further, in the (MgF2 / TiO2) x In MgF2, TiO2 is a high refractive index material with a refractive index of 2.54, and magnesium fluoride (MgF2) is a low refractive index material with a refractive index of 1.3.

[0009] Further, in the (SiO2 / Ta2O5) xTa2O5 in SiO2 is a high refractive index material with a refractive index of 2.2, and silicon dioxide (SiO2) is a low refractive index material with a refractive index of 1.47.

[0010] Furthermore, the base layer is borosilicate crown glass with a refractive index of 1.52 and an incident angle of 0 degree.

[0011] Furthermore, the first coating layer has a fifteen-layer structure, and the thickness of each layer is air|1.66L, 0.75H, 0.7L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.55L, 0.89H, 0.4L|base layer, and H and L represent the thickness of quarter-wavelength high and low refractive index film layers, respectively.

[0012] Furthermore, the second coating layer has a fifteen-layer structure, and the thickness of each layer is air|2L, 0.66H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.55L, 0.66H, 0.44L|base layer, where H and L represent the thickness of quarter-wavelength high and low refractive index film layers, respectively.

[0013] Furthermore, the first coating layer has a twenty-three-layer structure, and the thickness of each layer is air|1.66L, 0.76H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.62L, 0.99H, 0.62L, 0.99H, 0.99H, 0.56L, 0.88H, 0.56L, 0.88H, 0.56L, 0.88H, 0.42L, 0.51H, 0.42L|base layer, where H and L represent the thickness of quarter-wavelength high and low refractive index films, respectively.

[0014] Furthermore, the second coating layer has a twenty-three-layer structure, and the thickness of each layer is air|1.47L, 0.66H, 0.81L, 0.77H, 0.81L, 0.77H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.44H, 0.73L|base layer, and H and L represent the thickness of quarter-wavelength high and low refractive index film layers, respectively.

[0015] Furthermore, it also includes a third coating layer coated on the other side of the first coating layer, the third coating layer includes a first silicon dioxide film, multiple layers of first titanium pentoxide films and multiple layers of second silicon dioxide films, each layer of the second silicon dioxide film is coated with a layer of the first titanium pentoxide film on both sides respectively, the thickness of the first titanium pentoxide film is greater than the thickness of the second silicon dioxide film, the outermost layer of the first titanium pentoxide film is coated on one side of the outermost second silicon dioxide film, the other side of the first layer of the first silicon dioxide film is connected to the first coating layer by deepening optical glue, the thickness of the second silicon dioxide film is A times the optical thickness of a quarter wavelength, the thickness of the first titanium pentoxide film is A times the optical thickness of a quarter wavelength, and the value range of A is 0.5 to 1.5.

[0016] Furthermore, the thickness of the base layer is 0.3186 mm, the processing thickness tolerance is ±0.002 mm, and the optical axis of the base layer is parallel to the light-transmitting surface.

[0017] Compared with the prior art, the beneficial effects produced by the present invention are:

[0018] The invention has a simple structure and strong practicability. By setting the first coating layer to be (MgF2 / TiO2) x MgF2, the second coating layer is (SiO2 / Ta2O5) x SiO2 increases the transmittance of optical objects in blue light, improves the imaging effect of optical objects, and reduces the color deviation of objects.

[0019] In the present invention, the first coating layer is set to a fifteen-layer structure, and the thickness of each layer is air|1.66L, 0.75H, 0.7L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.55L, 0.89H, 0.4L|base layer, so that the transmittance of the first coating layer at an ultraviolet light wavelength of 400nm is 5%, the transmittance at a blue light wavelength of 450nm is 97.2%, the transmittance at a yellow-green light wavelength of 550nm is 95.6%, and the transmittance at a red light wavelength of 650nm is 98.8%.

[0020] In the present invention, the second coating layer is set to a fifteen-layer structure, and the thickness of each layer is air|2L, 0.66H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.55L, 0.66H, 0.44L|base layer, so that the second coating layer has a transmittance of 5% at an ultraviolet light wavelength of 400nm, a transmittance of 97.2% at a blue light wavelength of 450nm, a transmittance of 95.8% at a yellow-green light wavelength of 550nm, and a transmittance of 98.8% at a red light wavelength of 650nm.

[0021] In the present invention, the first coating layer is set to a twenty-three-layer structure, and the thickness of each layer is air|1.66L, 0.76H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.62L, 0.99H, 0.62L, 0.99H, 0.56L, 0.88H, 0.56L, 0.88H, 0.56L, 0.88H, 0.42L, 0.51H, 0.42L|base layer, so that the transmittance of the first coating layer at an ultraviolet light wavelength of 380nm is 2%, the transmittance at a blue light wavelength of 450nm is 99.1%, the transmittance at a yellow-green light wavelength of 550nm is 96.4%, and the transmittance at a red light wavelength of 650nm is 95.5%.

[0022] In the present invention, the second coating layer is arranged to have a twenty-three-layer structure, and the thickness of each layer is air|1.47L, 0.66H, 0.81L, 0.77H, 0.81L, 0.77H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.44H, 0.73L|base layer, so that the transmittance of the second coating layer at an ultraviolet light wavelength of 380nm is 2%, the transmittance at a blue light wavelength of 450nm is 99.1%, the transmittance at a yellow-green light wavelength of 550nm is 96.5%, and the transmittance at a red light wavelength of 650nm is 95.6%. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a structural schematic diagram of the present invention.

[0024] Figure 2 (MgF2 / TiO2) x Transmittance spectra of 15-layer and 23-layer MgF2 structures.

[0025] Figure 3(SiO2 / Ta2O5) x Transmittance spectra of SiO2 fifteen-layer structure and twenty-three-layer structure.

[0026] Figure 4 This is a schematic diagram of the structure of the third embodiment.

[0027] Figure 5 This is the blue light penetration spectrum of brown 20% anti-blue light lenses.

[0028] Figure 6 This is a structural diagram of Embodiment 5.

[0029] Figure 7 Schematic diagram of the optical path in Embodiment 5.

[0030] Figure 8 This is a structural diagram of Embodiment 7.

[0031] Fig. 9 4 is a flow chart of the steps of the dyeing method in Example 4. DETAILED DESCRIPTION

[0032] The specific embodiments of the present invention will be described below with reference to the accompanying drawings.

[0033] Embodiment 1, refer to Figure 1 An optical article with high light transmittance includes a base layer 12, a first coating layer 11 coated on one side of the base layer 12, and a second coating layer 13 coated on the other side of the base layer 12. The base layer 12 can be made into a lens shape.

[0034] Reference Figure 1 , the first coating layer 11 is (MgF2 / TiO2) x MgF2, the second coating layer 13 is (SiO2 / Ta2O5) x SiO2.

[0035] Reference Figure 1 By setting the first coating layer 11 to (MgF2 / TiO2) x MgF2, the second coating layer 13 is (SiO2 / Ta2O5) x SiO2 increases the penetration of blue light in optical objects, improves the imaging effect of optical objects, and reduces color deviation of objects.

[0036] Reference Figure 1 , in (MgF2 / TiO2) x MgF2 and (SiO2 / Ta2O5) x The value of X in SiO2 is 7 or 11. In this embodiment, the specific (MgF2 / TiO2)xMgF2 is (MgF2 / TiO2 ) 7MgF2 or (MgF2 / TiO2) 11 MgF2, (SiO2 / Ta2O5) x SiO2 is (SiO2 / Ta2O5) 7 SiO2 or (SiO2 / Ta2O5) 11 SiO2.

[0037] Reference Figure 1 , in (MgF2 / TiO2) x In MgF2, titanium dioxide (TiO2) is a high refractive index material with a refractive index of 2.54, and magnesium fluoride (MgF2) is a low refractive index material with a refractive index of 1.3.

[0038] Reference Figure 1 , in (SiO2 / Ta2O5) x Tantalum pentoxide (Ta2O5) in SiO2 is a high refractive index material with a refractive index of 2.2, and silicon dioxide (SiO2) is a low refractive index material with a refractive index of 1.47.

[0039] Reference Figure 1 The base layer 12 is borosilicate crown glass with a refractive index of 1.52 and an incident angle of 0 degrees.

[0040] Reference Figure 1 and Figure 2 The first coating layer 11 is a 15-layer structure, and the thickness of each layer is air|1.66L, 0.75H, 0.7L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.55L, 0.89H, 0.4L|base layer 12, so that the optical article has a transmittance of 5% at an ultraviolet wavelength of 400nm, a transmittance of 97.2% at a blue wavelength of 450nm, a transmittance of 95.6% at a yellow-green wavelength of 550nm, and a transmittance of 98.8% at a red wavelength of 650nm. The thickness of the first coating layer 11 is 694nm.

[0041] Reference Figure 1 and Figure 3The second coating layer 13 has a fifteen-layer structure, and the thickness of each layer is air|2L, 0.66H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.55L, 0.66H, 0.44L|base layer 12, so that the optical article has a transmittance of 5% at an ultraviolet light wavelength of 400nm, a transmittance of 97.2% at a blue light wavelength of 450nm, a transmittance of 95.8% at a yellow-green light wavelength of 550nm, and a transmittance of 98.8% at a red light wavelength of 650nm. The thickness of the second coating layer 13 is 741nm.

[0042] In this embodiment, H and L represent the thickness of the quarter-wavelength high and low refractive index film layers, respectively.

[0043] Reference Figure 1 , Figure 2 and Figure 3 In this embodiment, the cutoff wavelength of the fifteen-layer thin film structure of the first coating layer 11 has a transmittance of 4.4% at 373nm, which is 2.4% different from the cutoff wavelength of the existing lens of 2% at 383nm-389nm. Its transmittance at the wavelength of blue light 450nm, yellow-green light 550nm, and red light 650nm is about 1-2% higher than that of the existing lens.

[0044] Reference Figure 1 , Figure 2 and Figure 3 In this embodiment, the cutoff wavelength of the fifteen-layer thin film structure of the second coating layer 13 has a transmittance of 2.1% at 390nm, which is similar to the 2% transmittance of the existing lens at the cutoff wavelength of 383nm~389nm. Its transmittance at the wavelength of blue light 450nm, yellow-green light 550nm, and red light 650nm is about 1~2% higher than that of the existing lens.

[0045] Reference Figure 1 , Figure 2 and Figure 3 In this embodiment, the ultraviolet / visible light (UV / VIS) spectrometer used detects the transmission spectrum of the lens to detect the optical transmittance of the lens in the visible light band. The measurement band is from ultraviolet (UV) to near infrared (NIR) band, and the wavelength measurement range is 200 to 1000nm.

[0046] Reference Figure 1 After polishing both sides of the base layer 12, one side of the first coating layer 11 is coated on one side of the base layer 12 by deepening the photoresist, and one side of the second coating layer 13 is coated on the other side of the base layer 12 by deepening the photoresist.

[0047] Deepening of optical glue: After optical glue is applied, it can be placed in a pressure furnace for deepening and baking for 60 to 100 hours. The coating temperature is 180 to 220°C and the vacuum degree is 1.5 to 3.5*10 -3 Pa, the temperature of the pressure furnace is less than 300°C, so that the third coating layer 17 is more firmly arranged on the first coating layer 11, so that the third coating layer 17 is not easy to fall off from the first coating layer 11 and no glue is needed.

[0048] Example 2, refer to Figure 1 , Figure 2 and Figure 3 The difference between the second embodiment and the first embodiment is that the first coating layer 11 is a twenty-three-layer structure, and the thickness of each layer is air|1.66L, 0.76H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.62L, 0.99H, 0.62L, 0.99H, 0.56L, 0.88H, 0.56L, 0.8 8H, 0.56L, 0.88H, 0.42L, 0.51H, 0.42L|base layer 12, so that the transmittance of the first coating layer 11 at the ultraviolet light wavelength of 380nm is 2%, the transmittance at the blue light wavelength of 450nm is 99.1%, the transmittance at the yellow-green light wavelength of 550nm is 96.4%, the transmittance at the red light wavelength of 650nm is 95.5%, and the thickness of the first coating layer 11 is 979nm.

[0049] Reference Figure 1 , Figure 2 and Figure 3 The second coating layer 13 has a twenty-three-layer structure, and the thickness of each layer is air|1.47L, 0.66H, 0.81L, 0.77H, 0.81L, 0.77H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.44H, 0.73L|base layer 12, so that the transmittance of the second coating layer 13 at the ultraviolet light wavelength of 380nm is 2%, the transmittance at the blue light wavelength of 450nm is 99.1%, the transmittance at the yellow-green light wavelength of 550nm is 96.5%, and the transmittance at the red light wavelength of 650nm is 95.6%. The thickness of the second coating layer 13 is 1100nm.

[0050] In this embodiment, H and L represent the thickness of the quarter-wavelength high and low refractive index film layers, respectively.

[0051] Reference Figure 1 , Figure 2 and Figure 3In this embodiment, the cutoff wavelength of the twenty-three-layer thin film structure of the first coating layer is 380nm and its transmittance is 3.9%, which is similar to the 2% transmittance of the existing lens at the cutoff wavelength of 383nm~389nm. Its transmittance at the wavelength of blue light 450nm is 5% higher than that of the existing lens, and the transmittance at the wavelength of yellow-green light 550nm and red light 650nm is about 3~5% lower than that of the existing lens.

[0052] Reference Figure 1 , Figure 2 and Figure 3 In this embodiment, the cutoff wavelength of the twenty-three thin films of the second coating layer 13 has a transmittance of 1.5% at 390nm, which is 0.5% different from the cutoff wavelength of 2% at 383nm-389nm on the existing lens. Its transmittance at 450nm blue light, 550nm yellow-green light, and 650nm red light is about 3-5% higher than that of the existing lens.

[0053] The other structures are similar to those of the first embodiment and will not be described in detail here.

[0054] Example 3, refer to Figure 4 The difference between the third embodiment and the first embodiment is that the optical article further includes a third coating layer 17 coated on the other side of the first coating layer 11, and the third coating layer 17 and the first coating layer 11 are connected to each other by using a deep optical adhesive.

[0055] Reference Figure 4 The third coating layer 17 includes a first silicon dioxide film 15, a plurality of first titanium pentoxide films 16 and a plurality of second silicon dioxide films 14. Both sides of each second silicon dioxide film 14 are coated with a first titanium pentoxide film 16, and the thickness of the first titanium pentoxide film 16 is greater than that of the second silicon dioxide film 14. The outermost first titanium pentoxide film 16 is coated on one side of the outermost second silicon dioxide film 14, and the other side of the first silicon dioxide film 15 is connected to the first coating layer 11 by deepening the optical adhesive.

[0056] Reference Figure 4 The third coating layer is formed into a plurality of second silicon dioxide films 14 and a plurality of first titanium pentoxide films 16. Both sides of each second silicon dioxide film 14 are coated with a first titanium pentoxide film 16. The outermost first titanium pentoxide film 16 is coated on one side of the outermost second silicon dioxide film 14. The thickness of the first titanium pentoxide film 16 is greater than that of the second silicon dioxide film 14, thereby improving the clarity of the lens and making the lens have a better imaging effect.

[0057] Reference Figure 4, each layer of the second silicon dioxide film 14 is coated with a first titanium pentoxide film 16 on both sides thereof. In this embodiment, a plurality of second silicon dioxide films 14 and a plurality of first titanium pentoxide films 16 are stacked together, so that a layer of the second silicon dioxide film 14 is sandwiched between two layers of the first titanium pentoxide film 16, and the innermost layer of the first titanium pentoxide film 16 is coated on the first silicon dioxide film 15, and the thickness of the first titanium pentoxide film 16 is greater than that of the second silicon dioxide film 14.

[0058] Reference Figure 4 The refractive index of the base layer 12 in the light-sensitive band of 400nm to 950nm is less than 1.55. In this embodiment, the refractive index of the base layer 12 in the light-sensitive band of 400nm, 550nm and 700nm is preferably less than 1.55.

[0059] Reference Figure 4 The thickness of the second silicon dioxide film 14 is A times the optical thickness of a quarter wavelength, and the thickness of the first titanium pentoxide film 16 is A times the optical thickness of a quarter wavelength. The value range of A is 0.5 to 1.5, so that when the reflection angle of visible light or infrared light is 0 degrees, the reflectivity of the optical article is greater than 4%, and the transmittance in the visible light or infrared light region is about 94% to 96%. The optical thickness refers to the thickness of the material multiplied by its refractive index, and a quarter of the optical thickness is 1 / 4 multiplied by λ. λ is the wavelength of the light beam.

[0060] Reference Figure 4 When the reflection angle of visible light or infrared light is 45 degrees, the reflectivity is greater than 6%. The transmittance in the visible light and infrared light region is about 92% to 98%.

[0061] Reference Figure 4 , when the reflection angle of visible light or infrared light is 50 degrees, the reflectivity is greater than 6%. So it is used to reflect visible light.

[0062] Reference Figure 4 The refractive index of the second silicon dioxide film 14 is 1.4 to 1.5, and the refractive index of the first titanium pentoxide film 16 is 2.4 to 2.6.

[0063] Reference Figure 4 The total number of layers of the first titanium pentoxide film 16 is seven to eight layers, and the total number of layers of the second silicon dioxide film 14 is six to seven layers.

[0064] Reference Figure 4, the total number of layers of the first titanium pentoxide film 16 is eight, and the total number of layers of the second silicon dioxide film 14 is seven. For example, an optical coating machine is used to coat the first layer of the first titanium pentoxide film 16 on the first silicon dioxide film 15, and the first layer of the second silicon dioxide film 14 is coated on the first layer of the first titanium pentoxide film 16. The seven layers of the second silicon dioxide film 14 and the eight layers of the first titanium pentoxide film 16 are cyclically stacked and coated together until the eighth layer of the first titanium pentoxide film 16 is coated on the seventh layer of the second silicon dioxide film 14, and then the coating is terminated.

[0065] Reference Figure 4 A third coating layer 17 is formed by stacking a plurality of layers of a first titanium pentoxide film 16 with a higher refractive index and a second silicon dioxide film 14 with a lower refractive index. The third coating layer 17 protects the outer surface of one side of the first coating layer 11, so that the outer surface of the first coating layer 11 is not easily damaged after being impacted by the outside.

[0066] Reference Figure 4 In this embodiment, the specific thickness of the first titanium pentoxide film 16 and the second silicon dioxide film 14 should be determined according to the requirements of light reflectivity. The number of layers of the first titanium pentoxide film 16 and the second silicon dioxide film 14 is determined according to the requirements of light reflectivity. An evaluation function F is used to determine whether the optical thickness of the third coating layer 17 is improved. The improvement index is the evaluation function F: Where I0(λk) is the ideal target value, I(λk) is the design value, is the weight on the wavelength λk. When F becomes smaller, it means there is improvement.

[0067] Reference Figure 4 In this embodiment, the first coating layer 11 and the other side of the first silicon dioxide film 15 of the third coating layer 17 are photo-bonded together.

[0068] Deepening of optical glue: After optical glue is applied, it can be placed in a pressure furnace for deepening and baking for 60 to 100 hours. The coating temperature is 180 to 220°C and the vacuum degree is 1.5 to 3.5*10 -3 Pa, the temperature of the pressure furnace is less than 300° C., so that the third coating layer 17 is more firmly arranged on the first coating layer 11, so that the third coating layer 17 is not easy to fall off from the first coating layer 11 and no glue is needed.

[0069] The other structures are similar to those of the first embodiment and will not be described in detail here.

[0070] Embodiment 4, referring to Figure 1 , Figure 5 and Fig. 9The difference between the fourth embodiment and the first embodiment is that: in the present embodiment, the optical article is a lens, the base layer 12 is a borosilicate crown glass, the color of the base layer 12 is a brown 20% anti-blue light lens, and the dyeing method of the optical article includes the following steps: 1. Use an ultrasonic tank to vibrate the lens or use alcohol to remove impurities on the surface of the lens; 2. Put the lens on a fixed clamp and put it into a dye tank for dyeing; 3. Take out the sample color lens and put it on a white paper; 4. The dye tank has a constant temperature device (temperature is about 80℃~90℃) to maintain a certain temperature of the dye; 5. When the lens leaves the dye tank, it should be washed with clean water immediately to prevent uneven color, and the sample color piece placed on the white paper should be compared with the color or concentration, so as to achieve the correct color through this cycle.

[0071] Reference Figure 1 , Figure 5 and Fig. 9 When the lens enters the high-temperature dye, as the temperature rises, the molecular network structure of the lens structure gradually expands and microscopic pores appear. When the vibration frequency increases, the small molecules in the dye are accelerated to diffuse into the lens. When the thermal energy is further increased, the kinetic energy of the dye activates the small molecules to enter the lens and present a concentration difference. When the temperature drops, the pigment cools inside the lens, and the dye depth is about 0.3 to 0.1 mm.

[0072] The basic colors of dyes are black, green, blue, red, yellow, gray, etc., with R, G, and B as the main colors. In order to strengthen the color ratio of the dye, auxiliary dyes must be used. For example, white agent can deepen the color and even make the blue darker, but an excessive amount will cause the lens surface to appear striped; yellow agent can make the color lighter and turn yellow, but an excessive amount will not dissolve easily and cause uneven color; black agent can make the color lighter and turn brown, but an excessive amount will cause uneven dyeing or black stripes; depending on the material characteristics of the lens, the dye and temperature will also be different.

[0073] Table 1: Transmittance test table of lenses of different colors using a spectrometer.

[0074] Optical items Spectrometer detects transmittance Pink 78.97% green 78.93% blue 91.39% Purple 87.82% Brown 20% 85.94% Brown 30% 77.23% Blue film 92.52% yellow 70.23%

[0075] Table 2: CIExy coordinate color deviation percentage table for optical items.

[0076] Optical items x Y x+y Pink 1.17% 7.65% 8.82% green 0.97% 16.29% 17.26% blue 3.44% 7.36% 10.8% Purple 2.34% 6.77% 9.11% Brown 20% 1.75% 0.79% 2.54% Brown 30% 0.13% 6.67% 6.8% Blue film 1.95% 0.98% 2.93% yellow 0.84% 20.41% 21.25

[0077] Blue optical items have a relatively high blue light transmittance, while other colors of optical items have a relatively low blue light transmittance. Both brown 20% optical items and blue-filmed lenses are resistant to blue light and have a color deviation of only 3%. However, the blocking rate of blue-filmed optical items is only about 8%. Therefore, choose brown 20% optical items because they can block about 17% of blue light and are less expensive.

[0078] The ultraviolet / visible light (UV / VIS) spectrometer used in this embodiment detects the transmission spectrum of the lens to detect the optical transmittance of the lens in the visible light band. The measurement band is from ultraviolet (UV) to near infrared (NIR) band, and the wavelength measurement range is 200 to 1000nm.

[0079] The other structures are similar to those of the first embodiment and will not be described in detail here.

[0080] Example 5, refer to Figure 6 and Figure 7 The difference between the fifth embodiment and the first embodiment is that the optical article 1 further includes at least one incident surface of the optical axis 311 arranged on the outer side of the base layer 12, at least one first light-transmitting surface arranged on one side of the base layer 12, and at least one second light-transmitting surface arranged on the other side of the base layer 12.

[0081] Reference Figure 6 and Figure 7 The first light-transmitting surface includes at least one first polishing surface 121 disposed on one side of the base layer 12 and at least one second polishing surface 122 disposed on a side of the first polishing surface 121 away from the base layer 12 .

[0082] Reference Figure 6 and Figure 7 The second light-transmitting surface includes at least one second polished surface 122 disposed on the other side of the base layer 12 and at least one second coating layer 13 disposed on the second polished surface 122 away from the base layer 12 .

[0083] Reference Figure 6 and Figure 7 The outer dimensions of the base layer 12 can be circular, rectangular or square.

[0084] Reference Figure 6 and Figure 7 The thickness of the base layer 12 is 0.3186 mm, the processing thickness tolerance is ±0.002 mm, and the optical axis 311 of the base layer 12 is parallel to the light-transmitting surface. The optical axis 311 can be 45° or any other angle parallel to the light-transmitting surface.

[0085] Reference Figure 6 and Figure 7 The base layer 12 is made of quartz crystal material, that is, the processing thickness of the quartz crystal material is 0.3186mm, and the processing thickness tolerance is ±0.0002mm. The optical axis 311 is parallel to the light-transmitting surface of the quartz crystal. The base layer 12 can be used for red light with a wavelength of 633nm, green light with a wavelength of 532nm, or blue light with a wavelength of 461nm, which can meet the effect of optical articles. The wave plate is a single-piece low-grade quartz wave plate processed from quartz crystal. This single-piece structure wave plate has a higher damage threshold.

[0086] Reference Figure 6 and Figure 7 By setting the base layer 12 to be made of quartz crystal material, compared with magnesium fluoride crystal material, the quartz crystal material has higher hardness and is easy to be polished and processed to form a light-transmitting surface. On the one hand, it reduces the material cost of the optical article, reduces the processing difficulty and the processing cost. On the other hand, it improves the processing efficiency and is convenient for batch processing and production, achieving a two-fold effect.

[0087] Refer to Figure 6 and Figure 7 The included angle between the optical axis 311 and the first light-transmitting surface is X, where 0° < X < 360°, and the angle of X is preferably 45°.

[0088] Refer to Figure 6 and Figure 7 The included angle between the optical axis 311 and the second light-transmitting surface is Y, where 0° < Y < 360°, and the angle of Y is preferably 45°.

[0089] Refer to Figure 6 and Figure 7 The second polished surface 122 is connected to the first polished surface 121 in a way of plating light-transmitting deepening optical glue.

[0090] Refer to Figure 6 and Figure 7 The second coating layer 13 is connected to the second polished surface 122 in a way of plating deepening optical glue.

[0091] Refer to Figure 6 and Figure 7 The optical path design principle is: According to the optical path difference calculation formula of the wave plate (No - Ne)D = ±(2k + 1)λ / 2 (k = 0, 1, 2......). Where No and Ne are the refractive indices of the O light and E light in the wave plate, D is the processed thickness of the wave plate, λ is the wavelength of the red, green and blue light sources, and K is a natural number. It is necessary to design a thickness D to make both sides of the equation hold. And at the same time, it meets the usage requirements of the red, green and blue light sources for the half-wave plate.

[0092] Refer to Figure 6 and Figure 7 In this embodiment, a square optical quartz crystal raw material is specifically selected. The optical axis 311 is the diagonal line, the direction of the optical axis 311 is parallel to the light-transmitting surface, the second polished surface 122 and the first polished surface 121. The thickness of the quartz crystal is processed to the size range of 0.3186mm ± 0.002mm, and a first coating layer and a second coating layer are plated on the crystal surface to reduce the surface reflection loss.

[0093] Refer to Figure 6 and Figure 7To ensure a high phase delay accuracy, the parallelism between the first polished surface 121 and the second polished surface 122 needs to be less than 3 seconds, and the optical axis 311 is controlled to form an angle of 45° with the square edge.

[0094] Reference Figure 6 and Figure 7 The optical path is: the incident light is linearly polarized light of red, green and blue wavelengths, and the electric vector vibration forms an angle of 45° with the optical axis 311 of the substrate 12, and the polarization state of the outgoing light is rotated 90° relative to the incident light.

[0095] Reference Figure 6 and Figure 7 For example, a beam of linearly polarized light with a wavelength of 461 nm, when it passes vertically through the base layer 12, the polarization direction of the outgoing light becomes horizontal.

[0096] Reference Figure 6 and Figure 7 By setting the second polishing surface 122 on the first polishing surface 121, the reflection loss of the red, green and blue light sources on the surface of the base layer 12 is reduced, the damage threshold of the optical article is increased, and the service life of the optical article is extended.

[0097] Reference Figure 6 and Figure 7 By arranging the second coating layer 13 on the second polished surface 122, the reflection loss of the red, green and blue light sources on the surface of the base layer 12 is reduced, the damage threshold of the optical article is increased, and the service life of the optical article is extended.

[0098] Reference Figure 6 The manufacturing method of the optical article comprises the following steps:

[0099] Step S001, cutting the quartz crystal into a base layer 12 with a thickness of 0.3186 mm, the processing thickness tolerance of the base layer 12 is ±0.0002 mm, and cutting the shape of the quartz crystal into a circle, a rectangle or a square;

[0100] Step S002, polishing the left and right sides of the quartz crystal, so that one side of the quartz crystal forms a first polished surface 121, and the other side of the quartz crystal forms a second polished surface 122;

[0101] Step S003, connecting the first polishing surface 121 with the second polishing surface 122 by means of light-deepening polishing glue;

[0102] Step S004, connecting the second polished surface 122 with the second coating layer 13 by deepening the optical adhesive;

[0103] 6, the first coating layer 11 is (MgF2 / TiO2) xMgF2, the second coating layer 13 is (SiO2 / Ta2O5) x SiO2.

[0104] Reference Figure 6 By setting the first coating layer 11 to (MgF2 / TiO2) x MgF2, the second coating layer 13 is (SiO2 / Ta2O5) x SiO2 increases the blue light penetration of optical objects, improves the imaging effect of lenses, and reduces color deviation of objects.

[0105] Reference Figure 6 , in (MgF2 / TiO2) x MgF2 and (SiO2 / Ta2O5) x The value of X in SiO2 is 7 or 11. In this embodiment, the specific (MgF2 / TiO2) x MgF2 is (MgF2 / TiO2) 7 MgF2 or (MgF2 / TiO2) 11 MgF2, (SiO2 / Ta2O5) x SiO2 is (SiO2 / Ta2O5) 7 SiO2 or (SiO2 / Ta2O5) 11 SiO2.

[0106] Reference Figure 6 , in (MgF2 / TiO2) x In MgF2, titanium dioxide (TiO2) is a high refractive index material with a refractive index of 2.54, and magnesium fluoride (MgF2) is a low refractive index material with a refractive index of 1.3.

[0107] Reference Figure 6 , in (SiO2 / Ta2O5) x Tantalum pentoxide (Ta2O5) in SiO2 is a high refractive index material with a refractive index of 2.2, and silicon dioxide (SiO2) is a low refractive index material with a refractive index of 1.47.

[0108] Reference Figure 6 In this embodiment, the quartz crystal material is specifically processed to a thickness of 0.3186 mm, and the processing thickness tolerance is ±0.0002 mm. The optical axis 311 is parallel to the light-transmitting surface of the quartz crystal, so that the base layer 12 becomes a single-piece low-level quartz wave plate, and the first coating layer 11 and the second coating layer 13 are respectively coated on the surface.

[0109] The optical article in this embodiment is a single low-order wave plate, which has a simple structure, low cost, high damage threshold, and is suitable for mass production.

[0110] The half wave plate is an optical device often used in polarization light paths. When linearly polarized light is incident vertically on the half wave plate in the light path, the transmitted light is still linearly polarized light. If the angle between the vibration plane and the crystal optical axis 311 at the time of incidence is θ, then the vibration plane of the transmitted linearly polarized light rotates by 2θ from the original azimuth. For example, when θ=45°, the polarization angle of the polarized light can be rotated by 90° using a half wave plate. Therefore, half wave plates are widely used in polarization beam combining devices of laser systems. In laser systems, especially in red, green and blue three-wavelength combined laser systems, half wave plates with high transmittance, high phase delay accuracy and high damage threshold are required.

[0111] The other structures are similar to those of the first embodiment and will not be described in detail here.

[0112] Example 6, refer to Figure 1 The difference between the sixth embodiment and the first embodiment is that the base layer 12 is made of resin material, and the other structures are similar to those of the first embodiment, which will not be described here.

[0113] Embodiment 7, reference Figure 8 The difference between the seventh embodiment and the first embodiment is that the optical article further includes a fourth coating layer 87 coated on the other side of the first coating layer 11, and the fourth coating layer 87 and the first coating layer 11 are connected to each other by using a deep optical adhesive.

[0114] Reference Figure 8 The fourth coating layer 87 includes a third silicon dioxide film 85, a plurality of second titanium pentoxide films 86 and a plurality of fourth silicon dioxide films 84. Each layer of the second titanium pentoxide film 86 is coated with a layer of the fourth silicon dioxide film 84 on both sides. The thickness of the second titanium pentoxide film 86 is greater than that of the fourth silicon dioxide film 84. The innermost layer of the second titanium pentoxide film 86 is coated on one side of the third silicon dioxide film 85. The other side of the third silicon dioxide film 85 is connected to (MgF2 / TiO2)xMgF2 by deepening optical glue.

[0115] Reference Figure 8 The third coating layer is formed into a plurality of fourth silicon dioxide films 84 and a plurality of second titanium pentoxide films 86. Each of the two sides of the fourth silicon dioxide film 84 is coated with a second titanium pentoxide film 86. The innermost second titanium pentoxide film 86 is coated on the third silicon dioxide film 85. The thickness of the second titanium pentoxide film 86 is greater than that of the fourth silicon dioxide film 84. This improves the clarity of the lens and makes the lens have a better imaging effect.

[0116] Reference Figure 8A second titanium pentoxide film 86 is coated on both sides of each fourth silicon dioxide film 84. In this embodiment, multiple fourth silicon dioxide films 84 and multiple second titanium pentoxide films 86 are stacked together, so that one fourth silicon dioxide film 84 is sandwiched between two second titanium pentoxide films 86, and the outermost second titanium pentoxide film 86 is coated on the fourth silicon dioxide film 84. The thickness of the second titanium pentoxide film 86 is greater than that of the fourth silicon dioxide film 84.

[0117] Reference Figure 8 The refractive index of the base layer 12 in the light-sensitive band of 400nm to 950nm is less than 1.55. In this embodiment, the refractive index of the base layer 12 in the light-sensitive band of 400nm, 550nm and 700nm is preferably less than 1.55.

[0118] Reference Figure 8 The thickness of the fourth silicon dioxide film 84 is A times the optical thickness of a quarter wavelength, and the thickness of the second titanium pentoxide film 86 is A times the optical thickness of a quarter wavelength. The value range of A is 0.5 to 1.5, so that when the reflection angle of visible light or infrared light is 0 degrees, the reflectivity of the optical article is greater than 4%, and the transmittance in the visible light or infrared light region is about 94% to 96%.

[0119] Reference Figure 8 When the reflection angle of visible light or infrared light is 45 degrees, the reflectivity is greater than 6%. The transmittance in the visible light and infrared light region is about 92% to 98%.

[0120] Reference Figure 8 , when the reflection angle of visible light or infrared light is 50 degrees, the reflectivity is greater than 6%. So it is used to reflect visible light.

[0121] Reference Figure 8 , optical thickness is the thickness of the material multiplied by its refractive index, and one quarter of the optical thickness is 1 / 4 multiplied by λ. λ is the wavelength of the light beam.

[0122] Reference Figure 8 The refractive index of the fourth silicon dioxide film 84 is 1.4 to 1.5, and the refractive index of the second titanium pentoxide film 86 is 2.4 to 2.6.

[0123] Reference Figure 8 The total number of layers of the second titanium pentoxide film 86 is seven to eight layers, and the total number of layers of the fourth silicon dioxide film 84 is six to seven layers.

[0124] Reference Figure 8Taking the total number of layers of the second titanium pentoxide film 86 as eight and the total number of layers of the fourth silicon dioxide film 84 as seven as an example, an optical coating machine is used to coat the first layer of the second titanium pentoxide film 86 with the first layer of the fourth silicon dioxide film 84, and the second layer of the second titanium pentoxide film 86 is coated on the first layer of the fourth silicon dioxide film 84. The seven layers of the fourth silicon dioxide film 84 and the eight layers of the second titanium pentoxide film 86 are cyclically stacked and coated together until the eighth layer of the second titanium pentoxide film 86 is coated on the seventh layer of the fourth silicon dioxide film 84, and then the coating is terminated.

[0125] Reference Figure 8 A fourth coating layer 87 is formed by stacking multiple layers of a second titanium pentoxide film 86 with a higher refractive index and a fourth silicon dioxide film 84 with a lower refractive index. The fourth coating layer 87 protects the outer surface of one side of the first coating layer 11, so that the outer surface of the first coating layer 11 is not easily damaged after being impacted by the outside.

[0126] Reference Figure 4 In this embodiment, the specific thickness of the second titanium pentoxide film 86 and the fourth silicon dioxide film 84 should be determined according to the requirements of light reflectivity. The number of layers of the second titanium pentoxide film 86 and the fourth silicon dioxide film 84 is determined according to the requirements of light reflectivity. An evaluation function F is used to determine whether the optical thickness of the fourth coating layer 87 is improved. The improvement index is the evaluation function F: Where I0(λk) is the ideal target value, I(λk) is the design value, is the weight on the wavelength λk. When F becomes smaller, it means there is improvement.

[0127] Reference Figure 4 In this embodiment, the first coating layer 11 and the other side of the third silicon dioxide film 85 of the fourth coating layer 87 are photo-bonded together.

[0128] The other structures are similar to those of the first embodiment and will not be described in detail here.

[0129] The above is only a specific implementation of the present invention, but the design concept of the present invention is not limited thereto. Any non-substantial changes to the present invention using this concept shall be deemed as an infringement of the protection scope of the present invention.

Claims

1. An optical article with high light transmittance, characterized in that: The invention comprises a base layer, at least one first coating layer coated on one side of the base layer, and at least one second coating layer coated on the other side of the base layer, wherein the first coating layer is ((MgF2 / TiO2) x MgF2, the second coating layer is (SiO2 / Ta2O5) x SiO2, the first coating layer has a fifteen-layer structure, and the thickness of each layer is air |1.66L, 0.75H, 0.7L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.76L, 0.88H, 0.55L, 0.89H, 0.4L|base layer, H and L respectively represent the thickness of a quarter wavelength high and low refractive index film layers, the second coating layer has a fifteen-layer structure, and the thickness of each layer is air |2L, 0.66H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.8L, 0.88H, 0.55L, 0.66H, 0.44L|base layer, H and L respectively represent the thickness of a quarter wavelength high and low refractive index film layers.

2. An optical article with high light transmittance as claimed in claim 1, characterized in that: In the ((MgF2 / TiO2) x In MgF2, TiO2 is a high refractive index material with a refractive index of 2.54, and magnesium fluoride (MgF2) is a low refractive index material with a refractive index of 1.

3.

3. An optical article with high light transmittance as claimed in claim 1, characterized in that: In the (SiO2 / Ta2O5) x Ta2O5 in SiO2 is a high refractive index material with a refractive index of 2.2, and silicon dioxide (SiO2) is a low refractive index material with a refractive index of 1.

47.

4. An optical article with high light transmittance as claimed in claim 1, characterized in that: The base layer is borosilicate crown glass with a refractive index of 1.52 and an incident angle of 0 degree.

5. The optical article with high light transmittance as claimed in claim 1, characterized in that: It also includes a third coating layer coated on the other side of the first coating layer, the third coating layer includes a first silicon dioxide film, multiple layers of first titanium pentoxide films and multiple layers of second silicon dioxide films, each layer of the second silicon dioxide film is coated with a layer of the first titanium pentoxide film on both sides respectively, the thickness of the first titanium pentoxide film is greater than the thickness of the second silicon dioxide film, the outermost layer of the first titanium pentoxide film is coated on one side of the outermost second silicon dioxide film, the other side of the first layer of the first silicon dioxide film is connected to the first coating layer by deepening optical glue, the thickness of the second silicon dioxide film is A times the optical thickness of a quarter wavelength, the thickness of the first titanium pentoxide film is A times the optical thickness of a quarter wavelength, and the value range of A is 0.5 to 1.

5.

6. An optical article with high light transmittance as claimed in claim 1, characterized in that: The thickness of the base layer is 0.3186 mm, the processing thickness tolerance is ±0.002 mm, and the optical axis of the base layer is parallel to the light-transmitting surface.

7. An optical article with high light transmittance, characterized in that: The invention comprises a base layer, at least one first coating layer coated on one side of the base layer, and at least one second coating layer coated on the other side of the base layer, wherein the first coating layer is ((MgF2 / TiO2) x MgF2, the second coating layer is (SiO2 / Ta2O5) x SiO2, the first coating layer has a twenty-three-layer structure, and the thickness of each layer is air|1.66L, 0.76H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.69L, 0.99H, 0.62L, 0.99H, 0.62L, 0.99H, 0.56L, 0.88H, 0.56L, 0.88H, 0.56L, 0.88H, 0.42L, 0.51H, 0.42L|base layer, H and L represent quarter-wavelength high and low refractive index film layers, respectively. Film thickness: the second coating layer has a twenty-three-layer structure, and the thickness of each layer is air|1.47L, 0.66H, 0.81L, 0.77H, 0.81L, 0.77H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.87H, 0.81L, 0.44H, 0.73L|base layer, and H and L represent the thickness of quarter-wavelength high and low refractive index films, respectively.