A catalyst for preparing low-carbon olefins and its preparation method and application

By adding Cu, Group VIIA elements, alkali metals and halogens to the Fe100ZraCubAcXdOe catalyst to form small particle active components, the problem of insufficient selectivity of low carbon olefins in the synthesis gas Fischer-Tropsch synthesis catalyst is solved, and high CO conversion rate and selectivity are achieved sexual enhancement.

CN115970718BActive Publication Date: 2024-10-22CHIA TAI ENERGY MATERIALS DALIAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211676661.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-10-22
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

Existing synthesis gas Fischer-Tropsch synthesis catalysts have low low-carbon olefin selectivity under high CO conversion rates, making it difficult to effectively improve them.

Method used

Using Fe100ZraCubAcXdOe type catalyst, by adding Cu, Group VIIA elements, alkali metals and alkaline earth metals to the mixed oxide of iron and zirconium, combined with the addition of halogen, smaller particles of active components are formed to inhibit C5+ generation and hydrogenation reactions. , improve the selectivity of light olefins.

Benefits of technology

Under lower reaction pressure, high CO conversion (up to 98%) and high low-carbon olefin selectivity (up to 43%) were achieved, significantly improving the selectivity and activity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004017207150000101
    Figure BDA0004017207150000101
Patent Text Reader

Abstract

The present invention discloses a catalyst for preparing low-carbon olefins, a preparation method and an application thereof. The catalyst comprises the following composition: Fe 100 Zr a Cu b A c X d O e , wherein A is one or more elements of Group VIIA, and X is an auxiliary agent, including one or more alkali metal elements or (and) one or more alkaline earth metal elements. The catalyst of the present invention can achieve a CO single-pass conversion rate of more than 95% at a relatively low reaction pressure, and has a high selectivity for light olefins, and is suitable for industrial application in the direct conversion of synthesis gas to prepare light olefins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic chemistry and relates to a preparation method and application of a catalyst for directly converting synthesis gas into light olefins. Background Art

[0002] Light olefins (C2 = -C4 = ) is a particularly important petrochemical, natural gas chemical and coal chemical product, and is also a chemical raw material required for downstream polymer production. Foreign countries mostly produce light olefins by cracking light hydrocarbons, while domestically, light olefins are mainly produced by cracking naphtha. With the increasing depletion of oil resources, it is particularly important to study new technologies to replace traditional olefin production. Fischer-Tropsch synthesis (FTS) is one of the process routes for directly producing light olefins from synthesis gas. It is increasingly valued as a non-petroleum technology for producing light olefins. Iron-based catalysts are the focus of research on catalyst systems for direct preparation of light olefins from synthesis gas due to their low price, high water-gas shift activity, and high selectivity for light olefins, making them the most industrially valuable type of catalyst.

[0003] In the existing synthesis gas Fischer-Tropsch synthesis catalyst, the Fischer-Tropsch synthesis reaction product is widely distributed, and the selectivity of light olefins is relatively low. How to improve the selectivity of light olefins is a major challenge currently faced by researchers. Many researchers improve selectivity by adding some other components, such as alkali metals (Na, K, etc.), transition metals (Mn, Ru, etc.), and the effect of non-metals is less studied. As the patent document with publication number CN106607058A, a kind of iron-based catalyst and preparation method thereof for direct preparation of light olefins from synthesis gas are disclosed, and the excessive carbonization of the catalyst surface can be suppressed by introducing the poisoning of S or P so that the catalyst can run for a long time. As the patent document with publication number CN107413362A, a kind of ultra-high activity Fischer-Tropsch synthesis process is disclosed, by the introduction of carbon source or nitrogen source, the catalyst is provided with abundant pore structure, the particles are evenly dispersed, the surface is rich in abundant N-containing and O-containing functional groups, and its special structure can effectively prevent the agglomeration of particles, but the selectivity of light olefins is not high. In addition, the National Institute of Clean and Low-Carbon Energy published an article in Catalysts 2022, 12(8), 812, which prepared an iron-based catalyst with a silica carrier and a chlorine additive added by an impregnation method. The article showed that after adding the chlorine additive, the CO conversion rate was significantly reduced, but the products it targeted were mainly C5 + Carbon olefins. Summary of the invention

[0004] 1. Problem to be solved

[0005] The existing catalysts for direct preparation of light olefins from synthesis gas have low selectivity for light olefins at high CO conversion rates.

[0006] One of the objects of the present invention is to provide a catalyst with high selectivity;

[0007] At the same time, the present invention also provides a method for preparing the catalyst;

[0008] And, a method for directly preparing light olefins from synthesis gas using the catalyst.

[0009] 2. Technical solution

[0010] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0011] In a first aspect of the present invention, a catalyst for preparing light olefins is provided, wherein the catalyst comprises a substance as shown in the following formula (excluding impurities in the raw materials) calculated by atomic ratio:

[0012] Fe 100 Zr a Cu b A c X d O e

[0013] in,

[0014] The value range of a is 3.0 to 200.0; preferably 5 to 180; more preferably 5 to 150; and most preferably 10 to 150;

[0015] The value range of b is 0.2 to 30; preferably 0.5 to 25; more preferably 1.0 to 20; and most preferably 1.0 to 15;

[0016] The value range of c is 0.1 to 32; preferably 0.5 to 30; more preferably 1.0 to 30; and most preferably 1.0 to 25;

[0017] The value range of d is 0.1 to 50; preferably 0.5 to 40; more preferably 0.5 to 35; and most preferably 1.0 to 30;

[0018] e is the total number of oxygen atoms required to satisfy the valence of each element in the substance shown;

[0019] A is any one or more elements selected from Group VIIA;

[0020] X is any one or more alkali metal elements and / or any one or more alkaline earth metal elements.

[0021] It should be noted that the addition of halogen is the key to improving the conversion rate and selectivity of the catalyst for direct preparation of light olefins from synthesis gas, which can inhibit the C5 + The halogen can effectively improve the selectivity of olefins, especially low-carbon olefins, by inhibiting the further hydrogenation of olefins. In particular, the synergistic effect of halogen addition with iron oxide and zirconium oxide can make the active components form smaller particles while maintaining high catalytic activity.

[0022] Based on this, the range of values ​​of a and c is particularly important. Adding too much halogen elements will poison the catalyst and reduce the activity of the catalyst, while too little will not work. At the same time, too much zirconium oxide will cover the active components and affect the activity, while too little zirconium oxide will lose its additive effect and have a certain impact on the performance of the catalyst.

[0023] According to the catalyst of any embodiment of the first aspect of the present invention, A includes any one or more of F, Cl, Br, and I; most preferably, A is Cl or F.

[0024] According to the catalyst of any embodiment of the first aspect of the present invention, X includes any one or more of Be, Ca, Mg, Se, Ba, K, Na, Li, and Cs, and most preferably X is Ca, Mg, Ba, K, or Na.

[0025] The second aspect of the present invention provides a method for preparing a catalyst for preparing light olefins, comprising the following steps:

[0026] 1) preparing a mixed solution containing Fe and Zr, wherein the total metal ion concentration of Fe and Zr in the mixed solution is 0.1 mol / L to 3.0 mol / L;

[0027] Prepare a solution containing a precipitant, wherein the concentration of the precipitant in the solution is 0.1 mol / L to 3 mol / L, and the amount of the precipitant is to ensure complete precipitation of Fe and Zr ions;

[0028] 2) contacting and mixing the mixed solution in step 1) with a solution containing a precipitant to form a precipitate;

[0029] 3) aging and calcining the precipitate obtained in step 2) to obtain a mixed oxide of iron and zirconium, generally a mixed oxide composed of Fe2O3 and ZrO2;

[0030] 4) preparing a solution containing Cu, a Group VIIA element, and an alkali metal and / or an alkaline earth metal element as an impregnation solution;

[0031] 5) impregnating the mixed oxides of step 3) with the impregnation solution of step 4, and then drying and calcining to obtain a catalyst;

[0032] Wherein, the precipitant used includes one or more of ammonium carbonate, ammonium bicarbonate, ammonia water, sodium carbonate, urea, potassium carbonate, sodium hydroxide, and potassium hydroxide;

[0033] The Fe is derived from an Fe salt, and the Fe salt includes one or more of ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferric sulfate, and ferrous sulfate;

[0034] The Zr is derived from a Zr salt, and the Zr salt includes one or more of zirconium nitrate, zirconium oxychloride, and zirconium sulfate;

[0035] The Cu is derived from a Cu salt, and the Cu salt includes one or more of copper nitrate, copper chloride, and copper acetate;

[0036] The Group VIIA element may be introduced via a soluble salt with other elements in the catalyst, or one or more other acids or salts that do not introduce heteroatoms;

[0037] The pressure required for aging is normal pressure or self-increasing pressure in a closed polytetrafluoroethylene lined reactor.

[0038] According to the method for preparing a catalyst according to any embodiment of the second aspect of the present invention, in the step 2), a precipitate is obtained at a temperature of 40° C. to 180° C. and a pH value of 5 to 10.

[0039] According to the method for preparing a catalyst of any embodiment of the second aspect of the present invention, in the step 3), the aging time is 1 h to 20 h, and the temperature is 40° C. to 180° C.;

[0040] The calcination temperature is 350°C to 800°C, and the calcination time is 2h to 20h.

[0041] According to the method for preparing a catalyst of any embodiment of the second aspect of the present invention, in the step 3), after the aging of the precipitate is completed, it needs to be washed and dried, and then calcined;

[0042] The washing is performed until neutral or until no potassium or sodium is detected;

[0043] The drying temperature is 40° C. to 150° C., and the drying time is 6 h to 24 h.

[0044] According to the method for preparing the catalyst of any embodiment of the second aspect of the present invention, in the step 5), the calcination temperature is 350° C. to 800° C., and the calcination time is 2 h to 20 h;

[0045] The drying temperature is 40℃~150℃, and the drying time is 6h~24h.

[0046] The third aspect of the present invention provides a method for preparing light olefins, using any of the above catalysts, or a catalyst obtained by any of the above methods, to catalyze synthesis gas to form light olefins;

[0047] The steps include:

[0048] Prepare reducing gas, the reducing gas includes H2 and N2, and the volume content of H2 is not less than 20%;

[0049] Reducing the reducing gas; the reducing temperature is 300-550° C., the reducing pressure is 0.01-2.0 MPa, and the reducing time is 3-12 hours;

[0050] preparing a raw gas, wherein the raw gas comprises CO;

[0051] The raw gas is introduced into the reduction gas after the reduction treatment to carry out the reaction of preparing light olefins from the synthesis gas; the reaction temperature is 250-380° C., and the reaction pressure is 0.5-5.0 MPa;

[0052] Wherein, the molar ratio of H2 / CO is 0.5-3.

[0053] According to the method for preparing the catalyst of any embodiment of the third aspect of the present invention, a fixed bed reactor is used to catalyze the synthesis gas to form light olefins;

[0054] The gas space velocity of the reducing gas is 200 to 1000 h -1 ;

[0055] The total volume space velocity of the raw gas is 3000~15000h -1 .

[0056] Beneficial Effects

[0057] The catalyst provided by the present invention is based on a mixed oxide of iron and zirconium, and Cu, group VIIA elements and additives are added. When applied to the process of directly preparing light olefins from synthesis gas, high CO conversion rate and high light olefin selectivity can be achieved at a relatively low reaction pressure.

[0058] The method for preparing low-carbon olefins provided by the present invention comprises the following steps: 100 Zr a Cu b A c X d O e As a catalyst, in the process of direct preparation of light olefins from syngas, the reaction pressure is significantly lower than the general reaction pressure (general reaction pressure is 2.0Mpa), the CO conversion rate is as high as 98%, and the selectivity of light olefins reaches 43%. DETAILED DESCRIPTION

[0059] The present disclosure may be more easily understood by the following description with reference to examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or shown herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise indicated.

[0060] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.

[0061] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".

[0062] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.

[0063] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.

[0064] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.

[0065] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values ​​can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values ​​stated in the range includes each value within the range.

[0066] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.

[0067] The present invention is further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The essential characteristics and remarkable effects of the present invention can be reflected from the following examples, and the described embodiments are part of the embodiments of the present invention, rather than all the embodiments, and therefore, they do not limit the present invention in any way, and those skilled in the art make some non-essential improvements and adjustments based on the content of the present invention, which all belong to the protection scope of the present invention.

[0068] In the following specific embodiments:

[0069] Catalyst application evaluation: A fixed bed microreactor was used, 0.5 g of catalyst was loaded, 3.0 g of quartz sand was diluted and mixed evenly, and the catalyst reduction conditions were: V H2 :V N2 =1:4, reducing gas space velocity 500h -1 , the reduction pressure is 0.3MPa, the reduction temperature is 350℃, and the reduction time is 5 hours. After the catalyst reduction is completed, the temperature is lowered to below 100℃, and the raw gas is introduced, H2 / CO=2:1, the reaction temperature is 320℃, the reaction pressure is 1.0MPa, and the space velocity is 8000h -1 After the reaction was stable for 12 hours, the raw gas and the product were analyzed, and the results are listed in Appendix 1.

[0070] Example 1

[0071] The catalyst composition provided in this embodiment is Fe 100 Zr 16 Cu2Mg4K3Cl4O e .

[0072] A specific preparation process of the catalyst is as follows:

[0073] Weigh 20.4gFe(NO3)3·9H2O and 3.58gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 17.63g urea and dissolve it in 120ml deionized water, stir evenly, this is solution B. Mix solution A and solution B and put them into a polytetrafluoroethylene-lined autoclave for precipitation reaction. The reaction temperature is controlled at 140℃ and aged at this temperature for 3 hours. Wash the precipitate with deionized water until it is neutral, dry it at 60℃ for 12 hours, and roast it in air at 400℃ for 3 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0074] Weigh 0.078g Cu(CH3COO)2·H2O, 0.0681g CuCl2·2H2O, 0.096g KCl, and 0.308g Mg(NO3)2 respectively, dissolve in deionized water, and stir to obtain solution C. Grind Fe2O3 and ZrO2 mixed oxides uniformly, add solution C to achieve incipient wetness impregnation. After impregnation at room temperature for 24 hours, dry at 60°C for 12 hours, and calcine at 400°C for 3 hours to obtain the catalyst.

[0075] The prepared catalyst was pressed into tablets and crushed, and then passed through a 40-60 mesh sieve for evaluation.

[0076] Example 2

[0077] The catalyst composition provided in this embodiment is Fe 100 Zr 16 Cu2Cl4Mg4K 3e .

[0078] A specific preparation process of the catalyst is as follows:

[0079] Weigh 20.4gFe(NO3)3·9H2O and 3.58gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 11.82g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. The reaction temperature is controlled at 70℃ and aged at this temperature for 3 hours. Wash the precipitate with deionized water to neutralize it, dry it at 60℃ for 24 hours, and roast it in air at 500℃ for 3 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0080] Weigh 0.078g Cu(CH3COO)2·H2O, 0.0681g CuCl2·2H2O, 0.096g KCl, and 0.308g Mg(NO3)2, dissolve in deionized water, and stir to obtain solution C. Grind the Fe2O3 and ZrO2 mixed oxides uniformly, and add solution C to achieve initial wetness impregnation. After immersion at room temperature for 24 hours, dry at 60℃ for 12 hours, and calcine at 400℃ for 3 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Zr 16 Cu2Cl4Mg4K3O e .

[0081] Example 3

[0082] The catalyst composition provided in this embodiment is Fe 100 Zr 16 Cu2Cl3Na2Ca3O e .

[0083] A specific preparation process of the catalyst is as follows:

[0084] Weigh 20.4gFe(NO3)3·9H2O and 3.58gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 11.82g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with deionized water to neutralize it, dry it at 60℃ for 20 hours, and roast it in air at 450℃ for 3 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0085] Weigh 0.156g Cu(CH3COO)2·H2O, 0.113g NH4Cl, 0.063g NaCl, and 0.295g Ca(NO3)2 respectively, dissolve in deionized water, and stir to obtain solution C. Grind the uniform Fe2O3 and ZrO2 mixed oxides, add solution C to achieve initial wetness impregnation. After immersion at room temperature for 24 hours, dry at 60℃ for 12 hours, and calcine at 400℃ for 3 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Zr 16 Cu2Cl3Na2Ca3O e .

[0086] Example 4

[0087] The catalyst composition provided in this embodiment is Fe 100 Zr 16Cu2Cl4K3O e .

[0088] A specific preparation process of the catalyst is as follows:

[0089] Weigh 20.4gFe(NO3)3·9H2O and 3.58gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 11.82g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with deionized water to neutralize it, dry it at 60℃ for 20 hours, and roast it in air at 400℃ for 3 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0090] Weigh 0.156g Cu(CH3COO)2·H2O, 0.113g NH4Cl, and 0.1295g KNO3 respectively, dissolve in deionized water, and stir to obtain solution C. Grind the uniform Fe2O3 and ZrO2 mixed oxides, add solution C to achieve initial wetness impregnation. After impregnation at room temperature for 24 hours, dry at 60℃ for 18 hours, and calcine at 400℃ for 8 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Zr 16 Cu2Cl4K3O e .

[0091] Example 5

[0092] The catalyst composition provided in this embodiment is Fe 100 Zr 40 Cu 10 Cl7Ba1O e .

[0093] A specific preparation process of the catalyst is as follows:

[0094] Weigh 15.7gFe(NO3)3·9H2O and 6.94gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 10.57g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with an equal amount of deionized water to neutralize it, dry it at 60℃ for 20 hours, and roast it in air at 400℃ for 3 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0095] Weigh 0.7812g Cu(CH3COO)2·H2O, 0.1507g NH4Cl, and 0.095g Ba(NO3)2 respectively, dissolve in deionized water, and stir to obtain solution C. Grind the uniform Fe2O3 and ZrO2 mixed oxides, add solution C to achieve initial wetness impregnation. After impregnation at room temperature for 24 hours, dry at 60℃ for 18 hours, and calcine at 400℃ for 8 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Zr 40 Cu 10 Cl7Ba1O e .

[0096] Example 6

[0097] The catalyst composition provided in this embodiment is Fe 100 Zr 100 Cu3F 10 K5O e .

[0098] A specific preparation process of the catalyst is as follows:

[0099] Weigh 10.2gFe(NO3)3·9H2O and 10.83gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 9.7g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with an equal amount of deionized water to neutralize it, dry it at 60℃ for 20 hours, and roast it in air at 400℃ for 3 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0100] Weigh 0.1562g Cu(CH3COO)2·H2O, 0.097g NH4F, and 0.1295g KNO3 respectively, dissolve in deionized water, and stir to obtain solution C. Grind the Fe2O3 and ZrO2 mixed oxides uniformly, and add solution C to achieve initial wetness impregnation. After impregnation at room temperature for 20 hours, dry at 60℃ for 10 hours, and calcine at 450℃ for 8 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Zr 100 Cu2F5K3O e .

[0101] Example 7

[0102] The catalyst composition provided in this embodiment is Fe 100 Zr 50 Cu2Br2K5Oe .

[0103] A specific preparation process of the catalyst is as follows:

[0104] Weigh 14.4gFe(NO3)3·9H2O and 7.65gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 10.27g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with an equal amount of deionized water to neutralize it, dry it at 60℃ for 20 hours, and roast it in air at 450℃ for 3 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0105] Weigh 0.1562g Cu(CH3COO)2·H2O, 0.061g NH4Br, and 0.194g KNO3 respectively, dissolve in deionized water, and stir to obtain solution C. Grind the Fe2O3 and ZrO2 mixed oxides uniformly, and add solution C to achieve initial wetness impregnation. After impregnation at room temperature for 10 hours, dry at 60℃ for 10 hours, and calcine at 450℃ for 8 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Zr 60 Cu2Br1K3O e .

[0106] Comparative Example 1

[0107] The catalyst composition provided in this comparative example is Fe 100 Zr 16 .

[0108] A specific preparation process of the catalyst is as follows:

[0109] Weigh 20.4gFe(NO3)3·9H2O and 3.61gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 22.63g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with an equal amount of deionized water to neutralize it, dry it at 60℃ for 20 hours, and calcine it in air at 400℃ for 3 hours. The catalyst consists of Fe 100 Zr 16 .

[0110] Comparative Example 2

[0111] The catalyst composition provided in this comparative example is Fe 100 Al16 Cu2Cl4K3O e .

[0112] A specific preparation process of the catalyst is as follows:

[0113] Weigh 30.6gFe(NO3)3·9H2O and 1.01gα-Al2O3 respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 29.09g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with an equal amount of deionized water to neutralize it, dry it at 60℃ for 20 hours, and roast it in air at 400℃ for 3 hours to obtain a mixed oxide of Fe2O3 and α-Al2O3.

[0114] Weigh 0.1562g Cu(CH3COO)2·H2O, 0.113g NH4Cl, and 0.1295g KNO3 respectively, dissolve in deionized water, and stir to obtain solution C. Grind the Fe2O3 and α-Al2O3 mixed oxides uniformly, add solution C to achieve initial wetness impregnation. After impregnation at room temperature for 24 hours, dry at 60℃ for 18 hours, and calcine at 400℃ for 8 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Al 16 Cu2Cl4K3O e .

[0115] Comparative Example 3

[0116] The catalyst composition provided in this comparative example is Fe 100 Zr 16 Cu2Cl 35 K3O e .

[0117] A specific preparation process of the catalyst is as follows:

[0118] Weigh 20.4gFe(NO3)3·9H2O and 3.58gZr(NO3)4·5H2O respectively and dissolve them in 120ml deionized water, stir evenly, this is solution A. Weigh 11.82g ammonium carbonate and dissolve it in 120ml deionized water, stir evenly, this is solution B. Add solution A and solution B to a four-necked flask in parallel. Control the reaction temperature at 70℃ and age for 3 hours. Wash the precipitate with an equal amount of deionized water to neutralize it, dry it at 60℃ for 22 hours, and roast it in air at 400℃ for 4 hours to obtain a mixed oxide of Fe2O3 and ZrO2.

[0119] Weigh 0.1563g Cu(CH3COO)2·H2O, 0.9419g NH4Cl, and 0.1295g KNO3 respectively, dissolve in deionized water, and stir to obtain solution C. Grind the uniform Fe2O3 and ZrO2 mixed oxides, add solution C to achieve initial wetness impregnation. After impregnation at room temperature for 24 hours, dry at 60℃ for 20 hours, and calcine at 400℃ for 4 hours. The obtained catalyst is pressed into tablets and crushed through a 40-60 mesh sieve for evaluation. The composition of Fe in the catalyst is 100 Zr 16 Cu2Cl 22 K3O e .

[0120] Comparative Example 4

[0121] The catalyst composition provided in this comparative example is Fe 100 Zr 16 Cu2K3O e .

[0122] A specific preparation process of the catalyst is basically the same as that of Example 4, except that no NH4Cl is added.

[0123] Application Experiment

[0124] Table 1 Catalyst application evaluation

[0125]

[0126]

[0127] By comparing Examples 1 to 7 with Comparative Example 1, the simple mixed oxide of Fe2O3 and ZrO2 in Comparative Example 1 already has high activity and a high CO conversion rate. After adding Cu, halogens and additives to Examples 1 to 7, the CO conversion rates still remain at a high level, all above 95%. At the same time, the selectivity of low-carbon olefins is significantly improved, proving the advanced nature of this patent.

[0128] It can be seen from Example 4 and Comparative Example 2 that a mixed oxide of Fe2O3 and ZrO2 is also necessary. ZrO2 not only acts as a carrier to better disperse iron oxide, but also synergizes with other components to improve the selectivity of light olefins without reducing the activity of the catalyst.

[0129] In addition, it can be seen from Example 4 and Comparative Example 3 that after adding too much Cl additive, the activity decreases significantly. And it can be seen from Example 4 and Comparative Example 4 that the selectivity of light olefins for the catalyst without Cl additive decreases significantly. Therefore, the amount of Group VIIA elements should be controlled.

[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A catalyst for preparing light olefins from synthesis gas, characterized in that: Calculated by atomic ratio, the catalyst includes substances shown in the following formula: Fe 100 Zr a The b A c X d O e ; in, The value range of a is 10 to 150; The value range of b is 1.0~15; The value range of c is 2 to 10; The value range of d is 1.0~30; e is the total number of oxygen atoms required to satisfy the valence of each element in the substance shown; A is an element selected from Group VIIA, wherein the elements in Group VIIA include any one or more of F, Cl, Br, and I; X is any one or more alkali metal elements and / or any one or more alkaline earth metal elements.

2. The catalyst for preparing light olefins from synthesis gas according to claim 1, characterized in that: The X includes any one or more of Be, Ca, Mg, Se, Ba, K, Na, Li, and Cs.

3. The method for preparing a catalyst for preparing light olefins from synthesis gas according to any one of claims 1 to 2, characterized in that: 1) preparing a mixed solution containing Fe and Zr, wherein the total metal ion concentration of Fe and Zr in the mixed solution is 0.1 mol / L to 3.0 mol / L; Prepare a solution containing a precipitant, wherein the concentration of the precipitant in the solution is 0.1 mol / L to 3 mol / L, and the amount of the precipitant is to ensure complete precipitation of Fe and Zr ions; 2) contacting and mixing the mixed solution in step 1) with a solution containing a precipitant to form a precipitate; 3) aging and calcining the precipitate obtained in step 2) to obtain a mixed oxide of iron and zirconium; 4) preparing a solution containing Cu, a Group VIIA element and an alkali metal and / or an alkaline earth metal element as an impregnation solution; 5) impregnating the mixed oxides of step 3) with the impregnation solution of step 4), and then drying and calcining to obtain a catalyst; The precipitating agent used includes one or more of ammonium carbonate, ammonium bicarbonate, ammonia water, sodium carbonate, urea, potassium carbonate, sodium hydroxide and potassium hydroxide.

4. The method for preparing a catalyst for preparing light olefins from synthesis gas according to claim 3, characterized in that: In the step 2), a precipitate is obtained at a temperature of 40° C. to 180° C. and a pH value of 5 to 10.

5. The method for preparing a catalyst for preparing light olefins from synthesis gas according to claim 3, characterized in that: In the step 3), the aging time is 1h to 20h, and the temperature is 40°C to 180°C; The calcination temperature is 350°C to 800°C, and the calcination time is 2h to 20h.

6. The method for preparing a catalyst for preparing light olefins from synthesis gas according to claim 5, characterized in that: In the step 3), after the precipitate is aged, it needs to be washed, dried, and then roasted; The washing is washing until neutral or until no potassium or sodium is detected; The drying temperature is 40° C. to 150° C., and the drying time is 6 h to 24 h.

7. The method for preparing a catalyst for preparing light olefins from synthesis gas according to claim 3, characterized in that: In the step 5), the calcination temperature is 350°C to 800°C, and the calcination time is 2h to 20h; The drying temperature is 40℃~150℃, and the drying time is 6h~24h.

8. The catalyst for preparing light olefins from synthesis gas according to any one of claims 1 to 2, or the use of the catalyst for preparing light olefins from synthesis gas obtained by the method according to any one of claims 3 to 7, characterized in that: Used for catalytic synthesis of light olefins from synthesis gas; The steps include: Prepare reducing gas, the reducing gas includes H2 and N2, and the volume content of H2 is not less than 20%; The catalyst is reduced; the reduction temperature is 300-550° C., the reduction pressure is 0.01-2.0 MPa, and the reduction time is 3-12 h; preparing a raw gas, wherein the raw gas comprises CO and H2; After the reduction treatment, the raw gas is introduced to carry out the reaction of preparing light olefins from synthesis gas; the reaction temperature is 250-380° C., and the reaction pressure is 0.5-5.0 MPa; Wherein, the molar ratio of H2 / CO is 0.5-3.

9. The use of the catalyst for preparing light olefins from synthesis gas according to claim 8, characterized in that: Using fixed bed reactor to catalyze synthesis gas to produce light olefins; The gas space velocity of the reducing gas is 200 to 1000 h -1 ; The total volume space velocity of the raw gas is 3000~15000 h -1 .