A method for preparing low-cobalt and cobalt-free positive electrode materials by pre-burning lithium-poor process and its application
By pre-burning the lithium-poor process, the problems of lithium source loss and high cobalt content in traditional lithium-ion battery synthesis are solved, the full utilization of lithium and material cost reduction are achieved, and excellent electrochemical performance and stability are obtained.
Patent Information
- Application Number
- CN202211204549.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-29
AI Technical Summary
In the traditional lithium-ion battery synthesis process, high-temperature roasting leads to the loss of lithium sources and increases material costs, and the scarcity of cobalt and lithium limits the development of batteries.
The pre-fired lithium-depleted process is used to pre-fire and re-fire by mixing the precursor with the lithium source and controlling the heating rate and time to reduce the loss of lithium source and cobalt content and improve material utilization.
It achieves full utilization of lithium in lithium-ion batteries, reduces material costs, and obtains low-cobalt-free cathode materials with excellent electrochemical properties. The morphology and particle size are consistent, which improves the stability and performance of the battery.
Smart Images

Figure HDA0003873123790000011 
Figure HDA0003873123790000012 
Figure HDA0003873123790000021
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ternary cathode material synthesis, and in particular to a method and application thereof for preparing a low-cobalt or cobalt-free cathode material by a pre-burning lithium-poor process. Background Art
[0002] The conversion of common energy such as solar energy and wind energy requires core storage devices, and lithium-ion batteries are indispensable as storage devices for new energy sources. Positive electrode materials are the most critical raw materials for lithium-ion batteries, accounting for more than 30% of the cost of lithium-ion batteries. However, with the rapid development of lithium-ion batteries, the high prices of scarce resources such as cobalt and lithium have limited the rapid development of lithium-ion batteries to a certain extent.
[0003] However, the conventional preparation process uses a single-baking lithiation process during the synthesis process, which not only has a low degree of lithiation, but also has a severe reaction temperature that will cause a significant loss of lithium source, resulting in excessive lithium source being added during the ternary material calcination process and not being fully utilized, thereby increasing the material cost. For example, a nickel-cobalt-aluminum ternary positive electrode material, a preparation method, and a lithium-ion battery disclosed in a Chinese patent application (grant number CN109616663B) specifically prepare a ternary positive electrode material precursor, grind the precursor, mix it with a lithium salt, and calcine it to prepare a ternary positive electrode material, but the defects of the single-baking lithiation process cannot be ignored. Summary of the invention
[0004] In order to further effectively improve the cost-effectiveness of ternary positive electrode materials, we provide a method for preparing low-cobalt and cobalt-free positive electrode materials by pre-burning lithium-poor process. On the one hand, it reduces the proportion of cobalt content in ternary materials, and on the other hand, it makes full use of limited lithium in the synthesis of ternary positive electrode materials. Through the synergistic effect of the two, the positive result of reducing costs and increasing efficiency is achieved.
[0005] The present invention provides a method for preparing a low-cobalt and cobalt-free positive electrode material by pre-burning a lithium-poor process, which at least comprises the following steps:
[0006] (1) mixing the precursor and the lithium source at a high speed according to a metal ratio to obtain a mixture;
[0007] (2) After all the mixed materials are put into a pot, they are pre-burned in an air atmosphere, and after the materials are naturally cooled, they are mechanically crushed to obtain the pre-burned materials;
[0008] (3) Place the pre-fired material in a pot and re-fire it in an air atmosphere, and then allow it to cool naturally before it is ready.
[0009] As a preferred technical solution, the precursor in step (1) contains metal elements nickel, cobalt, and manganese; the source of the nickel, cobalt, and manganese is one of metal hydroxides, metal carbonates, metal oxides, and metal sulfates; preferably, the precursor in step (1) is Nix Co y Mn z (OH) 2 、Ni x Co y Mn z CO 3 、 x Co y Mn z O、Ni x Co y Mn z SO 4 One of the above, wherein x, y, and z are respectively the molar ratios of nickel, cobalt, and manganese elements in the nickel-cobalt-manganese precursor to the total molar amount of nickel, cobalt, and manganese, and 0≤y≤0.1, 0≤x≤1, and 0≤z≤1.
[0010] As a preferred technical solution, the lithium source in step (1) is one of organic acid lithium, alkyl alcohol lithium, and inorganic acid lithium;
[0011] Preferably, the alkyl alcohol lithium is selected from lithium ethoxide, lithium methanol, lithium isopropoxide, lithium butoxide; the organic acid lithium is selected from lithium acetate, lithium formate; the inorganic acid lithium is selected from LiNO 3 、LiNO 2 , Li 2 CO 3 , Li 2 SO 4 , Li 2 SO 3 、LiClO 4 、LiMnO 4 Preferably, the lithium source in step (1) is an inorganic acid lithium, and the inorganic acid lithium is Li 2 CO 3 .
[0012] As a preferred technical solution, the metal ratio (molar ratio) in step (1) is Li:Me (nickel + cobalt + manganese) = (0.8-1.5):1;
[0013] As a preferred technical solution, the conditions of the pre-sintering process in step (2) are: heating to 300°C-750°C at a heating rate of 4-6°C / min, and the pre-sintering time is 3h-24h. Preferably, the conditions of the pre-sintering process in step (2) are: heating to 400°C-700°C at a heating rate of 4-6°C / min, and the pre-sintering time is 4h-10h.
[0014] As a preferred technical solution, the conditions for re-calcination in step (3) are: heating to 750°C-1000°C at a heating rate of 4-6°C / min, and the re-calcination time is 6h-12h.
[0015] Based on the method provided by the present invention, by designing a pre-firing process, especially controlling the conditions of the pre-firing process: heating the temperature to 300°C-750°C at a heating rate of 4-6°C / min, and the pre-firing time is 3h-24h; the precursor has enough time to absorb oxygen and react more easily with the lithium source, the ternary positive electrode material is easier to achieve lithiation, and the problem of lithium source loss caused by the severe reaction temperature is effectively avoided, so that less lithium source is used to obtain the same level of electrochemical performance.
[0016] Based on the method for preparing low-cobalt and cobalt-free positive electrode materials by the pre-firing lithium-poor process provided by the present invention, after the pre-firing process, the heating rate is further controlled to 750°C-1000°C, and the re-firing time is 6h-12h, so that the prepared positive electrode material has consistent morphology, high consistency in particle size, and has excellent electrochemical properties.
[0017] On the other hand, the present invention provides an application of a method for preparing a low-cobalt or cobalt-free positive electrode material by a pre-burning lithium-deficient process, which is applied to the preparation of a low-cobalt or cobalt-free positive electrode material.
[0018] Beneficial effects:
[0019] 1. In order to further effectively improve the cost-effectiveness of ternary positive electrode materials, we provide a method for preparing low-cobalt and cobalt-free positive electrode materials by pre-burning lithium-poor process. On the one hand, it reduces the proportion of cobalt content in ternary materials, and on the other hand, it makes full use of limited lithium in the synthesis of ternary positive electrode materials. Through the synergistic effect of the two, the positive result of reducing costs and increasing efficiency is achieved.
[0020] 2. Based on the method provided by the present invention, by designing a pre-burning process, especially controlling the conditions of the pre-burning process: heating the temperature to 300°C-750°C at a heating rate of 4-6°C / min, and the pre-burning time is 3h-24h; the precursor has enough time to absorb oxygen and react more easily with the lithium source, the ternary positive electrode material is easier to achieve lithiation, and the problem of lithium source loss caused by the drastic reaction temperature is effectively avoided, so that less lithium source is used to obtain the same level of electrochemical performance.
[0021] 3. Based on the method for preparing low-cobalt and cobalt-free positive electrode materials by the pre-burning lithium-poor process provided by the present invention, after the pre-burning process, the heating rate is further controlled to 750℃-1000℃, and the roasting time is again 6h-12h, so that the prepared positive electrode material has consistent morphology, high consistency in particle size, and has excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The following are scanning electron microscope photos of low-cobalt positive electrode materials prepared in Example 1(a) and Comparative Example 1(b) of the present invention. Figure 1 It shows that the morphology of the low-cobalt positive electrode materials prepared in Example 1 (a) and Comparative Example 1 (b) is basically the same, and the primary particle sizes are comparable.
[0023] Figure 2 This is a comparison chart of the first charge and discharge curves of the low-cobalt positive electrode materials prepared in Example 1 and Comparative Example 1.
[0024] Figure 3 This is a comparison chart of the cycle performance (normal temperature 25° C.) of the low-cobalt positive electrode materials prepared in Example 1 and Comparative Example 1.
[0025] Figure 4 The scanning electron microscope photos of the cobalt-free positive electrode materials prepared in Example 2(a) and Comparative Example 2(b) of the present invention are shown in FIG. Figure 4 It shows that the morphology of the cobalt-free positive electrode materials prepared in Example 2 (a) and Comparative Example 2 (b) is basically the same, and the primary particle sizes are comparable.
[0026] Figure 5 This is a comparison chart of the first charge and discharge curves of the cobalt-free positive electrode materials prepared in Example 2 and Comparative Example 2.
[0027] Figure 6 This is a comparison chart of the cycle performance (normal temperature 25° C.) of the cobalt-free positive electrode materials prepared in Example 2 and Comparative Example 2. DETAILED DESCRIPTION
[0028] Example 1
[0029] Embodiment 1 of the present invention provides a method for preparing a low-cobalt and cobalt-free positive electrode material by pre-burning a lithium-poor process, comprising the following steps:
[0030] (1) mixing the precursor and the lithium source at a high speed according to a metal ratio to obtain a mixture;
[0031] (2) After all the mixed materials are put into a pot, they are pre-burned in an air atmosphere, and after the materials are naturally cooled, they are mechanically crushed to obtain the pre-burned materials;
[0032] (3) The pre-burned material is placed in a pot and sintered again in an air atmosphere, and after natural cooling, a low-cobalt ternary positive electrode material is obtained.
[0033] The precursor in step (1) contains the metal elements nickel, cobalt and manganese, specifically Ni 0.55 Co 0.05 Mn 0.4 (OH) 2 , model number is NCM550540.
[0034] In the step (1), the lithium source is an inorganic acid lithium, and the inorganic acid lithium is Li 2 CO 3 .
[0035] In the step (1), the metal ratio is Li:Me (nickel + cobalt + manganese) = 0.93:1;
[0036] The conditions of the pre-sintering process in step (2) are: heating to 620° C. at a heating rate of 5° C. / min, and the pre-sintering time is 6 hours.
[0037] The conditions for the re-roasting in step (3) are: heating to 930° C. at a heating rate of 5° C. / min, and the re-roasting time is 8 h.
[0038] Example 2
[0039] Embodiment 2 of the present invention provides a method for preparing a low-cobalt and cobalt-free positive electrode material by pre-burning a lithium-poor process, comprising the following steps:
[0040] (1) mixing the precursor and the lithium source at a high speed according to a metal ratio to obtain a mixture;
[0041] (2) After all the mixed materials are put into a pot, they are pre-burned in an air atmosphere, and after the materials are naturally cooled, they are mechanically crushed to obtain the pre-burned materials;
[0042] (3) The pre-burned material is placed in a pot and fired again in an air atmosphere, and after natural cooling, a cobalt-free ternary positive electrode material is obtained.
[0043] The precursor in step (1) contains metal elements nickel and manganese, specifically Ni 0.6 Mn 0.4 (OH) 2 , model number is NM6040.
[0044] In the step (1), the lithium source is an inorganic acid lithium, and the inorganic acid lithium is Li 2 CO 3 .
[0045] In the step (1), the metal ratio is Li:Me (nickel + manganese) = 0.96:1;
[0046] The conditions of the pre-sintering process in step (2) are: heating to 430° C. at a heating rate of 5° C. / min, and the pre-sintering time is 6 hours.
[0047] The conditions for the re-roasting in the step (3) are: heating to 900° C. at a heating rate of 5° C. / min, and the re-roasting time is 8 hours.
[0048] Comparative Example 1
[0049] Comparative Example 1 of the present invention adopts a traditional process to prepare a low-cobalt positive electrode material, which specifically includes the following steps:
[0050] The low-cobalt precursor NCM550540 and lithium carbonate are mixed at a high speed according to the metal ratio of Li / Me: 1.035. After all are put into a pot, the temperature is increased to 930°C at a heating rate of 5°C / min in an air atmosphere and then maintained at a constant temperature for 8 hours. After natural cooling, a low-cobalt ternary positive electrode material is obtained.
[0051] Comparative Example 2
[0052] Comparative Example 2 of the present invention adopts a traditional process to prepare a cobalt-free positive electrode material, which specifically includes the following steps:
[0053] The cobalt-free precursor NM6040 and lithium carbonate are mixed at a high speed according to the metal ratio of Li / Me: 1.065. After all are put into a pot, the temperature is increased to 900°C at a heating rate of 5°C / min in an air atmosphere, and then kept at a constant temperature for 10 hours. After natural cooling, a cobalt-free ternary positive electrode material is obtained.
[0054] Performance Testing Methods
[0055] 1. The low-cobalt ternary positive electrode material and the cobalt-free ternary positive electrode material prepared in the examples and comparative examples were characterized by scanning electron microscopy. Figure 1 , Figure 4 .
[0056] 2. The low-cobalt ternary positive electrode materials prepared in Example 1 and Comparative Example 1 were assembled into button-type CR2032 half-cells and tested at a current density of 0.2C under a voltage of 4.3V-3.0V. The test results are shown in Figure 2. It can be seen that the capacity of Comparative Example 1 is 167.2mAh / g, and that of Implementation Example 1 is 167.6mAh / g, and the gram capacity is basically the same.
[0057] 3. The low-cobalt ternary cathode materials prepared in Example 1 and Comparative Example 1 were assembled into button-type CR2032 half-cells, and the cycle performance test was carried out at room temperature and 25°C at a current density of 1.0C and a voltage of 4.30V. The results are shown in Figure 3 It can be seen that after 50 cycles, the gram capacity of comparative example 1 reaches 138.8 mAh / g, and the capacity retention rate is 90.3%; after 50 cycles, the gram capacity of embodiment 1 reaches 143.8 mAh / g, and the capacity retention rate is 93.9%; the cycle stability of embodiment 1 is improved compared with comparative example 1.
[0058] 4. The low-cobalt ternary positive electrode materials prepared in Example 2 and Comparative Example 2 were assembled into button-type CR2032 half-cells and tested at a current density of 0.2C under a voltage of 4.3V-3.0V. The test results are shown in Figure 5. It can be seen that the capacity of Comparative Example 2 is 163.6mAh / g, and that of Implementation Example 2 is 163.1mAh / g, and the gram capacity is basically the same.
[0059] 5. The low-cobalt ternary cathode materials prepared in Example 2 and Comparative Example 2 were assembled into button-type CR2032 half-cells, and the cycle performance test was carried out at room temperature and 25°C at a current density of 1.0C and a voltage of 4.30V. The results are shown in Figure 6 It can be seen that after 50 cycles, the gram capacity of Comparative Example 2 reaches 140.8 mAh / g, and the capacity retention rate is 98.1%; after 50 cycles, the gram capacity of Example 2 reaches 140.4 mAh / g, and the capacity retention rate is 98.1%; the cycle stability of Example 2 is basically equivalent to that of Comparative Example 2.
Claims
1. A method for preparing a low-cobalt positive electrode material by pre-burning a lithium-poor process, characterized in that: The following steps are involved: (1) Mixing the precursor and the lithium source at a high speed according to the metal ratio to obtain a mixture; (2) After all the mixed materials are put into a pot, they are pre-burned in an air atmosphere, and after the materials are naturally cooled, they are mechanically crushed to obtain the pre-burned materials; (3) After the pre-burned material is placed in a pot, it is roasted again in an air atmosphere, and after natural cooling, a low-cobalt ternary positive electrode material is obtained; The precursor in step (1) contains metal elements nickel, cobalt and manganese, specifically Ni 0.55 Co 0.05 Mn 0.4 (OH)2, model number is NCM550540; In the step (1), the lithium source is an inorganic acid lithium, and the inorganic acid lithium is Li2CO3; The metal ratio in step (1) is Li: (nickel + cobalt + manganese) = 0.93:1; The conditions of the pre-sintering process in step (2) are: heating to 620°C at a heating rate of 5°C / min, and the pre-sintering time is 6 hours; The conditions for the re-roasting in step (3) are: heating to 930° C. at a heating rate of 5° C. / min, and the re-roasting time is 8 h.
2. A method for preparing a cobalt-free positive electrode material by pre-burning a lithium-deficient process, characterized in that: The following steps are involved: (1) Mixing the precursor and the lithium source at a high speed according to the metal ratio to obtain a mixture; (2) After all the mixed materials are put into a pot, they are pre-burned in an air atmosphere, and after the materials are naturally cooled, they are mechanically crushed to obtain the pre-burned materials; (3) After the pre-burned material is placed in a pot, it is roasted again in an air atmosphere, and after natural cooling, a low-cobalt ternary positive electrode material is obtained; The precursor in step (1) contains metal elements nickel and manganese, specifically Ni 0.6 Mn 0.4 (OH)2, model number is NM6040; In the step (1), the lithium source is an inorganic acid lithium, and the inorganic acid lithium is Li2CO3; The metal ratio in step (1) is Li: (nickel + manganese) = 0.96:1; The conditions of the pre-sintering process in step (2) are: heating to 430°C at a heating rate of 5°C / min, and the pre-sintering time is 6 hours; The conditions for the re-roasting in step (3) are: heating to 900° C. at a heating rate of 5° C. / min, and the re-roasting time is 8 h.
Citation Information
Patent Citations
Nickel-cobalt-aluminum ternary cathode materials, preparation methods and lithium-ion batteries
CN109616663B