A solid waste-based low calcium-silicon ratio functional aggregate and its preparation method and application
Through the preparation of solid waste-based low-calcium-silicon functional aggregates, cement, granite sawing mud and other materials, combined with disk granulator and autoclave maintenance technology, the contradiction between traditional aggregate water absorption rate and cylinder pressure strength is solved, and the impact of the traditional aggregate water absorption rate and cylinder pressure strength is improved. The durability and structural stability of concrete.
Patent Information
- Application Number
- CN202211540785.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-12-02
AI Technical Summary
There is a contradiction between improving water absorption and cylinder pressure strength in traditional artificial aggregates, and the low apparent density causes aggregate to float, affecting the concrete strength and structural appearance.
Use solid waste-based low-calcium silicon-based functional aggregate, made of cement, granite sawing mud, copper tailing sand, lithium slag, calcined bentonite or calcined zeolite and other materials. Calcium is controlled through a disc granulator and autoclaved maintenance process. The silicon ratio is between 0.1 and 0.3, forming spherical particles with high water absorption and high cylinder pressure strength.
The cylinder pressure strength is achieved above 10MPa, the water absorption rate is above 8%, and the apparent density is 1800-2100kg/m3, which solves the contradiction between the water absorption rate and the cylinder pressure strength of traditional aggregates, and reduces the water-adhesive ratio and cement consumption of concrete. , improves the durability and structural stability of concrete.
Smart Images

Figure GDA0005027668930000041 
Figure GDA0005027668930000061 
Figure GDA0005027668930000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to a solid waste-based low calcium-silicon ratio functional aggregate for concrete and a preparation method thereof. Technical Background
[0002] As the most widely used raw material in the construction field, concrete's performance has a decisive impact on the safety of building structures. In actual projects, the largest amount of concrete used is strength grade C30-C50. To ensure adequate construction performance, this strength grade of concrete usually has a higher water-cement ratio. To ensure adequate strength, a larger excess of cement is usually required, which to a certain extent reduces the crack resistance of concrete and increases energy consumption during concrete production and application.
[0003] The advantages of artificial aggregates over natural aggregates are mainly reflected in two aspects: first, good sphericity can significantly improve the fluidity of concrete, reduce the water-cement ratio and cement dosage, increase the dosage of mineral admixtures, reduce shrinkage and hydration heat, and achieve energy conservation and emission reduction; second, artificial aggregates are usually composed of silicate minerals as the main component, which are similar to cement hydration products, and can effectively improve the interface transition zone and improve the durability of concrete such as impermeability and frost resistance.
[0004] CN 110078395 A provides an artificial silicate fine aggregate with cement and quicklime as calcium materials and quartz tailings and lead-zinc tailings as silicon materials, with a water absorption rate of more than 15% and an apparent density of 1600-1800kg / m 3 There are three main problems with this artificial fine aggregate: first, the raw material cost is relatively high, among which the calcium-silicon ratio is 0.3-0.7, and the total amount of calcium materials (quicklime and cement) is more than 20%, and the calcium materials directly determine the material cost; second, although organic binders such as cellulose ether can improve the ball-forming performance, increase the porosity and increase the water absorption rate of artificial aggregates, they will have a significant negative effect on the strength of steam-cured artificial aggregates, resulting in low cylinder pressure strength; third, the apparent density of the aggregate is lower than 1800kg / m 3 , and the density of the paste in concrete is usually 1900kg / m 3 The apparent density of crushed stone is about 2600-2800kg / m 3The apparent density is too low, which may cause obvious aggregate floating during concrete application, affecting the appearance of the structure and the strength of concrete. These are not conducive to the application of artificial aggregate in structural concrete. CN 111087213 A discloses a method for preparing high-strength slag silicate ceramsite by spraying and balling process of pre-hydrated cement slurry, which uses cement, slag and diatomaceous earth as the core structure and cement and fly ash as the shell. Although it has relatively good performance, the core-shell structure process is complicated, and the cement dosage is more than 15%, which is costly. Summary of the invention
[0005] The present invention mainly aims at the contradiction between increasing water absorption and improving cylinder pressure strength of traditional artificial aggregates, as well as a series of problems such as aggregate floating and low concrete strength caused by low apparent density in the application process of structural concrete, and provides a solid waste-based low calcium-silicon ratio functional aggregate for structural concrete and its preparation method. The cylinder pressure strength of the functional aggregate reaches more than 10MPa, the water absorption rate is more than 8%, and the apparent density is 1800-2100kg / m 3 , solving the conflicting problem between cylinder compressive strength and water absorption rate of traditional artificial aggregates.
[0006] The technical solution adopted by the present invention to solve the above-mentioned problems is:
[0007] A solid waste-based low calcium-silicon ratio functional aggregate is mainly made of the following raw materials in parts by weight: 10-20 parts of cement, 60-85 parts of siliceous material, 0-20 parts of steel slag and 5-10 parts of inorganic modifier; the siliceous material is one of granite saw mud, copper tailings and lithium slag, and the SiO2 content is ≥30wt.%; the inorganic modifier is one of calcined bentonite or calcined zeolite; the effective calcium content of the raw materials is tested according to GB / T 5762-2012 "Chemical Analysis Methods for Limestone, Quicklime and Hydrated Lime for Construction", and the calcium-silicon ratio (in molar ratio) of the functional aggregate is controlled to be 0.1-0.3 according to the effective calcium and SiO2 contents of the raw materials, that is, the molar ratio of the total amount of effective calcium oxide to the total amount of SiO2 in the raw materials is 0.1-0.3.
[0008] According to the above plan, the proportion of industrial solid waste in the raw materials reaches more than 70%, that is, the proportion of siliceous materials and steel slag in the total mass of raw materials reaches more than 70%.
[0009] According to the above scheme, the granite saw mud is the cutting tailings produced in the process of granite processing, wherein the SiO2 content is ≥65%; the copper tailings are powdery or gravel-like solid wastes produced after natural copper ore is crushed, sorted, and selected, wherein the Fe2O3 content is ≥10% and the SiO2 content is ≥30%; the lithium slag is the waste residue of lithium carbonate produced by lithium mica or spodumene through the sulfuric acid method, wherein the total content of Al2O3 and SiO2 is ≥60% and the SO3 content is ≤15%.
[0010] According to the above scheme, the steel slag is waste slag discharged from steelmaking, with Fe2O3 content ≤30wt.% (Fe2O3 is generally not less than 10wt.%), and MgO content ≤13wt.%. Specifically, the Fe2O3 content of the steel slag is ≤25wt.%, MgO content ≤13wt.%, and CaO content ≥30%.
[0011] According to the above scheme, the inorganic modifier is obtained by calcining bentonite or zeolite powder at 300° C. for 3 hours, and the total content of Al2O3 and SiO2 in the bentonite or zeolite powder is ≥70%.
[0012] According to the above scheme, the solid waste-based low calcium-silicon ratio functional aggregate is in good spherical shape, with a diameter of 3-10 mm, a cylinder pressure strength of ≥10 MPa, a 1h water absorption rate of ≥8%, and an apparent density of 1800-2100 kg / m 3 The present invention also provides a method for preparing the above-mentioned solid waste-based low calcium-silicon ratio functional aggregate, comprising the following steps:
[0013] S1. Weigh the following raw materials in parts by weight: 10-20 parts of cement, 60-85 parts of siliceous material, 0-20 parts of slag and 5-10 parts of inorganic modifier, and dry and grind the various raw materials to the required moisture content and specific surface area;
[0014] S2. The cement, siliceous material, slag and inorganic modifier are mixed to obtain a mixture; the mixture is uniformly fed into a disc granulator through a belt conveyor, and sprayed with atomized water, adjusting the angle and speed of the disc granulator, and the mixture and atomized water form a dense ball having a particle size of 3-10mm;
[0015] S3. Place the pellets in an autoclave after standing for 5-12 hours at room temperature, steam them at a pressure of 1.3-1.8 MPa for 3-5 hours, and then naturally cool them to room temperature and pressure to obtain the desired solid waste-based low calcium-silicon ratio functional aggregate.
[0016] According to the above scheme, in step S1, the water content is ≤3.0wt%, and the specific surface area is ≥380m 2 / kg.
[0017] According to the above scheme, in step S2, the amount of atomized water sprayed is 15-20% of the total mass of the raw materials.
[0018] In the above preparation method, various raw materials are mixed evenly, and then continuously rolled with 15-20% water in a disc granulator to form dense spherical particles. After a period of rest, the cement is hydrated to form a certain initial strength, and then put into an autoclave for autoclave curing. Under the pressure of 1.3-1.8MPa, the active calcium oxide in the cement and SiO2 in the siliceous material generate hydrated minerals such as CSH, C2SH(B), and tobermorite. These hydration products are mostly rod-shaped and flaky crystals. They overlap each other during the hydration growth process to form a stable and dense structure, thereby improving the strength of the artificial functional aggregate.
[0019] Among them, adding steel slag to the functional aggregate can, on the one hand, utilize the calcium oxide in the steel slag to react with the siliceous material to generate silicate hydration products; on the other hand, the Fe2O3 in the steel slag can improve the stability of tobermorite and avoid its transformation into other hydration products, thereby improving the strength of the functional aggregate.
[0020] Bentonite and zeolite are aluminosilicate minerals with stable skeleton structure, good ion exchange capacity and high adsorption performance. After low-temperature calcination at 300℃, the skeleton structure, ion exchange and adsorption performance of bentonite and zeolite powder are not significantly affected, but the activity of aluminosilicate minerals is significantly improved. Adding an appropriate amount of calcined bentonite or zeolite powder as an inorganic modifier to the raw materials can, on the one hand, utilize its good plasticity to improve the balling rate and shorten the balling time in the balling process. On the other hand, it can utilize its stable skeleton structure and high pore structure to improve the porosity of artificial aggregates during steam curing, which is beneficial to improve the water absorption rate of artificial functional aggregates. At the same time, the highly active Al2O3 and SiO2 participate in the hydration reaction to produce tobermorite, hydrated calcium aluminate and other hydration additions, improve the mechanical properties of artificial aggregates, thereby avoiding the contradiction between the water absorption rate and cylinder pressure strength brought by organic binders, and achieving high water absorption and high strength of artificial aggregates.
[0021] Industrial waste residues usually contain different types of harmful impurities, such as cutting aids in granite saw mud, heavy metal ions in copper tailings, soluble phosphorus, fluorine and heavy metal ions in lithium slag. If these harmful impurities enter concrete, they will affect the performance and structural safety of concrete and bring certain negative effects. Bentonite and zeolite can effectively eliminate the negative effects of organic matter, soluble phosphorus and fluorine and heavy metal ions on artificial aggregates and concrete due to their strong ion exchange and adsorption capacity.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] First, the cylinder compressive strength of the solid waste-based low calcium-silicon ratio functional aggregate of the present invention reaches more than 10MPa, and the water absorption rate is more than 8%, which solves the contradiction between the cylinder compressive strength and water absorption rate of traditional artificial aggregates; and the apparent density is 1800-2100kg / m 3 , which solves the problems of aggregate floating and low concrete strength caused by low apparent density during its application in structural concrete.
[0024] Second, the solid waste-based low calcium-silicon ratio functional aggregate of the present invention can be used in ordinary concrete to replace 15%-30% of coarse aggregate. Its good sphericity can be used to reduce the water-cement ratio of concrete, and the cement dosage can be reduced by 30-50kg. The shrinkage deformation of concrete can be reduced while reducing the hydration heat release, thereby effectively reducing the risk of concrete cracking; at the same time, the water absorption rate of the solid waste-based low calcium-silicon ratio functional aggregate is above 8%, and a large number of capillaries inside can absorb a large amount of free water. Through pre-absorption of water, the internal curing effect of concrete can be exerted, the degree of cement hydration can be increased, the internal structure of concrete can be improved, the shrinkage deformation of concrete can be reduced, the strength of concrete can be increased, and the long-term durability can be improved.
[0025] Third, the solid waste-based low calcium-silicon ratio functional aggregate of the present invention does not require the addition of auxiliary functional admixtures, has a simple structure, and a simple production process, thereby reducing production costs while increasing production capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 SEM image of solid waste-based low calcium-silicon ratio functional aggregate in Example 3;
[0027] Figure 2 Example 4 SEM image of solid waste-based low calcium-silicon ratio functional aggregate. DETAILED DESCRIPTION
[0028] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.
[0029] In the following examples, P·O 42.5 cement produced by Huaxin Cement Plant, steel slag produced by Wuhan Iron and Steel Co., Ltd., granite saw mud from Macheng, copper tailings from Daye Sanxin Mining, lepidolite slag produced by Jiangxi Ganfeng Lithium Industry and bentonite from Henan were selected. The chemical analysis of the raw materials is shown in Table 1:
[0030] Table 1 Chemical analysis of raw materials / wt.%
[0031]
[0032] Example 1
[0033] A solid waste-based low calcium-silicon ratio functional aggregate, the preparation method of which specifically comprises the following steps:
[0034] S1. Weigh 10 parts of cement, 85 parts of granite mud, and 5 parts of calcined bentonite by weight, with a calcium-silicon ratio of 0.10. Dry and grind the granite mud and calcined bentonite to a specific surface area of ≥380m 2 / kg, moisture content ≤3.0wt% (if the finished product meets this moisture content and specific surface area, drying and grinding treatment is not required);
[0035] S2. The cement, granite saw mud, bentonite are mixed evenly, and uniformly fed into the disc granulator through the feed port, and the atomized water is turned on, and 19% of the raw material mass of tap water is sprayed, and the angle and speed of the disc granulator are adjusted. The mixture and atomized water form a dense ball with a particle size of 3-10mm;
[0036] S3. Place the pellets in an autoclave after standing for 6 hours at room temperature, steam them at 1.8 MPa for 3 hours, and then naturally cool them to room temperature and pressure to obtain the desired solid waste-based low calcium-silicon ratio functional aggregate.
[0037] Example 2
[0038] A low calcium-silicon ratio solid waste-based functional aggregate with a low calcium-silicon ratio, the preparation method of which specifically comprises the following steps:
[0039] S1. Weigh 20 parts of cement, 60 parts of granite mud, 10 parts of steel slag, and 10 parts of calcined bentonite by weight, with a calcium-silicon ratio of 0.23. Dry and grind the granite mud and calcined bentonite to a specific surface area of ≥380m 2 / kg, moisture content ≤3.0wt%;
[0040] S2. The cement, granite saw mud, calcined bentonite are mixed evenly, and uniformly fed into the disc granulator through the feed port, and the atomized water is turned on, and 15% of the raw material mass of tap water is sprayed, and the angle and speed of the disc granulator are adjusted. The mixture and atomized water form a dense, particle size of 3-10mm ball;
[0041] S3. Place the pellets in an autoclave after standing for 6 hours at room temperature, steam them at 1.8 MPa for 3 hours, and then naturally cool them to room temperature and pressure to obtain the desired solid waste-based low calcium-silicon ratio functional aggregate.
[0042] Example 3
[0043] A low calcium-silicon ratio solid waste-based functional aggregate with a low calcium-silicon ratio, the preparation method of which specifically comprises the following steps:
[0044] S1. Weigh 10 parts of cement, 85 parts of copper tailings, and 5 parts of calcined zeolite powder by weight, with a calcium-silicon ratio of 0.20. Dry and grind the copper tailings and calcined zeolite powder to a specific surface area of ≥380m 2 / kg, moisture content ≤3.0wt%;
[0045] S2. The cement, copper tailings, calcined zeolite powder are mixed uniformly, and uniformly fed into the disc granulator through the feed port, and the atomized water is turned on, and 15% of the raw material mass of tap water is sprayed, and the angle and speed of the disc granulator are adjusted, and the mixture and atomized water form a dense, particle size of 3-10mm ball;
[0046] S3. Place the pellets in an autoclave after standing for 5 hours at room temperature, steam them at 1.3 MPa for 5 hours, and then naturally cool them to room temperature and pressure to obtain the desired solid waste-based low calcium-silicon ratio functional aggregate.
[0047] Example 4
[0048] A solid waste-based low calcium-silicon ratio functional aggregate, the preparation method of which specifically comprises the following steps:
[0049] S1. Weigh 10 parts of cement, 75 parts of copper tailings, 10 parts of steel slag, and 5 parts of calcined zeolite powder by weight, with a calcium-silicon ratio of 0.22. Dry and grind the copper tailings and calcined zeolite powder to a specific surface area of ≥380m 2 / kg, moisture content ≤3.0wt%;
[0050] S2. The cement, copper tailings, calcined zeolite powder are mixed uniformly, and uniformly fed into the disc granulator through the feed port, and the atomized water is turned on, and 15% of the raw material mass of tap water is sprayed, and the angle and speed of the disc granulator are adjusted, and the mixture and atomized water form a dense, particle size of 3-10mm ball;
[0051] S3. Place the pellets in an autoclave after standing for 5 hours at room temperature, steam them at 1.6 MPa for 5 hours, and then naturally cool them to room temperature and pressure to obtain the desired solid waste-based low calcium-silicon ratio functional aggregate.
[0052] Depend on Figure 1 and Figure 2 It can be seen that the main hydration products of functional aggregate during steam curing are needle-shaped tobermorite and lamellar calcium aluminosilicate hydrate crystals. These hydration products overlap with each other during the crystal growth process to form a dense structure, providing sufficient matrix strength for the functional aggregate.
[0053] Example 5
[0054] A low calcium-silicon ratio solid waste-based functional aggregate with a low calcium-silicon ratio, the preparation method of which specifically comprises the following steps:
[0055] S1. Weigh 15 parts of cement, 65 parts of lithium slag, 10 parts of steel slag, and 10 parts of calcined zeolite powder by weight, with a calcium-silicon ratio of 0.26, and dry and grind the lithium slag and calcined zeolite powder to a specific surface area of ≥380m 2 / kg, moisture content ≤3.0wt%;
[0056] S2. The cement, lithium slag, calcined zeolite powder are mixed uniformly, and uniformly fed into the disc granulator through the feed port, and the atomized water is turned on, and 17% of the raw material mass of tap water is sprayed, and the angle and speed of the disc granulator are adjusted. The mixture and the atomized water form a dense ball with a particle size of 3-10mm;
[0057] S3. Place the pellets in an autoclave after standing for 10 hours at room temperature, steam them at 1.3 MPa for 5 hours, and then naturally cool them to room temperature and pressure to obtain the desired solid waste-based low calcium-silicon ratio functional aggregate.
[0058] Table 2 shows the cylinder compressive strength, apparent density and 1h water absorption of the solid waste-based low calcium-silicon ratio functional aggregate prepared in Examples 1-5. The cylinder compressive strength is >10MPa, and the apparent density is between 1850-2100kg / m 3 Within the range, the 1h water absorption rate is greater than 12%. The determination standard is GB / T 17431.2-2010 Lightweight aggregate and its test method.
[0059] The comparative example is a 3-5 mm artificial aggregate produced by a Zhejiang enterprise with fly ash and cement as the main raw materials. The cylinder compressive strength is 16.3 MPa and the apparent density is less than 1800 kg / m 3 , water absorption rate in 1h is less than 8%.
[0060] Table 2 Basic properties of low calcium-silicon ratio functional aggregates based on solid waste with different proportions
[0061]
[0062] Table 3 shows the mix proportion of C35 concrete, which is divided into a benchmark group and an experimental group. The experimental group uses the functional aggregate of each embodiment or comparative example and calculates the dosage according to 20% of the stone volume, with a dosage of 134 kg / m 3 , replace the stone in the reference group with equal volume. Compared with the reference group, the water consumption of the experimental group is reduced by 10kg / m 3 , cement consumption is reduced by 30kg / m 3 , the amount of water reducing agent is 7.0kg / m 3 Increased to 8.0kg / m 3 .
[0063] Table 3 Mix ratio of concrete with functional aggregate (kg / m 3 )
[0064]
[0065] Table 4 Compressive strength of concrete with functional aggregate
[0066]
[0067] The application effects of the comparative example and Examples 1-5 in concrete are shown in Table 4. The collapse time of Examples 1-5 is less than that of the comparative example, the initial expansion is greater than that of the comparative example, the 28d compressive strength is higher than that of the benchmark group and the comparative example, and the 28d shrinkage value is significantly reduced relative to the benchmark group and the comparative example, indicating that the application effect of the solid waste-based low calcium-silicon ratio functional aggregate in the present invention in structural concrete is better than that of the comparative example, reducing the shrinkage deformation of concrete, effectively reducing the risk of cracking of concrete, increasing the strength of concrete and improving long-term durability.
[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A solid waste-based low calcium-silicon ratio functional aggregate, It is characterized in that The functional aggregate is made of the following raw materials in parts by weight: 10-20 parts of cement, 60-85 parts of siliceous material, 0-20 parts of steel slag and 5-10 parts of inorganic modifier; the calcium-silicon ratio of the functional aggregate is controlled at 0.1-0.3; the siliceous material is one of granite saw mud, copper tailings and lithium slag, SiO 2 Content ≥30wt.%; the inorganic modifier is obtained by calcining bentonite or zeolite powder at 250-350°C for 2.5-3.5h; The method for preparing the solid waste-based low calcium-silicon ratio functional aggregate comprises the following steps: S1. Weigh the following raw materials by weight: 10-20 parts of cement, 60-85 parts of siliceous materials, 0-20 parts of steel slag and 5-10 parts of inorganic modifiers, and dry and grind the raw materials to the required moisture content and specific surface area; the moisture content is required to be ≤3.0wt% and the specific surface area is ≥380m 2 / kg; S2. The cement, siliceous material, slag and inorganic modifier are mixed to obtain a mixture; the mixture is evenly fed into a granulator, and atomized water is sprayed into the granulator at the same time. The angle and speed of the granulator are adjusted, and the mixture and atomized water form a ball with a particle size of 3-10 mm; wherein the atomized water sprayed is 15-20% of the total mass of the raw materials; S3. The above-mentioned ball is placed in a pressure cooker at room temperature for 5-12 hours, and then steamed at a pressure of 1.3-1.8MPa for 3-5 hours and then naturally dropped to room temperature and pressure to obtain the solid waste-based low calcium-silicon ratio functional aggregate; The solid waste-based low calcium-silicon ratio functional aggregate is spherical in shape with a diameter of 3-10 mm; and has a cylinder pressure strength of ≥10 MPa, a 1h water absorption rate of ≥8%, and an apparent density of 1800-2100 kg / m 3 .
2. A solid waste-based low calcium-silicon ratio functional aggregate according to claim 1, It is characterized in that Siliceous materials and steel slag account for more than 70% of the total mass of raw materials.
3. The solid waste-based low calcium-silicon ratio functional aggregate according to claim 1, It is characterized in that The granite saw mud is the cutting tailings produced during the granite processing, in which SiO 2 Content ≥ 65%; copper tailings are powdery or gravel solid waste produced after natural copper ore processing operations, including Fe 2 O 3 Content ≥10%, SiO 2 Content ≥30%; lithium slag is the waste residue from lithium carbonate produced by lithium mica or spodumene through sulfuric acid process, in which Al 2 O 3 and SiO 2 Total content ≥ 60%, SiO 2 Content ≥30wt.%, SO 3 Content ≤15%.
4. The solid waste-based low calcium-silicon ratio functional aggregate according to claim 1, It is characterized in that The steel slag is waste slag discharged from steelmaking, Fe 2 O 3 Content ≤30wt.% and not less than 10 wt.%, MgO content ≤13wt.%, CaO content ≥30wt.%.
5. The solid waste-based low calcium-silicon ratio functional aggregate according to claim 1, It is characterized in that Al in bentonite or zeolite powder 2 O 3 and SiO 2 Total content ≥70 wt.%.
6. Application of the solid waste-based low calcium-silicon ratio functional aggregate according to claim 1 in concrete, Features The solid waste-based low calcium-silicon ratio functional aggregate is used to replace 15%-30% volume of coarse aggregate in concrete.