A tire disassembly and assembly lubricating paste

A lubricating paste for tire disassembly and assembly addresses issues of corrosion and environmental pollution by forming a dense film with suitable drying speed and lubricity, enhancing operational efficiency and reducing production costs.

CN115975714BActive Publication Date: 2024-12-06QINGDAO FIHONOR CHEM SCI & TECH +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211657082.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-12-06
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

Existing lubricating materials for tire disassembly and assembly, such as soapy water, detergent, butter, grease, and oil-based lubricants, cause corrosion, rubber aging, environmental pollution, and operational inefficiencies, and fail to provide suitable lubrication and drying properties.

Method used

A tire disassembly and assembly lubricating paste composed of sodium lactate, emulsifier, polyethylene glycol, polyethylene glycol stearate, defoamer, and preservative, formulated to form a dense film with suitable drying speed and lubricity, preventing rim deformation and tire displacement.

Benefits of technology

The lubricating paste forms a dense film, reducing damage to tires and rims, is environmentally friendly, and allows for efficient disassembly and assembly of over 100 tires per kilogram, lowering production costs while avoiding pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a tire disassembly lubricating paste and a preparation method, wherein the tire disassembly lubricating paste comprises, by mass, 7-11 parts of sodium lactate or sodium lauryl sulfate, 5-9 parts of emulsifier, 3-6 parts of polyethylene glycol, 2-4 parts of polyethylene glycol stearate, 0.1-2 parts of defoamer, 0.1-1 parts of preservative, and 65-80 parts of water. The tire disassembly lubricating paste of the present invention is an environmentally friendly water-based lubricating paste, does not contain petroleum and silicone oil, has a suitable drying speed, and compared with the prior art, reduces the damage to the tire during the disassembly process and prevents the rim from being deformed by excessive force; the tire disassembly lubricating paste forms a dense film after drying, which not only makes the tire disassembly more convenient but also can fill the small gap of the stopper, so that the tire is tightly combined with the rim, and prevents the tire and the rim from relative displacement during the vehicle driving process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lubricating materials, and more particularly to a tire disassembly and assembly lubricating paste. Background Art

[0002] During the process of disassembly and assembly, the car tire is very hard and tightly combined with the rim, so it is necessary to apply a layer of lubricating paste with good lubricity and easy to form a fine film on the surface to prevent damage to the tire during disassembly and assembly and deformation of the rim due to excessive force.

[0003] At present, there are four situations in domestic auto repair shops: First, soapy water or detergent is used instead of lubricating paste, which can easily cause rim corrosion and rust, and the tire toe will stick to the rim, and it is easy to pull the toe when disassembling again. In addition, soapy water or detergent can easily drip into the tire dismantling machine, causing the parts of the tire dismantling machine to rust, thereby causing equipment failure and shortening its service life. Second, industrial butter is used as tire disassembly and assembly lubricating paste. Since butter is a product of petroleum refining, it can accelerate rubber aging and make the tire rubber lose elasticity. In addition, butter products are not easy to dry, and it is easy to displace when the car brakes suddenly, and it may be seriously unhooked. Third, grease products are used, which have a good lubrication effect during disassembly and assembly, but the oiliness is too large, and it is not easy to dry after installation, and it is easy to separate the tire from the rim when braking. Fourth, oil-based lubricants are also used, but such products have the disadvantages of being flammable, corrosive and polluting the environment. In view of the problems and defects of the prior art, the research and development of tire disassembly and assembly lubricating paste is of great significance. Summary of the invention

[0004] The present invention provides a tire disassembly and assembly lubricating paste, and the specific technical scheme is as follows:

[0005] A tire disassembly lubricating paste, comprising, by weight: 7-11 parts of sodium lactate or sodium lauryl sulfate, 5-9 parts of emulsifier, 3-6 parts of polyethylene glycol, 2-4 parts of polyethylene glycol stearate, 0.1-2 parts of defoamer, 0.1-1 parts of preservative, and 65-80 parts of water;

[0006] Further, the ratio of polyethylene glycol to polyethylene glycol stearate is 1-2:1;

[0007] Further, the composition comprises, by mass: 7 parts of sodium lactate, 9 parts of emulsifier, 3 parts of polyethylene glycol, 3 parts of polyethylene glycol stearate, 1 part of defoamer, 1 part of preservative, and 76 parts of water;

[0008] Further, the emulsifier is a nonionic emulsifier;

[0009] Furthermore, the nonionic emulsifier is sorbitan fatty acid ester or alkylphenol polyoxyethylene ether;

[0010] Further, the defoamer is a GP type defoamer;

[0011] Further, the preservative is isothiazolinone or kasone;

[0012] Furthermore, a method for preparing a tire disassembly lubricating paste comprises the following steps: heating water to 70-80° C., adding sodium lactate or sodium lauryl sulfate and an emulsifier, stirring, then adding polyethylene glycol, polyethylene glycol stearate, a defoamer, and a preservative, stirring for 1-2 hours, and cooling and solidifying to obtain the tire disassembly lubricating paste;

[0013] Furthermore, the water heating temperature is 70°C.

[0014] Due to the adoption of the above technical solution, the beneficial technical effects of the present invention are:

[0015] 1. The present invention designs a tire disassembly and assembly lubricating paste, which is an environmentally friendly water-based lubricating paste, does not contain petroleum and silicone oil, has a suitable drying speed, and compared with the prior art, reduces the damage to the tire during the disassembly and assembly process and prevents the rim from being deformed due to excessive force;

[0016] 2. The tire disassembly and assembly lubricating paste of the present invention forms a dense film after drying, which not only makes tire disassembly and assembly more convenient but also fills the small gap of the stopper, so that the tire and the rim are tightly combined, and prevents the tire and the rim from relative displacement during vehicle driving;

[0017] 3. One kilogram of the tire disassembly and assembly lubricating paste of the present invention can disassemble and assemble more than 100 tires, thus comprehensively reducing the production cost for the enterprise;

[0018] 4. The manufacturing process of the tire disassembly and assembly lubricating paste of the present invention is simple and controllable, and has no pollution to the environment. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] A tire disassembly and assembly lubricating paste comprises, by weight: 7-11 parts of sodium lactate or sodium lauryl sulfate, 5-9 parts of emulsifier, 3-6 parts of polyethylene glycol, 2-4 parts of polyethylene glycol stearate, 0.1-2 parts of defoamer, 0.1-1 parts of preservative and 65-80 parts of water. Sodium lactate or sodium dodecyl sulfate makes the lubricating paste have a certain hardness. If the amount is small or not added, the product cannot become a paste; the emulsifier makes the lubricating paste have a certain softness. If not added or added in a small amount, the product will be too hard; polyethylene glycol makes the drying speed of the lubricating paste suitable. If not added or added in a small amount, the product will dry too fast and it will be difficult to disassemble and assemble the tire; polyethylene glycol stearate makes the lubricating paste have good lubricity. If not added or added in a small amount, the product will have very poor lubricity; the defoaming agent improves the appearance of the lubricating paste, otherwise there will be many pores, affecting the appearance of the product; the synergistic effect between the various components makes the lubricating paste weakly alkaline, with good lubricity, suitable drying speed, suitable cone penetration, and a dense film is formed on the tire surface after brushing and drying, which has good compatibility with rubber, prevents rust and protects the rim, and does not pollute the environment.

[0021] The dosage ratio of polyethylene glycol to polyethylene glycol stearate is 1-2: 1. Reasonably control the dosage ratio of polyethylene glycol to polyethylene glycol stearate to balance the drying speed and lubricating performance of the lubricating paste to achieve the best effect.

[0022] Furthermore, the emulsifier is a nonionic emulsifier and can have a synergistic effect with other substances in the formulation.

[0023] The nonionic emulsifier is sorbitan fatty acid ester or alkylphenol polyoxyethylene ether.

[0024] The defoamer is a GP type defoamer, and specifically, the GP type defoamer is a silicon-free modified polyether defoamer.

[0025] A preparation method of a tire disassembly lubricating paste comprises the following steps: heating water to 70-80°C, adding sodium lactate or sodium lauryl sulfate and an emulsifier, stirring, then adding polyethylene glycol, polyethylene glycol stearate, a defoamer, and a preservative, stirring for 1-2 hours, and cooling and solidifying to obtain the tire disassembly lubricating paste. The method is simple and controllable, and has no pollution to the environment.

[0026] Example 1

[0027] The tire disassembly and assembly lubricating paste comprises, by mass: 7 parts of sodium lactate, 3 parts of polyethylene glycol, 9 parts of sorbitan fatty acid ester, 3 parts of polyethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 76 parts of water.

[0028] The preparation steps are as follows:

[0029] 1. Heat 76 parts of water to 70°C, then put 7 parts of sodium lactate and 9 parts of sorbitan fatty acid ester into a stirring tank and stir evenly to obtain a premix.

[0030] 2. Add 3 parts of polyethylene glycol, 3 parts of polyethylene glycol stearate, 1 part of silicon-free modified polyether defoamer and 1 part of isothiazolinone into the reaction kettle.

[0031] 3. Add the premixed material in step 1 into the reactor and mix it with the raw materials in step 2. Stir for 1.5 hours. After stirring evenly, cool naturally or water cool to 60° C., fill while hot, and obtain a tire disassembly and assembly lubricating paste product after cooling and solidification.

[0032] Example 2

[0033] The tire disassembly and assembly lubricating paste includes, by mass: 11 parts of sodium lactate, 6 parts of polyethylene glycol, 5 parts of alkylphenol polyoxyethylene ether, 2 parts of ethylene glycol stearate, 0.1 part of silicon-free modified polyether defoaming agent, 0.1 part of kason, and 80 parts of water.

[0034] The preparation steps are as follows:

[0035] 1. Heat 80 parts of water to 75°C, then put 11 parts of sodium lactate and 5 parts of alkylphenol polyoxyethylene ether into a stirring tank and stir evenly to obtain a premix.

[0036] 2. Add 6 parts of polyethylene glycol, 2 parts of polyethylene glycol stearate, 0.1 parts of silicon-free modified polyether defoamer and 0.1 parts of Kathon into the reactor.

[0037] 3. Add the premixed material in step 1 into the reactor and mix it with the raw materials in step 2. Stir for 1 hour. After stirring evenly, cool naturally or water cool to 60° C., fill while hot, and obtain the tire disassembly and assembly lubricating paste product after cooling and solidification.

[0038] Example 3

[0039] The tire disassembly and assembly lubricating paste comprises, by mass: 10 parts of sodium lauryl sulfate, 6 parts of polyethylene glycol, 5 parts of sorbitan fatty acid ester, 2 parts of ethylene glycol stearate, 1.5 parts of silicon-free modified polyether defoamer, 0.2 parts of isothiazolinone, and 75 parts of water.

[0040] The preparation steps are as follows:

[0041] 1. Heat 75 parts of water to 80°C, then put 10 parts of sodium lauryl sulfate and 5 parts of sorbitan fatty acid ester into a stirring tank and stir evenly to obtain a premix.

[0042] 2. Add 6 parts of polyethylene glycol, 2 parts of polyethylene glycol stearate, 1.5 parts of silicon-free modified polyether defoamer and 0.2 parts of isothiazolinone into the reaction kettle.

[0043] 3. Add the premixed material in step 1 into the reactor and mix it with the raw materials in step 2. Stir for 2 hours. After stirring evenly, cool naturally or water cool to 60° C., fill while hot, and obtain the tire disassembly and assembly lubricating paste product after cooling and solidification.

[0044] Example 4

[0045] The tire disassembly and assembly lubricating paste comprises, by mass: 8 parts of sodium lactate, 4 parts of polyethylene glycol, 6 parts of dehydrated sorbitan fatty acid ester, 3 parts of ethylene glycol stearate, 2 parts of silicon-free modified polyether defoaming agent, 1 part of kason and 65 parts of water.

[0046] The preparation steps are as follows:

[0047] 1. Heat 65 parts of water to 75°C, then put 8 parts of sodium lactate and 6 parts of sorbitan fatty acid ester into a stirring tank and stir evenly to obtain a premix.

[0048] 2. Add 4 parts of polyethylene glycol, 3 parts of polyethylene glycol stearate, 2 parts of silicon-free modified polyether defoamer and 1 part of Kathon into the reactor.

[0049] 3. Add the premixed material in step 1 into the reactor and mix it with the raw materials in step 2. Stir for 2 hours. After stirring evenly, cool naturally or water cool to 60° C., fill while hot, and obtain the tire disassembly and assembly lubricating paste product after cooling and solidification.

[0050] Comparative Example 1

[0051] The raw material ratio of comparative example 1 is calculated by mass:

[0052] 5 parts of polyethylene glycol, 11 parts of sorbitan fatty acid ester, 4 parts of polyethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 78 parts of water. Other steps are the same as those in Example 1.

[0053] Comparative Example 2

[0054] The raw material ratio of comparative example 2 includes by mass:

[0055] 7 parts of sodium lactate, 11 parts of sorbitan fatty acid ester, 4 parts of polyethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 78 parts of water. Other steps are the same as those in Example 1.

[0056] Comparative Example 3

[0057] The raw material ratio of comparative example 3 is calculated by mass:

[0058] 7 parts of sodium lactate, 3 parts of polyethylene glycol, 10 parts of sorbitan fatty acid ester, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 78 parts of water. Other steps are the same as those in Example 1.

[0059] Comparative Example 4

[0060] The raw material ratio of Comparative Example 4 is calculated by mass:

[0061] 8 parts of sodium lactate, 6 parts of polyethylene glycol, 6 parts of polyethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 78 parts of water. Other steps are the same as those in Example 1.

[0062] Comparative Example 5

[0063] The raw material ratio of comparative example 5 is calculated by mass:

[0064] 9 parts of sodium lactate, 3 parts of polyethylene glycol, 9 parts of sorbitan fatty acid ester, 3 parts of polyethylene glycol stearate, 1 part of isothiazolinone, and 75 parts of water. Other steps are the same as those in Example 1.

[0065] Comparative Example 6

[0066] The raw material ratio of Comparative Example 6 includes, by mass:

[0067] 6 parts of sodium lactate, 4 parts of polyethylene glycol, 11 parts of sorbitan fatty acid ester, 3 parts of ethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 74 parts of water. Other steps are the same as those in Example 1.

[0068] Comparative Example 7

[0069] The raw material ratio of Comparative Example 7 is calculated by mass:

[0070] 7 parts of sodium lactate, 1 part of polyethylene glycol, 8 parts of sorbitan fatty acid ester, 4 parts of ethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 78 parts of water.

[0071] The temperature of water heating in the preparation step was 90°C.

[0072] Comparative Example 8

[0073] The raw material ratio of Comparative Example 8 is calculated by mass:

[0074] 8 parts of sodium lactate, 4 parts of polyethylene glycol, 4 parts of sorbitan fatty acid ester, 4 parts of ethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 78 parts of water.

[0075] The temperature of water heating in the preparation step was 60°C.

[0076] Comparative Example 9

[0077] The raw material ratio of Comparative Example 9 includes, by mass:

[0078] 9 parts of sodium lactate, 5 parts of polyethylene glycol, 9 parts of sorbitan fatty acid ester, 0.5 parts of ethylene glycol stearate, 1 part of silicon-free modified polyether defoamer, 1 part of isothiazolinone, and 75 parts of water. Other steps are the same as those in Example 1.

[0079] The lubricating pastes prepared in Examples 1-4 and Comparative Examples 1-9 were tested and analyzed to obtain the data shown in Table 1.

[0080] Table 1 Test results of lubricating pastes prepared in Examples 1-4 and Comparative Examples 1-9

[0081]

[0082] As can be seen from the table above, comparative example 1 (no sodium lactate) and comparative example 6 (low sodium lactate addition) cannot become a paste during the processing. Analysis shows that sodium lactate gives the product a certain hardness and can become a paste during the cooling process of the product. Its number of parts cannot be less than 7 parts.

[0083] The softness of the product is expressed by the cone penetration value. Comparative Examples 4 and 8 do not add sorbitan fatty acid ester or add too little, the cone penetration value of the product is very low, and the product hardness is large. This shows that sorbitan fatty ester can make the paste have a certain softness. Its value should not be less than 5 parts.

[0084] Drying speed: Comparative Examples 2 and 7 do not add or add less polyethylene glycol, and the product dries very quickly, which is not conducive to the disassembly and assembly of tires. This shows that the appropriate amount of polyethylene glycol makes the product dry at a suitable speed. Its amount cannot be less than 3 parts.

[0085] Lubricity: Comparative Examples 3 and 9 do not add or add less polyethylene glycol stearate, and the lubricity of the products is very poor. This shows that polyethylene glycol stearate is to make the product have good lubricity, and its proportion cannot be less than 2 parts.

[0086] The tire disassembly and assembly lubricating paste of the present invention forms a dense film after drying, does not contain petroleum and silicone oil, and has a suitable drying speed. One kilogram of the tire disassembly and assembly lubricating paste of the present invention can disassemble and assemble more than 100 tires, thereby comprehensively reducing the production cost for enterprises.

[0087] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A tire disassembly and assembly lubricating paste, characterized in that: The composition is composed of the following components by mass: 7 parts of sodium lactate, 9 parts of emulsifier, 3 parts of polyethylene glycol, 3 parts of polyethylene glycol stearate, 1 part of defoamer, 1 part of preservative, and 76 parts of water; The emulsifier is sorbitan fatty acid ester; The preparation method of the tire disassembly and assembly lubricating paste comprises the following steps: heating water to 70-80° C., adding sodium lactate and an emulsifier, stirring, then adding polyethylene glycol, polyethylene glycol stearate, a defoamer, and a preservative, stirring for 1-2 hours, and cooling and solidifying to obtain the tire disassembly and assembly lubricating paste.

2. A tire disassembly and assembly lubricating paste according to claim 1, characterized in that: The defoamer is a GP type defoamer.

3. The tire disassembly and assembly lubricating paste according to claim 1, characterized in that: The preservative is isothiazolinone or kasone.

4. The tire disassembly and assembly lubricating paste according to claim 1, characterized in that: The water heating temperature is 70°C.

Citation Information

Patent Citations

  • Lubricating agent for tyre assembling and preparation method thereof

    CN107118829A