A ferritic stainless steel 00Cr17 and a heating method thereof

Through specific heating and tempering treatment of 00Cr17 ferritic stainless steel, the problems of surface quality and yield rate are solved, an efficient processing process is achieved, the material performance and yield rate are improved, and it is suitable for subsequent cold deformation and mechanical processing.

CN115976312BActive Publication Date: 2024-10-18CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211700210.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-18
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

In the existing technology, it is difficult to ensure the surface quality and yield rate of 00Cr17 ferritic stainless steel during hot deformation, and the annealing method is not suitable for subsequent cold deformation and mechanical processing.

Method used

Heating method: heat the 00Cr17 ferritic stainless steel billet to 950-980°C, perform high-pressure water descaling, hot-roll deformation to 600-900°C, then air-cool to room temperature, and then perform tempering treatment at 800-830°C. Keep warm for 0.5-1 hour, then air-cool or air-cool to room temperature.

Benefits of technology

The surface quality of 00Cr17 ferritic stainless steel is improved, the internal stress during processing is eliminated, and the material properties are improved. The yield rate reaches more than 95%. The process is scientific and reasonable, cost-effective, and easy to operate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976312B_ABST
    Figure CN115976312B_ABST
Patent Text Reader

Abstract

The invention discloses a ferritic stainless steel 00Cr17 and a heating method thereof, and relates to the technical field of iron and steel metallurgy. The method comprises: heating a ferritic stainless steel 00Cr17 billet; performing high-pressure water descaling on the heated ferritic stainless steel 00Cr17 billet to form a 00Cr17 steel; hot-rolling and deforming the 00Cr17 steel to a specified size, and then air-cooling the steel to room temperature; and tempering the 00Cr17 steel after air-cooling to room temperature, and then air-cooling or air-cooling the steel to room temperature. The method of the invention greatly improves the surface quality of the 00Cr17 ferritic stainless steel, effectively eliminates the internal stress generated by the material during the processing, and obtains a recrystallized structure that is beneficial to improving the performance of the material itself.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a ferritic stainless steel 00Cr17 and a heating method thereof. Background Art

[0002] Foreign developed countries have successfully developed 00Cr17, a substitute for 304 and 316, since the 1970s. After the 1980s, developed countries represented by Japan have mass-produced and applied this steel. However, when 00Cr17 ferritic stainless steel is hot-deformed, a suitable heating temperature is required to ensure the surface quality of 00Cr17 ferritic stainless steel and improve the yield rate. After hot-rolling and tempering, 00Cr17 ferritic stainless steel has good comprehensive strength and toughness properties, which is suitable for subsequent cold deformation and mechanical processing.

[0003] Patent CN102363869A discloses "a method for manufacturing free-cutting ferritic stainless steel 430FM": molten steel is initially smelted in an electric arc furnace, and then the molten steel is refined in a ladle refining furnace and a vacuum oxygen decarburization refining furnace to obtain steel, wherein the steel contains 0.10-0.16wt% C, no more than 1.30wt% Mn, no more than 1.00wt% Si, no more than 0.060wt% P, more than 0.150wt% S, 15.00-17.00wt% Cr, no more than 0.60wt% Ni, 0.20-0.60wt% Mo, 0.0005-0.0030wt% Ca, 0.0010-0.0060wt% rare earth elements, and the remainder is iron and unavoidable impurities, and the ratio of Mn content to S content is not less than 4.

[0004] Patent CN107475491A discloses "a heat treatment process for ferritic stainless steel": including two annealing operations, the specific steps are as follows: A: annealing the material to be annealed at 900°C for 2 hours, and then air-cooling to room temperature; B: annealing the material cooled to room temperature at 850°C for 2 hours, and then air-cooling to room temperature.

[0005] Patent CN110343948B discloses "a ferritic stainless steel CB30 material and its heat treatment process": including the following steps: A: heating the ferritic stainless steel CB30 material to 770-800℃, then keeping it warm for 0.5h, and cooling it with coolant; B: heating the cooled ferritic stainless steel CB30 material to 600-650℃, keeping it warm for 30min for tempering, and cooling it to room temperature by air cooling after the insulation is completed. The temperature cooling rate must be greater than or equal to 200℃ / min.

[0006] In the above-mentioned prior art, there is no description about the production heating process, some of them need to go through two high-temperature annealing methods, and some are not suitable for subsequent cold deformation and mechanical processing. Summary of the invention

[0007] The present invention aims to provide a ferritic stainless steel 00Cr17 and a heating method thereof, which greatly improves the surface quality of the 00Cr17 ferritic stainless steel, effectively eliminates the internal stress generated in the material during processing, and obtains a recrystallized structure that is beneficial to improving the performance of the material itself.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] According to one aspect of the present disclosure, a method for heating ferritic stainless steel 00Cr17 is provided, the method comprising the following steps:

[0010] The ferritic stainless steel 00Cr17 billet is heated;

[0011] Descaling the heated ferritic stainless steel 00Cr17 billet with high pressure water to form a 00Cr17 steel material;

[0012] The 00Cr17 steel is hot-rolled and deformed to a specified size, and then air-cooled to room temperature;

[0013] After being air-cooled to room temperature, the 00Cr17 steel is tempered and then air-cooled or air-cooled to room temperature.

[0014] In a possible implementation, the heating temperature is 950-980°C.

[0015] In a possible implementation, the water pressure range of the high-pressure water descaling is 16 MPa to 28 MPa.

[0016] In a possible implementation, the temperature of the hot rolling deformation is 600°C to 900°C.

[0017] In a possible implementation manner, the final temperature of the hot rolling deformation is ≥ 600°C.

[0018] In a possible implementation manner, the tempering conditions include:

[0019] The tempering temperature is 800-830℃; the holding time is 0.5~1h.

[0020] According to one aspect of the present disclosure, a ferritic stainless steel 00Cr17 is provided, and the chemical composition and mass percentage of the ferritic stainless steel 00Cr17 include:

[0021] C: ≤0.02wt%; Si: 0.2-0.5wt%; Mn: ≤0.15wt%; P: ≤0.04wt%; S: ≤0.01wt%;

[0022] Cr: 16.8-18.5wt%; N: ≤0.015wt%; the balance is Fe and unavoidable impurities.

[0023] In a possible implementation manner, the yield rate of the ferritic stainless steel 00Cr17 is ≥97%.

[0024] Technical effects and advantages of the present invention:

[0025] The heating method of ferritic stainless steel 00Cr17 of the present invention can improve the surface quality of 00Cr17 ferritic stainless steel by hot rolling and tempering after heating in a specific temperature range, eliminate the internal stress generated by the material during the processing, obtain the recrystallization structure that is beneficial to improving the performance of the material itself, and increase the yield rate of 00Cr17 to more than 95%. The method is scientific, reasonable, economical, efficient and easy to operate.

[0026] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A flow chart of a heating method for ferritic stainless steel 00Cr17 according to an exemplary embodiment of the present invention;

[0028] Figure 2 The figure is a curve diagram showing the changes of the cross-sectional shrinkage and tensile strength of ferritic stainless steel 00Cr17 at different temperatures as a function of temperature according to an exemplary embodiment of the present invention;

[0029] Figure 3 This is a picture of the finished product under the first heating process in exemplary embodiment 1 of the present invention;

[0030] Figure 4 This is a picture of the finished product under the second heating process in exemplary embodiment 1 of the present invention;

[0031] Figure 5 This is a picture of the finished product under the third heating process in exemplary embodiment 1 of the present invention;

[0032] Figure 6 The finished product grain map under the (1) heating process in the exemplary embodiment 1 of the present invention;

[0033] Figure 7is a finished product grain map under the second heating process in exemplary embodiment 1 of the present invention;

[0034] Figure 8 is a finished product grain map under the third heating process in exemplary embodiment 1 of the present invention;

[0035] Fig. 9 is a finished product grain map under the first heating process in exemplary embodiment 2 of the present invention;

[0036] Fig.10 is a finished product grain map under the (2nd) heating process in exemplary embodiment 2 of the present invention;

[0037] Fig.11 This is a finished grain map of the third heating process in exemplary embodiment 2 of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Figure 1 A flow chart of a heating method for ferritic stainless steel 00Cr17 according to an exemplary embodiment of the present invention is shown in FIG. Figure 1 As shown, an exemplary embodiment of the present invention provides a heating method for ferritic stainless steel 00Cr17, comprising the following steps:

[0040] Step S1, heating the ferritic stainless steel 00Cr17 billet to 950° C. to 980° C.;

[0041] The optimal rolling temperature of ferritic stainless steel 00Cr17 is 600℃~900℃ and 1050~1350℃. Figure 2 The figure is a curve diagram showing the changes of the cross-sectional shrinkage and tensile strength of the ferritic stainless steel 00Cr17 at different temperatures with the temperature. Figure 2As shown in the figure, the tensile strength of 00Cr17 ferritic stainless steel decreases with increasing temperature; the change pattern of cross-sectional shrinkage with increasing tensile temperature is more complicated: the cross-sectional shrinkage is greater than 60% at 600-900℃; the cross-sectional shrinkage is less than 60% at 950℃ and 1000℃, and an obvious brittle zone appears in the temperature range of 900-1050℃; with the further increase of temperature, the cross-sectional shrinkage is greater than 60% after 1050℃, and good plasticity is obtained; when the temperature is greater than 1350℃, the cross-sectional shrinkage is less than 60%, and the plasticity decreases rapidly. That is, the thermoplasticity of 00Cr17 ferritic stainless steel has four characteristic temperature ranges: (1) low temperature plastic zone of 600-900℃; (2) medium temperature brittle zone of 900-1050℃; (3) high temperature plastic zone of 1050-1350℃; (4) high temperature brittle zone above 1350℃.

[0042] However, the higher the heating temperature during the heating and rolling process of the steel billet, the coarser the grains formed after recrystallization will be; at the same time, high temperature will reduce the strength of the steel, and it is easy to cause scratches during contact with the mold; in addition, the higher the heating temperature, the more fuel is consumed. For the above reasons, in this embodiment, the rolling temperature of the ferritic stainless steel 00Cr17 is set at 600℃~900℃.

[0043] At the same time, in order to avoid the formation of coarse grains after crystallization, the initial heating temperature of ferritic stainless steel 00Cr17 should not be too high. Preferably, in this embodiment, when heating the ferritic stainless steel 00Cr17 billet, the billet temperature is controlled at 950℃~980℃. The reason is as follows: After the billet is taken out of the furnace, it is necessary to perform operations such as high-pressure water dephosphorization. During this process, the temperature of the billet usually drops by 80℃~100℃. When hot rolling begins, its temperature has dropped to 850℃~900℃, which is just within the optimal rolling range of 600℃~900℃. However, the temperature of ferritic stainless steel 00Cr17 continues to drop during the rolling process. Therefore, in order to ensure that ferritic stainless steel 00Cr17 is always at the optimal rolling temperature during the rolling process, the temperature of ferritic stainless steel 00Cr17 should be ensured to be not less than 600℃ at the end of the final rolling.

[0044] Furthermore, the calculation formula for the heating time of the blank is: T=ad; wherein a represents the heating coefficient, the unit is mm / s (a=15~20), d represents the side length of the blank, the unit is mm, and T represents the heating time of the blank, the unit is s; for example, a square blank with a size of 150mm*150mm is selected, and its heating time is (15~20)*150 seconds, which is 37.5~50 minutes.

[0045] Specifically, the implementation step can be completed in a walking beam heating furnace.

[0046] Step S2, descaling the ferritic stainless steel 00Cr17 billet after heating with high pressure water to form 00Cr17 steel;

[0047] In the production process of hot-rolled steel, the furnace-generated iron scale on the surface of the billet is one of the main reasons affecting the surface quality of the steel. Due to its existence, various product defects such as pits, pitting, and iron oxide intrusion are generated on the surface of the steel. Therefore, in order to avoid the above problems, it is necessary to remove the iron scale on the surface of the billet in this step. Exemplarily, the descaling method can be high-pressure water dephosphorization: after the billet is taken out of the heating furnace, the iron scale covering its surface is rapidly cooled, and the iron scale generated in the furnace presents a network of cracks. Under the spraying of high-pressure water, the surface of the iron scale is locally cooled, resulting in a large contraction, thereby expanding the cracks of the iron scale. After the impact of the high-pressure water flow, the dynamic pressure of the high-pressure water in the crack becomes the static pressure of the fluid and drives into the bottom of the iron scale, so that the iron scale peels off from the surface of the billet, achieving the purpose of removing the iron scale. Specifically, the water pressure range of high-pressure water descaling is about 16MPa~28MPa.

[0048] Specifically, this implementation step can be completed using high-pressure descaling equipment.

[0049] Step S3, hot-rolling and deforming the 00Cr17 steel to a specified size, and then air-cooling to room temperature;

[0050] As described in step S1, the optimal rolling temperature of ferritic stainless steel 00Cr17 is between 600°C and 900°C. The temperature of ferritic stainless steel 00Cr17 will continue to drop during hot rolling. Therefore, in order to ensure that ferritic stainless steel 00Cr17 is always at the optimal rolling temperature during the rolling process, the temperature of ferritic stainless steel 00Cr17 should be no less than 600°C at the end of final rolling. After rolling, it can be quickly cooled to room temperature by air cooling for the next process.

[0051] Specifically, this implementation step can be completed using hot rolling equipment.

[0052] Step S4, tempering the 00Cr17 steel after cooling to room temperature.

[0053] In this step, the 00Cr17 steel obtained in step S3 is tempered to eliminate the internal stress generated in the material during processing. The specific treatment method is: heat the 00Cr17 steel to 800-830°C and keep it warm for 0.5-1h, and then cool it to room temperature by air or wind. The tempering treatment can statically recrystallize the deformed ferrite grains to obtain fine ferrite grains, thereby improving the comprehensive properties of strength and toughness of 00Cr17 ferritic stainless steel, and at the same time facilitate subsequent cold deformation and mechanical processing.

[0054] Specifically, this implementation step can be completed using a tempering furnace.

[0055] Example 1

[0056] The ferritic stainless steel 00Cr17 continuous casting billet of 150mm*150mm*6000mm was selected and rolled into a ∮5.5 round plate. The billet temperature was controlled at 950-980℃, and the scale was removed by high-pressure water after leaving the furnace. The wire drawing temperature was 600-680℃ after hot rolling, and it was air-cooled to room temperature. The main components of the steel are shown in Table 1 in terms of mass percentage. After the ∮5.5 round plate of the 00Cr17 steel was subjected to different heating processes + hot rolling + tempering, the surface conditions of the products were compared.

[0057] Table 100Cr17 steel chemical composition

[0058] Steel Type C Si Mn P S Cr N 00Cr17 0.01 0.28 0.16 0.015 0.002 17.7 0.01

[0059] The following three heating processes are carried out respectively:

[0060] (1) The 00Cr17 continuous casting billet was heated to 1080°C in a heating furnace and kept at this temperature for 45 minutes; hot rolled, air cooled to room temperature; and tempered at 830°C.

[0061] (2) The 00Cr17 continuous casting billet is heated to 1000°C in a heating furnace and kept at this temperature for 45 minutes; hot rolled, air cooled to room temperature; and tempered at 830°C.

[0062] (3) The 00Cr17 continuous casting billet is heated to 980°C in a heating furnace and kept at this temperature for 45 minutes; hot rolled, air cooled to room temperature; and tempered at 830°C.

[0063] Due to the long heating time in the heating furnace below 950℃ 23 C6 will aggregate and precipitate at the grain boundaries of the ingot (the columnar grains of the ingot are very large), and it is easy to crack during rolling, so heating below 950°C is not recommended.

[0064] Figure 3 This is a picture of the finished product under the first heating process in exemplary embodiment 1 of the present invention; Figure 4 This is a picture of the finished product under the second heating process in exemplary embodiment 1 of the present invention; Figure 5 This is a picture of the finished product under the third heating process in the exemplary embodiment 1 of the present invention; a comparison of the finished products under different heating processes Figure 3 , Figure 4 and Figure 5 It can be seen that the surface quality of the finished product obtained by the heating method (3) is the best. The surface quality of the products after the heating process (1) and the heating process (2) is poor, while the surface quality of the product after the heating process (3) is the best.

[0065] Figure 6The finished product grain map under the (1) heating process in the exemplary embodiment 1 of the present invention; Figure 7 is a finished product grain map under the second heating process in exemplary embodiment 1 of the present invention; Figure 8 The finished grain diagram of the third heating process in the exemplary embodiment 1 of the present invention is shown; the finished grain diagram of the third heating process is compared with the finished grain diagram of the third heating process. Figure 6 , Figure 7 and Figure 8 It can be seen that the finished product obtained by the third heating method has finer grains, which further indicates that the finished product obtained by the third heating method has better strength and toughness.

[0066] At the same time, the yield rate under different heating process conditions was measured. As shown in Table 2 below, the yield rate of the first heating process is 0%, the yield rate of the second heating process is only 5%, and the yield rate of the third heating process reaches 97%, indicating that the heating method of the present invention can effectively improve the yield rate of 00Cr17.

[0067] Table 2 Yield rate of different heating processes

[0068] Technology Yield (1) Heating process 0% (2) Heating process 5% (3) Heating process 97%

[0069] Example 2

[0070] The same test materials as those in Example 1 were selected, and the ferritic stainless steel 00Cr17 continuous casting billet was 150mm*150mm*6000mm, rolled into a ∮5.5 round plate, the billet temperature was controlled at 950-980℃, the billet was descaled by high-pressure water after leaving the furnace, the wire drawing temperature was 600-680℃ after hot rolling, and air-cooled to room temperature; the main components of the steel are shown in Table 3 in terms of mass percentage. The surface conditions of the ∮5.5 round plates of the 00Cr17 steel were compared after different heating processes + hot rolling + tempering.

[0071] Table 300Cr17 steel chemical composition

[0072] Steel Type C Si Mn P S Cr N 00Cr17 0.01 0.28 0.16 0.015 0.002 17.7 0.01

[0073] The following three heating processes are carried out respectively:

[0074] (1) The 00Cr17 continuous casting billet was heated to 980°C in a heating furnace and kept at this temperature for 45 minutes; hot rolled, air cooled to room temperature; and tempered at 830°C.

[0075] (2) The 00Cr17 continuous casting billet is heated to 980°C in a heating furnace and kept at this temperature for 45 minutes; hot rolled, air cooled to room temperature; and tempered at 880°C.

[0076] (3) The 00Cr17 continuous casting billet is heated to 980°C in a heating furnace and kept at this temperature for 45 minutes; hot rolled, air cooled to room temperature; and tempered at 950°C.

[0077] Fig. 9 is a finished product grain map under the first heating process in exemplary embodiment 2 of the present invention; Fig.10 is a finished product grain map under the (2nd) heating process in exemplary embodiment 2 of the present invention; Fig.11 This is a finished grain diagram of the third heating process in the exemplary embodiment 2 of the present invention; a comparison of finished grains under different heating processes Fig. 9 , Fig.10 and Fig.11 It can be seen that the finished product obtained by the heating method (1) has the finest grains, which further indicates that the finished product obtained by the heating method (1) has better strength and toughness.

[0078] At present, this method has been put into practical application and production. As the international nickel price continues to rise, 00Cr17 ferritic stainless steel has a good market prospect as an alternative to 304 high-nickel steel, and the product has high added value. When the product yield rate is increased to more than 95%, the economic benefit is expected to reach 10 million per year.

[0079] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A heating method for ferritic stainless steel 00Cr17, It is characterized in that The method comprises the following steps: The ferritic stainless steel 00Cr17 billet is heated to a temperature of 950-980° C. The heating time of the billet is calculated as follows: T=ad; wherein a represents the heating coefficient, in units of mm / s, a=15-20, d represents the side length of the billet, in units of mm, and T represents the heating time of the billet, in units of s; The heated ferritic stainless steel 00Cr17 billet is subjected to high-pressure water descaling to form 00Cr17 steel, wherein the water pressure range of the high-pressure water descaling is 16MPa-28MPa; The 00Cr17 steel is hot-rolled to a specified size and then air-cooled to room temperature; the hot-rolling deformation temperature is 600°C to 900°C, and the final temperature of the hot-rolling deformation is ≥ 600°C; The 00Cr17 steel material after air cooling to room temperature is tempered and then air cooled or air cooled to room temperature; the tempering conditions include: the tempering temperature is 800-830°C; the holding time is 0.5-1h.

2. A ferritic stainless steel 00Cr17, prepared by the method according to claim 1, It is characterized in that The chemical composition and mass percentage of the ferritic stainless steel 00Cr17 include: C: ≤0.02wt%; Si: 0.2-0.5wt%; Mn: ≤0.15wt%; P: ≤0.04wt%; S: ≤0.01wt%; Cr: 16.8-18.5wt%; N: ≤0.015wt%; the balance is Fe and unavoidable impurities.

3. The ferritic stainless steel 00Cr17 according to claim 2, It is characterized in that The yield rate of the ferritic stainless steel 00Cr17 is ≥97%.

Citation Information

Patent Citations

  • Manufacturing method of free-cutting ferritic stainless steel 430FM

    CN102363869A

  • Heat treatment process of ferrite stainless steel

    CN107475491A

  • A ferritic stainless steel CB30 material and its heat treatment process

    CN110343948B