Coated particles and method for producing the same

Coated particles with conductive particles and insulating fine particles having no glass transition temperature address short circuit and insulation issues by maintaining shape and hardness, ensuring reliable conduction and insulation.

CN115989252BActive Publication Date: 2024-12-03NIPPON CHEMICAL IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180052261.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-24
Filing Date
2021-08-18
Publication Date
2024-12-03
Estimated Expiration
2041-08-18

AI Technical Summary

Technical Problem

Anisotropic conductive materials using conductive particles with small particle sizes face issues of short circuits due to undesirable conduction and inadequate insulation reliability, particularly when thermocompressed, as the insulating resin particles deform and entangle between electrodes.

Method used

The development of coated particles with conductive particles coated by insulating fine particles having no glass transition temperature and a sphericity of 0.90 or more, achieved through a method involving polymerization of non-crosslinking and crosslinking monomer components to maintain shape and hardness during thermal compression.

Benefits of technology

The coated particles ensure excellent conduction reliability and insulation reliability by preventing short circuits and maintaining a spherical shape during thermocompression, enhancing connectivity with electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004092527410000101
    Figure BDA0004092527410000101
  • Figure BDA0004092527410000221
    Figure BDA0004092527410000221
  • Figure HDA0004092527430000011
    Figure HDA0004092527430000011
Patent Text Reader

Abstract

The present invention aims to provide coated particles capable of improving conduction reliability and insulation reliability, the coated particles comprising conductive particles having a metal coating formed on the surface of a core material and insulating particles coating the conductive particles, wherein the insulating particles do not have a glass transition temperature and have a sphericity of 0.90 or more. The surface layer of the insulating particles is preferably a polymer containing a crosslinkable monomer component, and is also preferably a polymer containing a monomer component having the following functional group, the functional group having an electric charge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to coated particles in which conductive particles are coated with an insulating layer. Background Art

[0002] Conductive particles in which a metal film such as nickel or gold is formed on the surface of resin particles are used as conductive materials such as conductive adhesives, anisotropic conductive films, and anisotropic conductive adhesives.

[0003] In recent years, with the further miniaturization of electronic devices, the circuit width or spacing of electronic circuits has become smaller and smaller. In response to this, the conductive particles used in the above-mentioned conductive adhesives, anisotropic conductive films, anisotropic conductive adhesives, etc. are required to have a small particle size. When using such conductive particles with a small particle size, in order to improve its connectivity, the amount of conductive particles in the conductive material has to be increased. However, if the amount of conductive particles is increased, the following problem will arise: short circuits are generated due to conduction in an undesirable direction, that is, conduction in a direction different from the opposing electrode, and it is difficult to obtain insulation in this direction.

[0004] In order to solve the above problems, insulating layer coated conductive particles are used, in which the surface of the conductive particles is coated with an insulating substance having a functional group having an affinity for the metal film to prevent the metal films of the conductive particles from contacting each other. Coated particles with such a structure are usually made by hot pressing the coated particles between electrodes to melt, deform or peel off the insulating layer, exposing the metal surface of the conductive particles, thereby enabling conduction between the electrodes, but it is known that the technology of improving the characteristics such as conduction reliability by studying the constituent components of the insulating layer is known.

[0005] For example, Patent Document 1 describes that conductive particles are coated with core-shell particles having a higher glass transition temperature or softening temperature than the glass transition temperature or softening temperature of the core particles, and the particles obtained thereby can reliably conduct the connection between substrates and prevent leakage between adjacent particles. In addition, Patent Document 2 describes that the following conductive particles obtained by coating water-soluble and dispersible core-shell particles having a glass transition temperature of -30 to 150°C have excellent current supply and insulation properties, and the core of the core-shell particles contains a copolymer of styrene and 2-ethylhexyl acrylate, and the shell contains a copolymer of styrene and acrylic acid. In addition, Patent Document 3 describes conductive particles obtained by coating resin particles having a glass transition temperature of 180°C or less, which can provide insulating conductive particles that can maintain good conduction between opposing electrodes and reliably suppress lateral conduction, and the resin particles contain a copolymer of polymerizable components that must at least have an alkyl (meth) acrylate and a polyvalent (meth) acrylate.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-149764

[0009] Patent Document 2: Japanese Patent Application No. 2006-525641

[0010] Patent Document 3: Japanese Patent Application Publication No. 2012-72324 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] However, the anisotropic conductive material using the conductive particles described in the above-mentioned patent documents 1 to 3 has the problem of failing to exhibit the desired conductivity because the insulating resin particles cannot ensure the desired hardness when the electrodes are thermocompressed, and the deformed insulating resin particles are entangled and remain between the conductive layer of the conductive particles and the electrodes. In order to reduce the influence of heat on the hardness of the resin particles, it is conceivable to increase the proportion of cross-linking monomer components during the production of the resin particles and then polymerize them to obtain harder resin particles. However, if the proportion of the cross-linking monomer components is increased, the shape of the particles will be deformed, and it will be difficult to control the particle size, so that problems will arise in terms of insulation reliability.

[0013] Therefore, an object of the present invention is to provide coated particles that solve the above-mentioned technical problems and can improve conduction reliability and insulation reliability.

[0014] Technical solutions for solving technical problems

[0015] The inventors of the present invention have conducted intensive research to solve the above technical problems, and as a result, found that when obtaining insulating fine particles, after polymerizing a non-crosslinking monomer component to obtain a spherical core material portion, a crosslinking monomer component is further added for polymerization, so that insulating fine particles having no glass transition temperature, a required hardness, a spherical shape, and a uniform particle size can be obtained. It is also found that the insulating fine particles obtained in this way are not easily deformed during thermal compression, and maintain a spherical shape, and will not remain between the conductive layer and the electrode and be effectively removed. Therefore, the conductive particles coated with the insulating fine particles have excellent conduction reliability, thereby completing the present invention.

[0016] That is, the present invention provides coated particles comprising conductive particles having a metal coating formed on the surface of a core material, and insulating fine particles coating the conductive particles, wherein the insulating fine particles have no glass transition temperature and a sphericity of 0.90 or more.

[0017] In addition, the present invention provides a method for producing coated particles, the coated particles comprising: conductive particles having a metal coating formed on the surface of a core material and insulating fine particles coating the conductive particles, the method comprising:

[0018] A first step of polymerizing a non-crosslinkable monomer component to obtain an insulating fine particle precursor;

[0019] a second step of polymerizing a polymerizable compound containing a crosslinkable monomer component in the presence of an insulating fine particle precursor to obtain insulating fine particles; and

[0020] The third step is to mix the dispersion containing insulating fine particles and conductive particles to allow the insulating fine particles to adhere to the surfaces of the conductive particles.

[0021] Effects of the Invention

[0022] According to the present invention, coated particles coated with spherical insulating fine particles having a uniform particle size and not having a glass transition temperature can be obtained, so coated particles having excellent conduction reliability and insulation reliability and a method for producing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a SEM image of the insulating fine particles obtained in Example 1.

[0024] Figure 2 This is a DSC curve of the insulating fine particles obtained in Example 1 obtained by differential scanning calorimetry.

[0025] Figure 3 is a SEM image of the coated particles obtained in Example 1.

[0026] Figure 4 This is a SEM image of the insulating fine particles obtained in Example 2.

[0027] Figure 5 This is a DSC curve of the insulating fine particles obtained in Example 2 obtained by differential scanning calorimetry.

[0028] Figure 6 This is a SEM image of the insulating fine particles obtained in Comparative Example 1.

[0029] Figure 7 This is a DSC curve of the insulating fine particles obtained in Comparative Example 1 obtained by differential scanning calorimetry.

[0030] Figure 8 This is a SEM image of the insulating fine particles obtained in Comparative Example 2.

[0031] Fig. 9This is a DSC curve of the insulating fine particles obtained in Comparative Example 2 obtained by differential scanning calorimetry.

[0032] Fig.10 This is a SEM image of the insulating fine particles obtained in Comparative Example 3.

[0033] Fig.11 This is a DSC curve of the insulating fine particles obtained in Comparative Example 3 obtained by differential scanning calorimetry. DETAILED DESCRIPTION

[0034] The coated particles of the present invention are described below based on preferred embodiments thereof. The coated particles of the present invention are coated particles comprising conductive particles having a metal coating formed on the surface of a core material, and insulating particles coating the conductive particles, wherein the insulating particles are insulating particles that do not have a glass transition temperature and have a sphericity of 0.90 or more.

[0035] As the conductive particles, known conductive particles conventionally used in conductive adhesives, anisotropic conductive films, and anisotropic conductive adhesives can be used.

[0036] As the core material in the conductive particles, it is granular, whether it is inorganic or organic, it can be used without special restrictions. As the core material particles of inorganic matter, metal particles, alloys, glass, ceramics, silicon dioxide, metal or non-metal oxides (also including hydrates) of gold, silver, copper, nickel, palladium, solder, etc., metal silicates including aluminosilicates, metal carbides, metal nitrides, metal carbonates, metal sulfates, metal phosphates, metal sulfides, metal acid salts, metal halides and carbon, etc. can be listed. On the other hand, as the core material particles of organic matter, thermoplastic resins, alkyd resins, phenolic resins, urea resins, benzoguanamine resins, melamine resins, xylene resins, silicone resins, epoxy resins, diallyl phthalate resins, etc., such as natural fibers, natural resins, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polybutene, polyamides, polyacrylates, polyacrylonitrile, polyacetals, ionomers, polyesters, etc. can be listed. They can be used alone or in combination of two or more.

[0037] The core particles can be composed of a material containing both inorganic and organic substances instead of the material composed of any one of the above-mentioned inorganic and organic substances. In the case where the core particles are composed of a material containing both inorganic and organic substances, as the existence of the inorganic and organic substances in the core particles, for example, a core composed of an inorganic substance and a shell composed of an inorganic substance covering the surface of the core, or a core composed of an organic substance and a shell composed of an inorganic substance covering the surface of the core, etc. can be cited. In addition to these, a mixed type composition in which inorganic and organic substances are mixed or randomly fused in one core particle can also be cited. As a core particle composed of a material containing both inorganic and organic substances, the material constituting the core particles of the above-mentioned inorganic substance or the core particles of the organic substance can be used. The core particles can use each material of the inorganic substance and the organic substance in a separate composition, or can use the inorganic substance and the organic substance in a composition of two or more materials.

[0038] The core particles are preferably composed of organic matter or a material comprising both inorganic and organic matter, and more preferably composed of a material comprising both inorganic and organic matter. The above-mentioned inorganic matter is preferably glass, ceramic, silicon dioxide, metal or non-metal oxide (also including hydrate), metal silicate including aluminosilicate, metal carbide, metal nitride, metal carbonate, metal sulfate, metal phosphate, metal sulfide, metal acid salt, metal halide and carbon. In addition, the above-mentioned organic matter is preferably a thermoplastic resin such as natural fiber, natural resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polybutene, polyamide, polyacrylate, polyacrylonitrile, polyacetal, ionomer, polyester. By using a core material composed of such a material, the dispersion stability of the particles can be improved. In addition, when the electronic circuit is electrically connected, it can show appropriate elasticity and improve conduction.

[0039] When an organic substance is used as the core particle, it is preferred that the core particle has no glass transition temperature or has a glass transition temperature exceeding 100°C from the viewpoint of easily maintaining the shape of the core particle in the anisotropic conductive connection process and the shape of the core particle in the process of forming the metal film. In addition, when the core particle has a glass transition temperature, the glass transition temperature is preferably 200°C or less from the viewpoint that the conductive particles are easily softened in the anisotropic conductive connection and the contact area is increased, thereby easily achieving conduction. From this viewpoint, when the core particle has a glass transition temperature, the glass transition temperature is more preferably greater than 100°C and less than 180°C, and particularly preferably greater than 100°C and less than 160°C. The glass transition temperature can be measured by the method described in the examples described later.

[0040] When an organic substance is used as the core particle, when the organic substance is a highly cross-linked resin, the glass transition temperature is hardly observed even when measured at 200°C by the method described in the following examples. In this specification, such particles are referred to as particles without a glass transition temperature, and such core particles can also be used in the present invention. As a specific example of the core particle material without a glass transition temperature, it can be obtained by copolymerizing the monomer constituting the organic substance exemplified above and a cross-linking monomer. Examples of the crosslinking monomer include tetramethylene di(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, ethylene oxide di(meth)acrylate, ethylene tetraoxide (meth)acrylate, 1,6-hexane di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane di(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and tetramethylolpropane tri(meth)acrylate. Methane tetra(meth)acrylate, tetramethylolpropane tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, glycerol di(meth)acrylate, glycerol tri-di(meth)acrylate and other multifunctional (meth)acrylates, divinylbenzene, divinyltoluene and other multifunctional vinyl monomers, vinyltrimethoxysilane, trimethoxysilylstyrene, γ-(meth)acryloxypropyltrimethoxysilane and other silane-containing monomers, triallyl isocyanurate, diallyl phthalate, diallyl acrylamide, diallyl ether and other monomers. In particular, in the field of COG (Chip on Glass), core particles formed of such hard organic materials are often used.

[0041] The shape of the core particles is not particularly limited. Generally, the core particles are spherical. However, the core particles may also be in shapes other than spherical, such as fibrous, hollow, plate-like or needle-like, or may have a plurality of protrusions on the surface or an amorphous shape. In the present invention, spherical core particles are preferred from the viewpoint of excellent filling properties and easy metal coating.

[0042] The shape of the conductive particles also depends on the shape of the core particles, but there is no particular limitation. For example, it can be fibrous, hollow, plate-like or needle-like, or it can be a shape with protrusions on its surface or an amorphous shape. In the present invention, from the viewpoint of excellent filling and connectivity, it is preferably spherical or has a protrusion on the surface. In the case where the conductive particles are in a shape with protrusions on the surface, it is preferred to have multiple protrusions on the surface, and more preferably have multiple protrusions on a spherical surface. In the case where the conductive particles are in a shape with multiple protrusions, the core particles may have multiple protrusions, or the core particles may not have protrusions, while the metal film has multiple protrusions. It is preferred that the core particles have no protrusions and the metal film has a shape with multiple protrusions.

[0043] The coated particles of the present invention may have protrusions on the surface of the conductive particles in order to make electrical conduction reliable. By having protrusions on the surface of the conductive particles, when the conductive particles are compressed by the electrodes during installation, the insulating layer can be effectively pushed away by the protrusions. When the thickness of the insulating layer is set to L, the height H of the protrusions of the conductive particles is greater than or equal to 0.1, which is preferred from the perspective of excluding the insulating layer during installation to make electrical conduction reliable. In addition, H / L is less than 10, which is preferred from the perspective of obtaining filling properties and insulation in a direction different from the opposing electrode. From these viewpoints, H / L is further preferably greater than or equal to 0.2 and less than or equal to 5. In their preferred range, the thickness L refers to the average particle size of the insulating particles when the insulating layer is insulating particles.

[0044] The height H of the protrusion is 20 nm or more on average, and is particularly preferably 50 nm or more. The number of protrusions also depends on the particle size of the conductive particles, but from the viewpoint of further improving the conductivity of the conductive particles, it is preferably 1 to 20,000, particularly 5 to 5,000, per particle on average. In addition, the aspect ratio of the protrusion is preferably 0.3 or more, and more preferably 0.5 or more. If the aspect ratio of the protrusion is large, it is advantageous because it can easily pierce the oxide film formed on the electrode surface. The aspect ratio refers to the ratio of the height H of the protrusion to the length D of the base of the protrusion, that is, the value defined by H / D. The height H of the protrusion and the length D of the base of the protrusion are average values ​​measured by an electron microscope for 20 different particles observed, and the aspect ratio of the protrusion is the average value obtained by calculating the aspect ratios of 20 different particles observed by an electron microscope. The length D of the base refers to the length of the base of the protrusion along the surface of the conductive particle in the electron microscope image.

[0045] The aspect ratio of the protrusions formed on the surface of the conductive particles is as described above. The length D of the base of the protrusion itself is preferably 5 to 500 nm, particularly preferably 10 to 400 nm. The height H of the protrusion is preferably 20 to 500 nm, particularly preferably 50 to 400 nm.

[0046] The metal film in the conductive particles has conductivity, and as its constituent metal, for example, in addition to metals such as gold, platinum, silver, copper, iron, nickel, tin, lead, antimony, bismuth, cobalt, indium, titanium, germanium, aluminum, chromium, palladium, tungsten, molybdenum, or their alloys, metal compounds such as ITO and solder can also be listed. Among them, gold, silver, copper, nickel, palladium or solder is preferred due to its low resistance, and nickel, gold, nickel alloy or gold alloy is particularly suitable for use because it has high binding properties with the functional group when the insulating fine particles of the present invention described later have a functional group. The metal in the conductive particles can be used alone or in combination of two or more.

[0047] The metal film may be a single layer structure or a laminated structure consisting of multiple layers. In the case of a laminated structure consisting of multiple layers, the outermost layer is preferably nickel, gold, a nickel alloy or a gold alloy. From the viewpoint of reducing the amount of expensive precious metals, the outermost layer of the metal film preferably has a small amount of palladium, preferably less than 5% by mass, more preferably less than 1% by mass, and most preferably does not contain palladium.

[0048] In addition, the metal film may not cover the entire surface of the core particle, but may cover only a portion thereof. In the case of covering only a portion of the surface of the core particle, the covering portion may be continuous or may be discontinuously covered in an island shape, for example. The thickness of the metal film is preferably 0.001 μm or more and 2 μm or less.

[0049] Examples of methods for forming a metal film on the surface of the core particles include dry methods such as vapor deposition, sputtering, mechanochemical methods, and hybridization methods, and wet methods such as electrolytic plating and electroless plating methods. In addition, these methods may be combined to form a metal film on the surface of the core particles.

[0050] The average particle size of the conductive particles is preferably 0.1 μm to 50 μm, more preferably 1 μm to 30 μm. When the average particle size of the conductive particles is within the above range, the obtained coated particles will not short-circuit in a direction different from that between the opposing electrodes, and it is easy to ensure the conduction between the opposing electrodes. In addition, in the present invention, the average particle size of the conductive particles is the average value of the particle size measured using a scanning electron microscope (Scanning Electron Microscope: SEM). In which, when the conductive particles are spherical in the scanning electron microscope image, the particle size measured using SEM refers to the diameter of the circular conductive particle image. In the case where the conductive particles are not spherical, the particle size measured using SEM refers to the maximum length (maximum length) in the line segment crossing the conductive particle image. This is also the same for the average particle size of the insulating particles described later. However, in the case where the conductive particles have protrusions, the average of the above-mentioned maximum length of the portion other than the protrusion is taken as the average particle size.

[0051] Specifically, the average particle size of the conductive particles is measured by the method described in Examples.

[0052] The insulating particles used in the present invention to coat the conductive particles do not have a glass transition temperature. Therefore, since the coated particles of the present invention are coated with insulating particles that are not easily deformed during thermocompression bonding, the insulating particles do not remain between the conductive layer and the electrode and are effectively eliminated. Therefore, since the coated particles of the present invention have increased connectivity with the electrode, they have the effect of preventing short circuits in a direction different from that between the opposing electrodes, and at the same time, it can be expected that the conduction reliability will be improved.

[0053] The glass transition temperature can be measured by, for example, the following method.

[0054] Using a differential scanning calorimeter (e.g., "STAR SYSTEM" manufactured by METTLER TOLEDO), 0.04 to 0.06 g of a sample is heated to 200°C, and then cooled from this temperature to 25°C at a cooling rate of 5°C / min. Next, the sample is heated at a heating rate of 5°C / min, and the heat is measured. When a peak is observed, the temperature of the peak is taken as the glass transition temperature. When no peak is observed but a step difference is observed, the temperature at the intersection of the tangent line showing the maximum slope of the curve of the step difference portion and the extended line of the baseline on the high temperature side of the step difference is taken as the glass transition temperature.

[0055] In the present invention, “having no glass transition temperature” means that neither a peak nor a step difference is observed when differential scanning calorimetry is performed by the above-mentioned method.

[0056] As the insulating particles in the present invention, it is preferred that at least the surface layer thereof is composed of a polymer containing a cross-linking monomer component. By making the surface layer of the insulating particles a polymer containing a cross-linking monomer component, it is possible to obtain insulating particles that do not have a glass transition temperature and have a hardness that can withstand high temperatures during thermal compression. In addition, as the insulating particles in the present invention, it is preferred that the core material portion is formed by a polymer obtained by polymerizing a non-cross-linking monomer component. By making the core material portion of the insulating particles a polymer obtained by polymerizing a non-cross-linking monomer component, it is easy to obtain spherical insulating particles with uniform particle size. In addition, as long as the core material portion remains spherical, from the viewpoint of ensuring the strength of the insulating particles, it can be a polymer obtained by adding a cross-linking monomer component in any amount in addition to the non-cross-linking monomer component and polymerizing it. From the above, it can be seen that from the viewpoint of being able to obtain insulating microparticles having a sphericity range described below and having no glass transition temperature, it is particularly preferred that the insulating microparticles include: a spherical core portion formed by polymerizing a non-crosslinking monomer component, and a surface portion formed by a polymer containing a crosslinking monomer component, and have no glass transition temperature as a whole particle.

[0057] Examples of the crosslinkable monomer component constituting the insulating fine particles of the present invention include aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; allyl methacrylate, 1,3,5-triacryloylhexahydro-1,3,5-triazine (triacrylformal), triallyl isocyanate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate. A compound having two or more polymerizable ethylenically unsaturated bonds such as polyfunctional acrylate compounds such as esters, 1,6-hexanediol di(meth)acrylate, trimethylolpropane trimethacrylate, glycerol dimethacrylate, dimethylol-tricyclodecane diacrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, neopentyl glycol acrylate benzoate, trimethylolpropane acrylate benzoate, 2-hydroxy-3-acryloxypropyl methacrylate, hydroxypivalic acid neopentyl glycol diacrylate, di-trimethylolpropane tetraacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, etc. These can be used alone or in combination of two or more. When the insulating fine particles contain a plurality of crosslinking monomer components, the presence of the structural units of the crosslinking monomer components in the polymer may be random, alternating, or block as a copolymer.

[0058] In the present invention, the crosslinkable monomer component is preferably at least one selected from divinylbenzene, allyl methacrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate and 1,10-decanediol di(meth)acrylate. By having a polymer containing such a crosslinkable monomer component on at least the surface layer of the insulating fine particles, not only can the effect of preventing short circuits in a direction different from between the opposing electrodes be obtained, but also during thermal compression bonding, the insulating fine particles can be effectively removed without remaining between the conductive layer and the electrode.

[0059] In the polymer constituting the insulating fine particles according to the present invention, the amount of the crosslinking monomer component in all the structural units is preferably more than 20% by mass and less than 95% by mass, and more preferably more than 21% by mass and less than 80% by mass. By mixing the crosslinking monomer component within this range, insulating fine particles having no glass transition temperature and having a desired hardness during thermocompression bonding can be obtained.

[0060] The insulating particles in the present invention preferably further contain a compound including a functional group having a charge. As a result, the conductive particles of the coated particles of the present invention have high adhesion to the insulating particles. Therefore, the coated particles of the present invention are easy to exert the effect of preventing short circuits in a direction different from between the opposing electrodes, and it is expected that the insulation in this direction will be improved. In particular, it is preferred that the surface layer of the insulating particles is a polymer containing a monomer component including a functional group having a charge.

[0061] As the functional group having a charge, for example, onium functional groups such as phosphonium, ammonium, and coronium, or amino groups can be cited. Among these, from the viewpoint of improving the adhesion between the conductive particles and the insulating particles and forming coated particles having both insulating properties and conduction reliability at a high level, an ammonium group or a phosphonium group is preferred, and a phosphonium group is more preferred.

[0062] Preferred examples of the functional group having a charge include functional groups represented by the following general formula (1).

[0063]

[0064] (In the formula, X is a phosphorus atom, a nitrogen atom or a sulfur atom, and R may be the same or different and is a hydrogen atom, a linear, branched or cyclic alkyl group, or an aryl group. When X is a nitrogen atom or a phosphorus atom, n is 1, and when X is a sulfur atom, n is 0. * represents a valence bond.)

[0065] As the counter ion for the cationic group, for example, halide ions can be mentioned. Examples of halide ions include Cl - 、F -Br - ,I - .

[0066] In formula (1), examples of the straight-chain alkyl group represented by R include straight-chain alkyl groups having 1 to 20 carbon atoms, specifically, methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-pentadecyl, n-hexadecyl, n-heptadecyl, n-octadecyl, n-nonadecyl, and n-eicosyl groups.

[0067] In formula (1), examples of the branched alkyl group represented by R include branched alkyl groups having 3 to 8 carbon atoms, specifically isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, sec-pentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, ethylhexyl and the like.

[0068] In the formula (1), examples of the cyclic alkyl group represented by R include cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl and cyclooctadecyl.

[0069] In the formula (1), examples of the aryl group represented by R include phenyl, benzyl, tolyl, and o-xylyl.

[0070] In the general formula (1), from the viewpoint of improving the adhesion between the conductive particles and the insulating particles and from the viewpoint of easily ensuring conduction by detaching the insulating particles from the conductive particles when the anisotropic conductive film is thermally pressed inside, R is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, and most preferably an alkyl group having 1 to 8 carbon atoms. In addition, from the viewpoint of easily allowing the insulating particles to approach the conductive particles and adhere to them, R is also preferably a linear alkyl group.

[0071] Examples of the monomer component including a functional group having a charge include compounds including a functional group having a charge and having a polymerizable ethylenically unsaturated bond. Specifically, examples of the polymerizable compound having an onium functional group and having an ethylenically unsaturated bond include compounds having an ammonium group such as N,N-dimethylaminoethyl methacrylate, N,N-dimethylaminopropyl acrylamide, and N,N,N-trimethyl-N-2-methacryloyloxyethyl ammonium chloride; compounds having an onium group such as methacrylic acid phenyl dimethyl coronium methyl sulfate; 4-(vinylbenzyl)triethylphosphonium chloride, 4-(vinylbenzyl)trimethylphosphonium; Phosphonium chloride, 4-(vinylbenzyl)tributylphosphonium chloride, 4-(vinylbenzyl)trioctylphosphonium chloride, 4-(vinylbenzyl)triphenylphosphonium chloride, 2-(methacryloyloxyethyl)trimethylphosphonium chloride, 2-(methacryloyloxyethyl)triethylphosphonium chloride, 2-(methacryloyloxyethyl)tributylphosphonium chloride, 2-(methacryloyloxyethyl)trioctylphosphonium chloride, 2-(methacryloyloxyethyl)triphenylphosphonium chloride and the like; and the like.

[0072] In the present invention, the monomer component including a functional group having a charge is preferably at least one selected from the above-mentioned compound having an ammonium group and the above-mentioned compound having a phosphonium group. By having a polymer including such a monomer component having a functional group having a charge on at least the surface layer of the insulating particles, it is easy to improve the adhesion between the conductive particles and the insulating particles, or to arrange the insulating particles regularly, so that coated particles having both insulation and conduction reliability at a high level can be obtained.

[0073] In the polymer constituting the insulating fine particles according to the present invention, the proportion of the structural unit to which the functional group having a charge is bonded in all the structural units is preferably 0.01 mol% to 5.0 mol%, more preferably 0.02 mol% to 2.0 mol%. In addition, as one of the monomer components constituting the surface layer of the insulating fine particles, a monomer containing a functional group having a charge is preferably used.

[0074] The insulating fine particles of the present invention are at least a polymer containing a cross-linking monomer component in their surface layer, but the material constituting the portion other than the surface layer, such as the inside of the insulating fine particles, may be either an inorganic substance or an organic substance, and can be used without particular limitation. When an inorganic substance is used, metal particles such as gold, silver, copper, nickel, palladium, solder, alloys, glass, ceramics, silicon dioxide, metal or non-metal oxides (including hydrates), metal silicates including aluminosilicates, metal carbides, metal nitrides, metal carbonates, metal sulfates, metal phosphates, metal sulfides, metal acid salts, metal halides, and carbon, etc., can be cited. On the other hand, when using organic matter, thermoplastic resins, alkyd resins, phenolic resins, urea resins, benzoguanamine resins, melamine resins, xylene resins, silicone resins, epoxy resins, diallyl phthalate resins etc. such as natural fiber, natural resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polybutene, polyamide, polyacrylate, polyacrylonitrile, polyacetal, ionomer, polyester etc. can be enumerated. They can be used alone, and more than two kinds can be used in combination. Among these, from the viewpoint that the specific gravity of metal is little and difficult for sedimentation, dispersion stability is excellent, preferably formed by resin material.

[0075] As the above-mentioned resin material constituting the part other than the surface layer of the insulating fine particles, a polymer of a polymerizable compound having an ethylenically unsaturated bond is preferably used. As polymerizable compounds having an ethylenically unsaturated bond, styrenes, olefins, esters, α, β unsaturated carboxylic acids, amides, nitriles, etc. can be cited. As styrenes, core-substituted styrenes such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, dimethylstyrene, ethylstyrene, chlorostyrene, or styrene derivatives such as α-methylstyrene, α-chlorostyrene, β-chlorostyrene, etc. can be cited. As olefins, ethylene, propylene, etc. can be cited. As esters, vinyl esters such as vinyl acetate, vinyl propionate, and vinyl benzoate, and esters of (meth) acrylic acid such as methyl (meth) acrylate, ethyl (meth) acrylate, propyl (meth) acrylate, and phenyl (meth) acrylate can be cited. As α, β unsaturated carboxylic acids, acrylic acid, methacrylic acid, itaconic acid, maleic acid, etc. can be cited. Salts of these α, β unsaturated carboxylic acids are also included in α, β unsaturated carboxylic acids. As amides, acrylamide, methacrylamide, etc. can be cited. As nitriles, acetonitrile, etc. can be cited. They can also be substituted, and as substituents, phosphonium, amino, quaternary ammonium, amide, thiocyanate, sulfonic acid, mercapto, carboxyl, phosphoric acid, cyano, aldehyde, ester, carbonyl, etc. can be cited. These monomers can be used alone or in combination of two or more. In particular, polymers containing at least one non-crosslinking monomer component selected from styrenes, esters and nitriles are preferred in terms of high polymerization rate and easy spherical formation. When the polymer constituting the above-mentioned resin material has a variety of structural units, the presence of these structural units in the polymer can be either random, alternating, or block. The polymer constituting the resin material can be crosslinked or non-crosslinked. In the present invention, from the viewpoint of easily obtaining spherical insulating particles, the above-mentioned resin material constituting the part outside the surface layer, that is, the core material part, is preferably formed by a polymer polymerized from non-crosslinking monomer components.

[0076] The average particle size (D) of the insulating fine particles is preferably 10 nm to 3,000 nm, more preferably 15 nm to 2,000 nm. When the average particle size of the insulating fine particles is within the above range, the obtained coated particles can easily ensure conduction between the opposing electrodes without short-circuiting in a direction different from that between the opposing electrodes. In the present invention, the average particle size of the insulating fine particles is a value measured by observation using a scanning electron microscope, specifically, measured by the method described in the examples described later.

[0077] The particle size distribution of the insulating fine particles measured by the above method has a width. Generally, the width of the particle size distribution of a powder is represented by the coefficient of variation (hereinafter also referred to as "CV") shown in the following calculation formula (1).

[0078] CV (%) = (standard deviation / average particle size) × 100 (1)

[0079] When the CV is large, it means that the particle size distribution has a wide range, while when the CV is small, it means that the particle size distribution is sharp. The coated particles of this embodiment preferably use insulating particles with a CV of preferably 0.1% to 20%, more preferably 0.5% to 15%, and most preferably 1% to 10%. When the CV is within this range, there is an advantage that the thickness of the coating layer formed by the insulating particles can be made uniform.

[0080] The sphericity of the insulating particles is greater than 0.90. In the present invention, the sphericity refers to the value obtained by dividing the short diameter of the insulating particles by the long diameter. The sphericity is measured, for example, by using a scanning electron microscope at a measurement magnification of about 50 to 100 insulating particles contained in one field of view, and the arithmetic mean based on the number is calculated. The above-mentioned sphericity is preferably greater than 0.92, more preferably greater than 0.94, and even more preferably greater than 0.95. The upper limit of the above-mentioned sphericity is not particularly limited, and is generally about 0.99. By having the sphericity within this range, the insulating particles can be effectively excluded from between the conductive layer and the electrode during thermocompression bonding, and an improvement in conduction reliability can be expected.

[0081] Next, a preferred method for producing the coated particles according to the present embodiment will be described.

[0082] The production method comprises: a first step of polymerizing a non-crosslinking monomer component to obtain an insulating particle precursor;

[0083] A second step of polymerizing a polymerizable compound containing a crosslinkable monomer component in the presence of an insulating fine particle precursor to obtain insulating fine particles;

[0084] The third step is to mix the dispersion containing insulating fine particles and conductive particles to allow the insulating fine particles to adhere to the surfaces of the conductive particles.

[0085] (First process)

[0086] The insulating particle precursor involved in the manufacturing method of the present invention is a polymer obtained by polymerizing a non-crosslinking monomer component. As the above-mentioned non-crosslinking monomer component, a resin material constituting the portion other than the surface layer of the above-mentioned insulating particles and a polymerizable compound having an ethylenically unsaturated bond can be cited. In particular, the non-crosslinking monomer component is preferably selected from at least one of styrene, o-methylstyrene, m-methylstyrene or p-methylstyrene, dimethylstyrene, ethylstyrene, chlorostyrene, vinyl acetate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate and phenyl (meth)acrylate. In addition, when using a plurality of non-crosslinking monomer components, as a preferred constituent ratio of the polymerizable compound, a constituent ratio of a preferred structural unit or a preferred amount ratio of the polymer constituting the above-mentioned insulating particle precursor can be cited.

[0087] In the first step, a polymerizable compound containing a monomer component including a charged functional group in addition to a crosslinkable monomer component may be polymerized. Examples of the monomer component including a charged functional group include the monomer component including a charged functional group constituting the insulating fine particles.

[0088] As the polymerization method, emulsion polymerization, emulsifier-free emulsion polymerization, dispersion polymerization, suspension polymerization, etc. can be listed. Any polymerization method can be used. In the case of emulsifier-free emulsion polymerization, it is preferred because it has the advantage of being able to produce monodisperse particles without using a surfactant. In the case of emulsifier-free emulsion polymerization, a water-soluble initiator can be used as a polymerization initiator. The polymerization is preferably carried out under an inactive atmosphere such as nitrogen or argon.

[0089] From the viewpoint of obtaining insulating fine particle precursors that are true spherical particles with uniform particle diameters, the polymerization time is preferably from 0.3 hours to 20 hours, and particularly preferably from 0.5 hours to 12 hours.

[0090] Insulating fine particle precursors can be obtained in the above manner.

[0091] (Second process)

[0092] In the second step, in the presence of the insulating particle precursor obtained in the first step, a polymerizable compound containing a crosslinkable monomer component is polymerized to obtain insulating particles. As the above-mentioned crosslinkable monomer component, the crosslinkable monomer component constituting the above-mentioned insulating particles can be listed, and in particular, at least one selected from divinylbenzene, allyl methacrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate and 1,10-decanediol di(meth)acrylate is preferred. In addition, when using multiple crosslinkable monomer components, as a preferred constituent ratio of the polymerizable compound, a constituent ratio of a preferred structural unit or a preferred amount ratio of the polymer constituting the above-mentioned insulating particles can be listed.

[0093] In the second step, a polymerizable compound containing a monomer component including a charged functional group in addition to a crosslinkable monomer component may be polymerized. Examples of the monomer component including a charged functional group include the monomer component including a charged functional group constituting the insulating fine particles.

[0094] As the polymerization method, the same method as the first step can be cited, and emulsion polymerization, emulsifier-free emulsion polymerization, dispersion polymerization, suspension polymerization, etc. can be cited. In particular, when emulsifier-free emulsion polymerization is used, it has the advantage of being able to produce monodisperse particles without using a surfactant, so it is preferred. The polymerization is preferably carried out under an inactive atmosphere such as nitrogen or argon.

[0095] From the viewpoint of obtaining insulating fine particles having a true spherical shape and a uniform particle size, the polymerization time is preferably from 0.3 hours to 20 hours, and particularly preferably from 0.5 hours to 12 hours.

[0096] Insulating fine particles can be obtained in the above manner.

[0097] (Third process)

[0098] Next, the insulating fine particles and the conductive particles are mixed so that the insulating fine particles adhere to the surface of the conductive particles. The mixing of the insulating fine particles and the conductive particles is preferably carried out in a liquid medium. Examples of the liquid medium include water, organic solvents, and mixtures thereof, preferably water.

[0099] When insulating particles and conductive particles are mixed in a liquid medium, it is preferred that the dispersion containing these particles and the liquid medium contains an inorganic salt, an organic salt or an organic acid, which is preferred from the viewpoint of easily obtaining coated particles with a coverage ratio of a certain level or more. As the inorganic salt, organic salt or organic acid, a substance that can dissociate anions is preferably used, and as the anion, Cl - 、F -Br - ,I - 、SO4 2- 、CO3 2- 、NO3 - 、COO - ,RCOO - (R is an organic group) etc. As inorganic salts, for example, NaCl, KCl, LiCl, MgCl2, BaCl2, NaF, KF, LiF, MgF2, BaF2, NaBr, KBr, LiBr, MgBr2, BaBr2, NaI, KI, LiI, MgI2, BaI2, Na2SO4, K2SO4, Li2SO4, MgSO4, Na2CO3, NaHCO3, K2CO3, KHCO3, Li2CO3, LiHCO3, MgCO3, NaNO3, KNO3, LiNO3, Mg(NO3)2, Ba(NO3)2 etc. can be used. In addition, as organic salts, sodium succinate, sodium oxalate, sodium acetate, sodium citrate, sodium malonate, sodium tartrate, sodium fumarate, sodium maleate etc. can be used. As the organic acid, amino acids such as glycine, succinic acid, oxalic acid, acetic acid, citric acid, tartaric acid, malonic acid, fumaric acid, maleic acid, and the like can be used.

[0100] The concentration of the preferred inorganic salt, organic salt and organic acid varies depending on the extent of the coating area occupied by the insulating fine particles in the surface area of ​​the conductive particles. In the dispersion containing the insulating fine particles and the conductive particles, for example, a concentration of 5 mmol / L or more and 100 mmol / L or less is preferred because it is easy to obtain coated particles with a preferred coating rate and a single layer of insulating fine particles. From this viewpoint, the concentration of the inorganic salt, organic salt and organic acid in the dispersion is more preferably 7 mmol / L or more and 90 mmol / L or less, and particularly preferably 10 mmol / L or more and 80 mmol / L or less.

[0101] When the insulating fine particles and the conductive particles are mixed in the liquid medium, the dispersion containing the insulating fine particles and the conductive particles may be mixed, or the dispersion containing the conductive particles and the insulating fine particles may be mixed, or the insulating fine particles and the conductive particles may be added to the liquid medium separately, or the dispersion medium containing the insulating fine particles and the dispersion medium containing the conductive particles may be mixed. In the dispersion containing the conductive particles and the insulating fine particles, the conductive particles are preferably contained in an amount of 100 ppm to 100,000 ppm, more preferably 500 ppm to 80,000 ppm, based on mass.

[0102] In the dispersion containing the conductive particles and the insulating fine particles, the insulating fine particles are contained in an amount of preferably 10 ppm to 50,000 ppm, and more preferably 250 ppm to 30,000 ppm, based on mass.

[0103] From the viewpoint of easily obtaining coated particles of constant quality, the temperature of the dispersion containing the conductive particles and the insulating particles is generally preferably set to 20° C. to 100° C., and particularly preferably 40° C. to 90° C. Within this range, the insulating particles adhere closely to the conductive particles while maintaining their shape, and a suitable contact area between the insulating particles and the conductive particles is easily obtained.

[0104] In the dispersion after the conductive particles are mixed, the time required for the insulating particles to adhere to the conductive particles is preferably 0.1 hours to 24 hours. During this time, the dispersion is preferably stirred. Then, the solid content of the dispersion is washed and dried as needed to obtain coated particles in which the insulating particles are attached to the surface of the conductive particles.

[0105] The coated particles obtained as described above can be suitably used as conductive materials such as conductive adhesives, anisotropic conductive films, and anisotropic conductive adhesives by utilizing the insulation between coated particles and the connectivity between opposing electrodes brought about by the advantages of conductive particles and insulating fine particles having no glass transition temperature.

[0106] Example

[0107] The present invention will be described below using examples. However, the scope of the present invention is not limited to these examples. The properties in the examples were measured by the following methods.

[0108] (1) Average particle size

[0109] 200 particles are randomly selected from a scanning electron microscope (SEM) photograph (magnification 100,000 times) of the measurement object, and their particle diameters are measured, and the average value is defined as the average particle diameter. The average particle diameter is as described above.

[0110] (2) CV (coefficient of variation)

[0111] The average particle size was determined by the following formula from the above-mentioned measurement.

[0112] CV (%) = (standard deviation / average particle size) × 100

[0113] (3) Glass transition temperature

[0114] The calorific value change from the measurement temperature of 25° C. to 200° C. was measured in a nitrogen atmosphere at a temperature rise and fall rate of 5° C. / min according to the above-mentioned operation procedure using a differential scanning calorimeter (manufactured by METTLER TOLEDO, STAR SYSTEM).

[0115] (4) Sphericity

[0116] 200 particles were randomly selected from a scanning electron microscope (SEM) photograph (magnification 100,000 times) of the measurement object, their short diameter and long diameter were measured, and the value obtained by dividing the short diameter by the long diameter of each particle was obtained. The average value was used as the sphericity.

[0117] (Example 1)

[0118] [Manufacturing of Phosphonium-Based Insulating Fine Particles]

[0119] 1200 mL of pure water was added to a 2000 mL four-necked flask equipped with a stirring blade of 60 mm in length. Then, 288 mmol of styrene monomer (manufactured by Kanto Chemical Co., Ltd.), 63.6 mmol of n-butyl acrylate (manufactured by Kanto Chemical Co., Ltd.), and 5.0 mmol of 2,2'-azobis(2-methylpropionamidine) dihydrochloride (manufactured by Wako Pure Chemical Industries, Ltd., V-50) as a polymerization initiator were added. Nitrogen was passed through for 15 minutes to expel the dissolved oxygen, and then the temperature was raised to 65°C and maintained for 6 hours to carry out the polymerization reaction.

[0120] Then, 108 mmol of divinylbenzene monomer (manufactured by Nippon Steel & Sumitomo Metal Corporation) and 2.16 mmol of 4-(vinylbenzyl)triethylphosphonium chloride (manufactured by Nippon Chemical Industry Co., Ltd.) were added to the reaction system, and the temperature was maintained at 65° C. for 10 hours to terminate the reaction.

[0121] The dispersion of the polymerized microparticles was passed through a SUS sieve with a mesh size of 150 μm to remove agglomerates. The dispersion from which the agglomerates were removed was centrifuged at 20,000 rpm for 20 minutes using a centrifuge (CR-21N, manufactured by Hitachi Koki Co., Ltd.) to allow the microparticles to settle, and the supernatant was removed. Pure water was added to the obtained solid to wash it, to obtain spherical microparticles. The various properties of the obtained microparticles are shown in Table 1. The SEM photograph of the obtained insulating microparticles is shown in Figure 1 In addition, the results of measuring the glass transition temperature are shown in Figure 2 .

[0122] [Manufacturing of insulating fine particle-coated conductive particles]

[0123] Prepare Ni-plated particles (manufactured by Nippon Chemical Industry Co., Ltd.) having a nickel film with a thickness of 0.125 μm and an average particle size of 3 μm on the surface of spherical resin particles. The resin particles are composed of crosslinked acrylic resins with a glass transition temperature of 120°C. 100 mL of pure water is added to 5.0 g of the above-mentioned Ni-plated particles and stirred to obtain a dispersion of Ni-plated particles. 10 mL of an aqueous solution of 1% by mass of benzotriazole is added to the dispersion and stirred for 5 minutes for surface treatment. Then, filter with a membrane filter with a mesh size of 2.0 μm to recover Ni-plated particles having a benzotriazole layer on the surface. After washing the recovered Ni-plated particles with pure water, 100 mL of pure water is added to obtain a dispersion of Ni-plated particles having a benzotriazole layer on the surface. Add the insulating particles obtained above and Na2SO4 to the dispersion, and stir it at 40°C for 30 minutes. After adding insulating fine particles and Na2SO4, the solid content concentration of insulating fine particles in the dispersion was 10,000 ppm by mass, and the concentration of Na2SO4 was 5 mmol / L. After removing the supernatant, the dispersion was washed with pure water and then vacuum dried at 50°C to obtain conductive particles coated with insulating fine particles. The SEM photograph of the obtained coated particles is shown in Figure 3 .

[0124] (Example 2)

[0125] [Manufacturing of ammonium insulating fine particles]

[0126] 1200 mL of pure water was added to a 2000 mL four-necked flask equipped with a stirring blade of 60 mm in length. Then, 288 mmol of styrene monomer (manufactured by Kanto Chemical Co., Ltd.), 63.6 mmol of n-butyl acrylate (manufactured by Kanto Chemical Co., Ltd.), and 5.0 mmol of 2,2'-azobis(2-methylpropionamidine) dihydrochloride (manufactured by Wako Pure Chemical Industries, Ltd., V-50) as a polymerization initiator were added. Nitrogen was passed through for 15 minutes to expel the dissolved oxygen, and then the temperature was raised to 65°C and maintained for 6 hours to carry out the polymerization reaction.

[0127] Then, 108 mmol of divinylbenzene monomer (manufactured by Nippon Steel & Sumitomo Metal Corporation) and 2.0 mmol of 4-(vinylbenzyl)triethylammonium chloride (manufactured by Nippon Chemical Industry Co., Ltd.) were added to the reaction system, and the reaction was completed by maintaining the temperature at 65° C. for 10 hours.

[0128] The dispersion of the polymerized microparticles was passed through a SUS sieve with a mesh size of 150 μm to remove agglomerates. The dispersion from which the agglomerates were removed was centrifuged at 20,000 rpm for 20 minutes using a centrifuge (CR-21N, manufactured by Hitachi Koki Co., Ltd.) to allow the microparticles to settle, and the supernatant was removed. Pure water was added to the obtained solid to wash it, to obtain spherical microparticles. The various properties of the obtained microparticles are shown in Table 1. The SEM photograph of the obtained insulating microparticles is shown in Figure 4 In addition, the results of measuring the glass transition temperature are shown in Figure 5 .

[0129] [Manufacturing of insulating fine particle-coated conductive particles]

[0130] The same method as in Example 1 was carried out to obtain insulating fine particle-coated conductive particles.

[0131] (Comparative Example 1)

[0132] [Manufacturing of Phosphonium-Based Insulating Fine Particles]

[0133] 1200 mL of pure water was added to a 2000 mL four-necked flask equipped with a stirring blade of 60 mm in length. Then, 288 mmol of styrene monomer (manufactured by Kanto Chemical Co., Ltd.), 63.6 mmol of n-butyl acrylate (manufactured by Kanto Chemical Co., Ltd.), 108 mmol of divinylbenzene monomer (manufactured by Nippon Steel & Sumitomo Metal Corporation), 1.44 mmol of 4-(vinylbenzyl)triethylphosphonium chloride (manufactured by Nippon Chemical Industry Co., Ltd.), and 5.0 mmol of 2,2'-azobis(2-methylpropionamidine) dihydrochloride (manufactured by Wako Pure Chemical Industries, Ltd., V-50) as a polymerization initiator were added. Nitrogen was passed through for 15 minutes to discharge the dissolved oxygen, and then the temperature was raised to 65°C and maintained for 8 hours for polymerization reaction. The dispersion of the microparticles after polymerization was passed through a SUS sieve with a mesh size of 150 μm to remove the agglomerates. The dispersion after the agglomerates were removed was centrifuged at 20,000 rpm for 20 minutes using a centrifuge (CR-21N, manufactured by Hitachi Koki Co., Ltd.) to precipitate the particles and remove the supernatant. Pure water was added to the obtained solid to wash it, and spherical particles were obtained. The various properties of the obtained particles are shown in Table 1. The SEM photograph of the obtained insulating particles is shown in Figure 6 In addition, the results of measuring the glass transition temperature are shown in Figure 7 .

[0134] [Manufacturing of insulating fine particle-coated conductive particles]

[0135] Prepare Ni-plated particles (manufactured by Nippon Chemical Industry Co., Ltd.) having a nickel film with a thickness of 0.125 μm and an average particle size of 3 μm on the surface of spherical resin particles. The resin particles are composed of crosslinked acrylic resins with a glass transition temperature of 120°C. 100 mL of pure water is added to 5.0 g of the above-mentioned Ni-plated particles and stirred to obtain a dispersion of Ni-plated particles. 10 mL of an aqueous solution of 1% by mass of benzotriazole is added to the dispersion and stirred for 5 minutes for surface treatment. Then, filter with a membrane filter with a mesh size of 2.0 μm to recover Ni-plated particles having a benzotriazole layer on the surface. After washing the recovered Ni-plated particles with pure water, 100 mL of pure water is added to obtain a dispersion of Ni-plated particles having a benzotriazole layer on the surface. Add the insulating particles obtained above and Na2SO4 to the dispersion, and stir it at 40°C for 30 minutes. After adding insulating fine particles and Na2SO4, the solid content concentration of insulating fine particles in the dispersion was 10,000 ppm by mass and the concentration of Na2SO4 was 5 mmol / L. After removing the supernatant, the dispersion was washed with pure water and then vacuum dried at 50°C to obtain insulating fine particle-coated conductive particles.

[0136] (Comparative Example 2)

[0137] [Manufacturing of ammonium insulating fine particles]

[0138] 1200 mL of pure water was added to a 2000 mL four-necked flask equipped with a stirring blade of 60 mm in length. Then, 288 mmol of styrene monomer (manufactured by Kanto Chemical Co., Ltd.), 63.6 mmol of n-butyl acrylate (manufactured by Kanto Chemical Co., Ltd.), 108 mmol of divinylbenzene monomer (manufactured by Nippon Steel & Sumitomo Metal Corporation), 2.0 mmol of 4-(vinylbenzyl)triethylammonium chloride (manufactured by Nippon Chemical Industry Co., Ltd.), and 5.0 mmol of 2,2'-azobis(2-methylpropionamidine) dihydrochloride (manufactured by Wako Pure Chemical Industries, Ltd., V-50) as a polymerization initiator were added. Nitrogen was passed through for 15 minutes to discharge the dissolved oxygen, and then the temperature was raised to 65°C and maintained for 8 hours for polymerization reaction. The dispersion of the microparticles after polymerization was passed through a SUS sieve with a mesh size of 150 μm to remove agglomerates. The dispersion after the agglomerates were removed was centrifuged at 20,000 rpm for 20 minutes using a centrifuge (CR-21N, manufactured by Hitachi Koki Co., Ltd.) to precipitate the particles and remove the supernatant. Pure water was added to the obtained solid to wash it, and spherical particles were obtained. The various properties of the obtained particles are shown in Table 1. The SEM photograph of the obtained insulating particles is shown in Figure 8 In addition, the results of measuring the glass transition temperature are shown in Fig. 9 .

[0139] [Manufacturing of insulating fine particle-coated conductive particles]

[0140] Insulating fine particle-coated conductive particles were obtained in the same manner as in Comparative Example 1.

[0141] (Comparative Example 3)

[0142] [Manufacturing of Phosphonium-Based Insulating Fine Particles]

[0143] 1200 mL of pure water was added to a 2000 mL four-necked flask equipped with a stirring blade of 60 mm in length. Then, 360 mmol of styrene monomer (manufactured by Kanto Chemical Co., Ltd.), 63.6 mmol of n-butyl acrylate (manufactured by Kanto Chemical Co., Ltd.), 1.44 mmol of 4-(vinylbenzyl)triethylphosphonium chloride (manufactured by Nippon Chemical Industry Co., Ltd.), and 5.0 mmol of 2,2'-azobis(2-methylpropionamidine) dihydrochloride (manufactured by Wako Pure Chemical Industries, Ltd., V-50) as a polymerization initiator were added. Nitrogen was passed through for 15 minutes to discharge the dissolved oxygen, and then the temperature was raised to 65°C and maintained for 8 hours for polymerization reaction. The dispersion of the microparticles after polymerization was passed through a SUS sieve with a mesh size of 150 μm to remove the agglomerates. The dispersion after the agglomerates were removed was centrifuged at 20,000 rpm for 20 minutes using a centrifuge (CR-21N, manufactured by Hitachi Koki Co., Ltd.) to precipitate the particles and remove the supernatant. Pure water was added to the obtained solid to wash it, and spherical particles were obtained. The various properties of the obtained particles are shown in Table 1. The SEM photograph of the obtained insulating particles is shown in Fig.10 In addition, the results of measuring the glass transition temperature are shown in Fig.11 .

[0144] [Manufacturing of insulating fine particle-coated conductive particles]

[0145] Insulating fine particle-coated conductive particles were obtained in the same manner as in Comparative Example 1.

[0146] [Table 1]

[0147]

[0148] (Evaluation of conductivity and insulation)

[0149] <Evaluation of conductivity>

[0150] An insulating adhesive obtained by mixing 100 parts by mass of epoxy resin, 150 parts by mass of curing agent and 70 parts by mass of toluene is mixed with 15 parts by mass of coated particles obtained in the examples and comparative examples to obtain an insulating paste. The paste is applied to a silicone-treated polyester film using a rod coater, and then the paste is dried to form a thin film on the film. The obtained thin film-forming film is arranged between a glass substrate on which aluminum is vapor-deposited on the entire surface and a polyimide film substrate on which a copper pattern is formed at a spacing of 50 μm, and electrically connected. The conductivity of the coated particles is evaluated at room temperature (25°C·50% RH) by measuring the on-resistance between the substrates. The lower the resistance value, the higher the conductivity of the coated particles can be evaluated. In the conductivity evaluation of the coated particles, a resistance value of less than 2Ω was evaluated as "very good" (indicated by the symbol "○" in Table 2), a resistance value of 2Ω or more and less than 5Ω was evaluated as "good" (indicated by the symbol "△" in Table 2), and a resistance value of 5Ω or more was evaluated as "poor" (indicated by the symbol "×" in Table 2). The results are shown in Table 2.

[0151] <Evaluation of insulation properties>

[0152] Using a micro compression tester MCTM-500 (manufactured by Shimadzu Corporation), 20 coated particles were used as the object, and the coated particles of the embodiment and the comparative example were compressed under the condition of a load speed of 0.5 mN / second, and the compressive strain until the resistance value was detected was measured, thereby evaluating the insulation of the coated particles. The greater the compressive strain until the resistance value is detected, the higher the insulation of the coated particles can be evaluated. In the evaluation of the insulation of the coated particles, the case where the arithmetic mean of the compressive strain until the resistance value is detected is 10% or more is evaluated as "very good" (indicated by the symbol "○" in Table 2), the case where the arithmetic mean of the compressive strain exceeds 3% and is less than 10% is evaluated as "good" (indicated by the symbol "△" in Table 2), and the case where the arithmetic mean of the compressive strain is less than 3% is evaluated as "poor" (indicated by the symbol "×" in Table 2). The results are shown in Table 2.

[0153] [Table 2]

[0154] Continuity Insulation Example 1 ○ ○ Example 2 ○ ○ Comparative Example 1 × △ Comparative Example 2 × △ Comparative Example 3 △ ×

[0155] As shown in Table 2, it can be seen that the coated particles of the examples can maintain conductivity and have excellent insulation properties compared to the coated particles of the comparative examples.

[0156] Industrial Applicability

[0157] The coated particles of the present invention are coated with insulating fine particles having a spherical shape and a uniform particle size and having no glass transition temperature, and therefore can have high conduction reliability and insulation reliability.

Claims

1. A coated particle, characterized in that: The invention comprises conductive particles having a metal coating formed on the surface of a core material and insulating fine particles covering the conductive particles. The insulating fine particles are insulating fine particles that do not have a glass transition temperature and have a sphericity of 0.90 or more, The surface layer of the insulating fine particles is a polymer containing a cross-linkable monomer component.

2. The coated particles according to claim 1, characterized in that: The crosslinking monomer component is at least one selected from divinylbenzene, allyl methacrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate and 1,10-decanediol di(meth)acrylate.

3. The coated particles according to claim 1 or 2, characterized in that: The surface layer of the insulating fine particles is a polymer containing a monomer component having the following functional group, the functional group having a charge, and the functional group having a charge is a phosphonium group, an ammonium group, a coronium group, or an amino group.

4. The coated particles according to claim 3, characterized in that: The functional group is an ammonium group or a phosphonium group.

5. The coated particles according to claim 1 or 2, characterized in that: The coefficient of variation (CV) of the particle diameter of the insulating fine particles is 0.1% to 20%.

6. The coated particles according to claim 1 or 2, characterized in that: The metal film is a film composed of at least one selected from the group consisting of nickel, gold, a nickel alloy, and a gold alloy.

7. The coated particles according to claim 1 or 2, characterized in that: The conductive particles have a plurality of protrusions on the surface.

8. A conductive material, characterized in that: The invention comprises the coated particles according to claim 1 or 2 and an insulating resin.

9. A method for producing coated particles, characterized in that: The coated particles include conductive particles having a metal coating formed on the surface of a core material and insulating fine particles coating the conductive particles. The manufacturing method comprises: A first step of polymerizing a non-crosslinkable monomer component to obtain an insulating fine particle precursor; a second step of polymerizing a polymerizable compound containing a crosslinkable monomer component in the presence of an insulating fine particle precursor to obtain insulating fine particles; and The third step is to mix the dispersion containing insulating fine particles and conductive particles to allow the insulating fine particles to adhere to the surfaces of the conductive particles. The polymerization in the first step or the second step is performed using a polymerization method selected from emulsion polymerization, emulsifier-free emulsion polymerization, dispersion polymerization, and suspension polymerization, and the polymerization time is 0.3 hours to 20 hours.

10. The method for producing coated particles according to claim 9, wherein: The non-crosslinking monomer component is at least one selected from styrene, o-methylstyrene, m-methylstyrene or p-methylstyrene, dimethylstyrene, ethylstyrene, chlorostyrene, vinyl acetate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate and phenyl (meth)acrylate.

11. The method for producing coated particles according to claim 9 or 10, characterized in that: The crosslinking monomer component is at least one selected from divinylbenzene, allyl methacrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate and 1,10-decanediol di(meth)acrylate.

12. The method for producing coated particles according to claim 9 or 10, characterized in that: After the insulating fine particle precursor is obtained in 0.3 to 20 hours through the first step, the second step is performed.