Bismuth metal-doped carbon nitride catalyst and preparation method and application thereof
By preparing a bismuth metal-doped carbon nitride catalyst, the problems of low activity and poor stability of existing electrochemical CO2 reduction catalysts are solved, and high selectivity and high activity of CO2 reduction to formic acid are achieved.
Patent Information
- Application Number
- CN202211020268.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-24
AI Technical Summary
Existing electrochemical CO2 reduction catalysts have low activity, poor product selectivity and poor stability, making it difficult to meet the needs of industrial production.
Using a bismuth metal-doped carbon nitride catalyst, a catalyst with a porous nanosheet structure is prepared by calcining urea and bismuth sources under the protection of an inert gas and performing pickling treatment, which is used to electrocatalyze the reduction of CO2 to formic acid.
It improves the stability and catalytic activity of the catalyst, provides higher electrochemical reaction active sites and a richer reaction active surface area, and achieves high selectivity and efficient conversion of CO2 reduction products.
Smart Images

Figure CN115992365B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy materials and electrocatalysis, and more specifically, relates to a bismuth metal-doped carbon nitride catalyst and a preparation method and application thereof. Background Art
[0002] Fossil fuels such as oil, coal and natural gas have become the main energy sources for human and industrial activities. It is estimated that human CO2 emissions are 40 billion tons per year, and this trend is still growing. The rapid increase in atmospheric CO2 concentration has brought about a large number of environmental problems. At present, there are two main ways to reduce the concentration of atmospheric CO2. On the one hand, CO2 capture and storage, which has the disadvantages of high capture cost, low storage and utilization value, and the risk of leakage, which limits its large-scale application; on the other hand, CO2 conversion and utilization, converting CO2 into other products with high added value. Among them, electrocatalytic reduction of CO2 has the advantages of mild reaction conditions, simple process, simple device, no need for external hydrogen source, and combined with renewable energy as the driving force, it solves the problems of CO2 emissions and energy shortages, realizes the storage of electrical energy and carbon recycling, and is regarded as one of the most promising CO2 conversion and utilization technologies in the 21st century. Due to the high energy barrier of CO2 reduction reaction, it is difficult to occur under natural conditions, but if it is under the action of catalyst, CO2 can be reduced to valuable products. The main problems currently faced are the low selectivity and stability of the catalyst, so it is necessary to study a catalyst with high selectivity and good stability.
[0003] Among the many reduction products of CO2, formic acid can be directly used in industrial production with high economic benefits. The prior art found that Sn and Sn-based catalysts have high catalytic activity and selectivity for the electrochemical reduction of carbon dioxide to produce formic acid. For example, Chinese patent application CN103715436A discloses a tin dioxide catalyst with a nanoflower structure, which improves the specific surface area of the catalyst, increases the electrochemical catalytic activity of the catalyst, effectively inhibits the hydrogen evolution reaction, and enhances the selectivity of the product formic acid. However, the tin dioxide nanocatalyst has poor stability and is not corrosion-resistant, and cannot meet the needs of long-term use.
[0004] Therefore, there is an urgent need to provide a highly selective, highly active and highly stable catalyst for the electrocatalytic production of formic acid from CO2. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing electrochemical reduction of CO2 catalysts, such as low activity, poor product selectivity and poor stability, and to provide a method for preparing a bismuth metal-doped carbon nitride catalyst.
[0006] The purpose of the present invention is to provide a bismuth metal-doped carbon nitride catalyst.
[0007] Another object of the present invention is to provide an application of a bismuth metal-doped carbon nitride catalyst.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] Carbon nitride materials are generally considered to be a promising new material due to their simple preparation route, easy large-scale production, good chemical stability, thermal stability and mechanical stability, and easy modification. However, as a type of semiconductor material, carbon nitride itself is often limited in its performance in electrocatalytic reactions. Modifying it with metals is an effective way to improve its catalytic performance, but metal nitrogen-doped carbon materials are prone to agglomeration and sintering of nanoparticles during the preparation and reaction process, resulting in a decrease in catalytic performance.
[0010] In order to solve the above problems, the present invention is implemented by the following technical solutions:
[0011] A method for preparing a bismuth metal-doped carbon nitride catalyst comprises the following steps:
[0012] S1. dispersing urea and bismuth source in water, mixing thoroughly, and freeze-drying to obtain a precursor;
[0013] S2. The precursor obtained in step S1 is calcined at 500-1000° C. under the protection of an inert gas, and a solid product is obtained after cooling. The solid product is acid-washed and post-treated to obtain a bismuth metal-doped carbon nitride catalyst powder.
[0014] Preferably, in step S1, the bismuth source is one or more of bismuth nitrate pentahydrate and bismuth chloride.
[0015] Preferably, in step S1, the mass ratio of urea to bismuth source is 1.0:(0.025-0.5).
[0016] More preferably, in step S1, the mass ratio of urea to bismuth source is 1.0:(0.05-0.2).
[0017] Most preferably, in step S1, the mass ratio of urea to bismuth source is 1.0:0.15.
[0018] Preferably, the freeze-drying conditions in step S1 are: temperature of -10 to -60°C, and drying time of 12 to 48 hours.
[0019] Preferably, in step S2, the calcination temperature is 550-1000°C.
[0020] Furthermore, in step S2, the heating rate of the calcination is 2-10°C / min.
[0021] Furthermore, in step S2, the calcination time is 1 to 4 hours.
[0022] Preferably, in step S2, the inert gas is one or more of nitrogen and argon.
[0023] Preferably, in step S2, the flow rate of the inert gas is 40.0 to 100.0 mL / min.
[0024] Specifically, in step S2, the material is ground before pickling, and then dried and ground again after pickling.
[0025] Furthermore, the acid washing condition is: the solid product obtained in step S2 is first washed with an acidic solution, and then washed with water until the solution is neutral.
[0026] Preferably, the acidic solution is a nitric acid solution.
[0027] More preferably, the molar concentration of the nitric acid solution is 0.5M.
[0028] Preferably, the drying method is vacuum drying.
[0029] Preferably, the vacuum drying temperature is 50-100° C., and the drying time is 12-48 hours.
[0030] More preferably, the vacuum drying temperature is 60° C. and the drying time is 24 h.
[0031] The bismuth metal-doped carbon nitride catalyst is obtained by the preparation method.
[0032] Furthermore, the bismuth metal-doped carbon nitride catalyst has a porous nanosheet structure.
[0033] Furthermore, the bismuth metal-doped carbon nitride catalyst consists of two parts: bismuth metal and carbon nitride, with the former being supported on the latter.
[0034] In addition, the present invention also provides an application of a bismuth metal-doped carbon nitride catalyst in electrocatalytic CO2 reduction to produce formic acid.
[0035] Specifically, the application method comprises the following steps:
[0036] A gas diffusion electrode system is used, with 0.5M-1.0M KOH as the electrolyte, Ar is first introduced to exclude air and then CO2 is introduced, the flow rate of which is 10.0-30.0mL / min, and the bismuth metal-doped carbon nitride catalyst prepared by the present invention is configured into ink and then coated on a glassy carbon electrode or carbon paper as a working electrode. Specifically, 1.0-20.0mg of bismuth metal-doped carbon nitride catalyst, 100-1000μL of anhydrous ethanol (95%), and 10-100uL of 5wt% perfluorosulfonic acid-polytetrafluoroethylene copolymer solution are taken, and after being mixed evenly by ultrasonic treatment, ink is obtained, and the obtained ink is brushed / dripped on a carbon paper / glassy carbon electrode, and dried at room temperature to obtain a cathode working electrode. Among them, the loading of the bismuth metal-doped carbon nitride catalyst on the paper / glassy carbon electrode is 0.01-5.0mg / cm 2 The reference electrode was set to Ag / AgCl electrode and the counter electrode was set to platinum wire for electrochemical performance testing. The test potential range was -0.6V to -1.0V relative to the standard hydrogen electrode, and CO2 was electrocatalytically reduced. The electrochemical performance of the catalyst was tested and analyzed by an electrochemical workstation; the gas phase product of the electroreduction of CO2 was analyzed by gas chromatography; the liquid product of the electrocatalytic CO2 reduction reaction was tested and analyzed by a Bruker 400MHz superconducting nuclear magnetic resonance instrument; the morphological characteristics of the catalyst were photographed by a HT7700 transmission electron microscope.
[0037] Preferably, the molar concentration of the electrolyte is 1M.
[0038] The present invention has the following beneficial effects:
[0039] 1. Compared with conventional metal-doped catalysts, the bismuth metal-doped carbon nitride catalyst prepared in the present invention has a porous sheet structure, thereby having more catalyst active sites and higher stability.
[0040] 2. The freeze-drying method improves the dispersion of bismuth metal nanoparticles on the carbon nitride carrier, providing a larger electrochemical reaction active surface area and more abundant reaction active sites, thereby giving the bismuth metal-doped carbon nitride catalyst a higher catalytic activity.
[0041] 3. The bismuth metal-doped carbon nitride catalyst prepared by the present invention can achieve fine control of its micromorphology, chemical composition, etc., has simple operation steps, a green and environmentally friendly process, and is easy to mass produce. It is not limited to the electrocatalytic reduction of CO2, but has broad application prospects in other electrocatalytic reduction fields or photocatalytic fields, such as in the field of photocatalytic CO2 reduction. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 12 are transmission electron micrographs of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 4; a to d correspond to the transmission electron micrographs of Examples 1 to 4, respectively;
[0043] Figure 2 The scanning electron microscope image (left half) and spherical aberration electron microscope image (right half) of the bismuth metal-doped carbon nitride catalyst prepared in Example 4;
[0044] Figure 3 is an elemental analysis diagram of the bismuth metal-doped carbon nitride catalyst prepared in Example 4;
[0045] Figure 4 is the XRD pattern of the bismuth metal-doped carbon nitride catalyst prepared in Examples 1 to 5;
[0046] Figure 5 This is the infrared absorption spectrum of the bismuth metal-doped carbon nitride catalyst prepared in Examples 1 to 5;
[0047] Figure 6 is an X-ray photoelectron spectroscopy (XPS) graph of the bismuth metal-doped carbon nitride catalyst prepared in Example 4;
[0048] Figure 7 is a curve diagram showing the change of current density during electrolysis of the bismuth metal-doped carbon nitride catalyst prepared in Example 4 as a function of electrolysis time;
[0049] Figure 8 The linear sweep cyclic voltammetry (LSV) curves of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 4;
[0050] Fig. 9 The electrochemical impedance spectroscopy (EIS) diagram of the bismuth metal-doped carbon nitride catalyst prepared in Examples 1 to 4;
[0051] Fig.10 The NMR spectra of the electrocatalytic CO2 products of the bismuth metal-doped carbon nitride catalysts prepared in Examples 2 to 5;
[0052] Fig.11 This is a bar graph of the Faraday efficiency of the electrocatalytic CO2 reduction products of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 5. DETAILED DESCRIPTION
[0053] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0054] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0055] Example 1 Preparation of a Bismuth Metal-Doped Carbon Nitride Catalyst
[0056] A preparation method of a bismuth metal-doped carbon nitride catalyst comprises the following steps:
[0057] S1. 2 g of urea and 0.05 g of bismuth nitrate pentahydrate were dispersed in 10 mL of deionized water, and after sufficient stirring, the mixed solution was freeze-dried to obtain a precursor;
[0058] S2. Place the precursor in a corundum porcelain boat, heat it from room temperature to pyrolysis temperature at a heating rate of 3°C / min under the protection of inert gas nitrogen, calcine it at 550°C for 2h, and obtain a solid product after natural cooling;
[0059] S3. The solid product was ground into uniform fine powder using a mortar, 40 mL of 0.5 M nitric acid was added and stirred at room temperature for 10 h, centrifuged, washed with ultrapure water for 4 to 5 times until the solution was neutral, then dried at 60 ° C in a vacuum drying oven for 24 h, and ground again to obtain a bismuth metal-doped carbon nitride catalyst Bi-0.05-gCN.
[0060] Examples 2-5 Preparation of a Bismuth Metal-Doped Carbon Nitride Catalyst
[0061] The difference between Example 2 and Example 1 is that the weighed bismuth nitrate pentahydrate is 0.1 g, that is, the mass ratio of urea to bismuth nitrate pentahydrate is 2:0.1, and a bismuth metal-doped carbon nitride catalyst Bi-0.1-gCN is obtained.
[0062] The difference between Example 3 and Example 1 is that the weighed bismuth nitrate pentahydrate is 0.2 g, that is, the mass ratio of urea to bismuth nitrate pentahydrate is 2:0.2, and a bismuth metal-doped carbon nitride catalyst Bi-0.2-gCN is obtained.
[0063] The difference between Example 4 and Example 1 is that the weighed bismuth nitrate pentahydrate is 0.3 g, that is, the mass ratio of urea to bismuth nitrate pentahydrate is 2:0.3, and a bismuth metal-doped carbon nitride catalyst Bi-0.3-gCN is obtained.
[0064] The difference between Example 5 and Example 1 is that the weighed bismuth nitrate pentahydrate is 0.4 g, that is, the mass ratio of urea to bismuth nitrate pentahydrate is 2:0.4, and a bismuth metal-doped carbon nitride catalyst Bi-0.4-gCN is obtained.
[0065] Other parameters and operations are referred to Example 1.
[0066] Comparative Examples 1 to 4 Preparation of Bismuth Metal-Doped Carbon Nitride Catalyst
[0067] The difference between Comparative Example 1 and Example 4 is that nitric acid is not added for pickling, and the bismuth metal-doped carbon nitride catalyst is directly ground to obtain the catalyst.
[0068] The difference between Comparative Example 2 and Example 4 is that the calcination temperature is 500°C.
[0069] The difference between Comparative Example 3 and Example 4 is that the weighed bismuth nitrate pentahydrate is 2 g, that is, the mass ratio of urea to bismuth nitrate pentahydrate is 1:1.
[0070] The difference between Comparative Example 4 and Example 4 is that a vacuum desiccant is used for drying instead of a freeze dryer.
[0071] Other parameters and operations are referred to Example 1.
[0072] Experimental example
[0073] 1. Physical characterization and composition analysis of bismuth metal-doped carbon nitride catalyst
[0074] The transmission electron microscopy images of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 4 were measured, and the results were as follows: Figure 1 As shown in (a), (b), (c), and (d), it can be observed that the bismuth metal-doped carbon nitride catalyst has a porous sheet structure;
[0075] The scanning electron microscope image of the bismuth metal-doped carbon nitride catalyst prepared in Example 4 was measured, and the results were as follows: Figure 2 As shown in the left half of the figure, the three-dimensional multilayer stacking morphology of the surface of the bismuth metal-doped carbon nitride catalyst powder can be seen;
[0076] The spherical aberration electron microscopy image of the bismuth metal-doped carbon nitride catalyst prepared in Example 4 was measured, and the results were as follows: Figure 2 As shown in the right half of the figure, it can be seen that the Bi atoms are highly evenly dispersed, and the individual bright spots are the dispersed Bi atoms;
[0077] The elemental analysis of the bismuth metal-doped carbon nitride catalyst prepared in Example 4 was measured, and the results were as follows: Figure 3 As shown, it can be observed that C, N, O and Bi elements are uniformly distributed in the catalyst;
[0078] The XRD patterns of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 5 were measured, and the results were as follows: Figure 4 As shown, it can be seen that the 2θ values of 13.1° and 27.3° correspond to the (100) crystal plane and (002) crystal plane of graphite phase carbon nitride, respectively;
[0079] The infrared absorption spectra of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 5 were measured, and the results were as follows: Figure 5 As shown, we can see that we can observe 3000cm-1 To 3500cm -1 The broad peak at 2180cm -1 The single peak that appears should correspond to the asymmetric stretching vibration of the N≡C group, 1200cm -1 and 1700cm -1 The characteristic stretching mode between the CN heterocycles also exists at 890 cm -1 The characteristic vibration peak confirms the NH bond, 810cm -1 The absorption bands are assigned to the breathing mode of the heptazine ring system. These results indicate that the absorption peaks of -NH2 and -NH weaken with increasing Bi content, the absorption peak of N≡C increases, and the nitrogen defect points in the carbon nitride gC3N4 framework increase;
[0080] The X-ray photoelectron spectrum of the bismuth metal-doped carbon nitride catalyst prepared in Example 4 was measured, and the results were as follows: Figure 6 As shown in the figure, it can be seen that Bi 4f can be attributed to two obvious peaks, which are 159.5eV and 164.7eV, corresponding to Bi 3+ There are two less obvious peaks, 157.7eV and 163.3eV corresponding to Bi 0 The binding energy of C 1s spectrum is 287.9eV, which is sp2 hybridized carbon (NC=N) bound to nitrogen, while the peak at 284.5eV corresponds to graphitic carbon (CC). The N1s spectrum can be decomposed into four peaks, namely pyridinic N at 398.4eV, pyrrolic N at 399.8eV, graphitized N at 401.2eV, and oxidized N at 404.8eV.
[0081] 2. Performance test of bismuth metal-doped carbon nitride catalyst
[0082] A gas diffusion electrode system was used, with Ag / AgCl as reference electrode and platinum wire as counter electrode, and the bismuth metal-doped carbon nitride catalyst obtained in the present invention was made into a working electrode, wherein the loading of the catalyst prepared in the present invention on the carbon cloth electrode was 0.025 mg / cm 2 , the electrolyte is 1M KOH, the CO2 flow rate is 20cm 3 / min, room temperature, and loading voltages of -0.6V, -0.7V, -0.8V, -0.9V and -1.0V respectively. Electrochemical tests were carried out. The results are shown in Tables 1 and 2.
[0083] Table 1 Faradaic efficiency of formic acid in Examples 1 to 5
[0084]
[0085] Table 2 Faraday efficiency of formic acid in comparative examples 1 to 4
[0086]
[0087] As can be seen from Table 1, the Faraday efficiency of the electrolysis product formic acid of the bismuth metal-doped carbon nitride catalyst prepared in the above Examples 1 to 5 at an applied voltage of -1.0 is poor, which is significantly lower than the yield at a lower applied voltage of -0.6V under the same conditions. It can be seen that the selectivity of carbon dioxide reduction to formic acid is higher at a lower applied voltage.
[0088] The current density of the bismuth metal-doped carbon nitride catalyst prepared in Example 4 was measured as a function of electrolysis time. The results are as follows: Figure 7 As shown, it can be seen that the catalyst exhibits a relatively stable current density when electrolyzed at different potentials for one hour;
[0089] The linear scanning cyclic voltammetry curves of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 4 were measured, and the results were as follows: Figure 8 As shown, it can be seen that in the CO2-saturated 0.5M KHCO3 electrolyte, the Faraday onset potentials of the CO2 reduction reaction of Bi-0.3-gCN, Bi-0.2-gCN, Bi-0.1-gCN and Bi-0.05-gCN electrodes are -0.4, -0.8, -0.75 and 0.7 V vs. RHE, respectively;
[0090] The electrochemical impedance spectroscopy (EIS) spectra of the bismuth metal-doped carbon nitride catalysts prepared in Examples 1 to 4 were measured, and the results were as follows: Fig. 9 As shown, for Bi-0.05-gCN, Bi-0.1-gCN, Bi-0.2-gCN and Bi-0.3-gCN, the fitted impedances are 59, 77, 90 and 25Ω, respectively. The EIS graph shows that the charge transfer resistance of Bi-0.3-gCN is the smallest, and the charge transfer process in CO2-saturated KHCO3 solution is faster, indicating a more active electrochemical reaction;
[0091] The H NMR spectra of the electrolytic liquid products of the bismuth metal-doped carbon nitride catalysts prepared in Examples 2 to 5 were measured, and the results were as follows: Fig.10 As shown, it can be seen that deuterated water is used as the solvent, the internal standard is dimethyl sulfoxide (DMSO) with a peak position of about 2.6 ppm, and the main product formic acid has a peak position of about 8.4 ppm;
[0092] The Faraday efficiency bar graph of the product of electrocatalytic CO2 reduction of the bismuth metal-doped carbon nitride catalyst prepared in Example 4 was measured, and the results were as follows: Fig.11 As shown, it can be seen that the catalyst exhibits excellent catalytic activity and selectivity for electroreduction of CO2 at a relatively low potential of -0.6V, and can be used as an electrode material for electrocatalytic CO2 reduction reaction. Its electrochemical test performance shows that the formic acid yield can reach up to more than 95%;
[0093] The following conclusions can be drawn from Table 2:
[0094] As shown in the results of the Faraday efficiency of formic acid in Comparative Example 1, when nitric acid pickling is not used, the catalytic performance of the obtained catalyst is obviously inferior to that of the catalyst prepared in Example 4. The purpose of pickling is to remove impurities. Without pickling, it is impossible to obtain an ideal morphology and catalytic active sites.
[0095] As shown in the results of the Faraday efficiency of formic acid in Comparative Example 2, when the calcination temperature is lower than 550°C, the active sites of the catalyst are insufficient, and the catalytic performance is significantly reduced compared with the catalyst obtained in Example 4. This is because a catalyst having a highly dispersed bismuth metal-doped graphite phase carbon nitride gC3N4 structure cannot be successfully prepared at this temperature;
[0096] As shown in the results of the Faraday efficiency of formic acid in Comparative Example 3, when the amount of metal salt added is excessive, the catalytic performance is significantly reduced compared with the catalyst obtained in Example 4. This is because the excessive bismuth metal nanoparticles are prone to agglomeration;
[0097] As shown in the results of the Faraday efficiency of formic acid in Comparative Example 4, when the precursor is not dried by freeze-drying, the catalytic performance is greatly reduced compared with the catalyst obtained in Example 4. This is because the bismuth source is easily hydrolyzed to form a basic salt precipitate when not dried by freeze-drying, and a highly dispersed metal-doped catalyst cannot be formed.
[0098] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a bismuth metal-doped carbon nitride catalyst, characterized in that: The following steps are involved: S1. dispersing urea and a bismuth source in water, mixing thoroughly, and freeze-drying to obtain a precursor; S2. The precursor obtained in step S1 is calcined at 550-1000° C. under the protection of an inert gas, and a solid product is obtained after cooling, and the solid product is ground, acid-washed, and then washed with water until the solution is neutral, dried, and ground again to obtain a bismuth metal-doped carbon nitride catalyst; The pickling step is to add 0.5M nitric acid and stir for 10 hours at room temperature; In step S1, the bismuth source is one or more of bismuth nitrate pentahydrate and bismuth chloride; In step S1, the mass ratio of urea to bismuth source is 1.0: (0.025-0.5); In step S1, the freeze-drying conditions are: temperature of -10 to -60°C, and drying time of 12 to 48 hours.
2. The preparation method according to claim 1, characterized in that: In step S2, the heating rate of the calcination is 2-10°C / min.
3. The preparation method according to claim 1, characterized in that: In step S2, the calcination time is 1 to 4 hours.
4. The bismuth metal-doped carbon nitride catalyst obtained by the preparation method according to any one of claims 1 to 3.
5. The bismuth metal-doped carbon nitride catalyst according to claim 4, characterized in that: The bismuth metal-doped carbon nitride catalyst has a porous nanosheet structure.
6. Use of the bismuth metal-doped carbon nitride catalyst according to claim 4 or 5 in electrocatalysis of CO2.
7. The use according to claim 6, characterized in that: The specific method of electrocatalyzing CO2 comprises the following steps: A gas diffusion electrode system is adopted, 0.5M~1.0M KOH is used as the electrolyte, CO2 is introduced at a flow rate of 10.0~30.0mL / min, the bismuth metal-doped carbon nitride catalyst described in claim 4 or 5 is configured into ink and then coated on a glassy carbon electrode or carbon paper as a working electrode, the reference electrode is a saturated silver chloride electrode or a mercury / mercury oxide electrode, the counter electrode is a platinum wire or a carbon rod, a voltage is applied, and CO2 is electrocatalytically reduced.