A method for catalytically producing hydrogen and enriching carbon dioxide
The method catalytically produces hydrogen and enriches CO2 by regenerating deactivated catalysts in a fluidized reactor, improving hydrogen yield and facilitating CO2 capture, addressing efficiency and environmental issues in hydrogen production.
Patent Information
- Application Number
- CN202111229727.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-22
AI Technical Summary
Existing hydrogen production methods, particularly from fossil fuels, face challenges in efficiency, environmental impact, and the inability to meet growing demand, especially from refinery by-products, while CO2 emissions and capture are critical issues.
A method involving catalytic decomposition of hydrocarbon raw materials in a fluidized reactor, followed by high-temperature gasification of deactivated catalysts to regenerate and recycle catalysts, producing hydrogen and enriching CO2, using a catalyst composition of natural minerals, oxides, and metal active components.
Enhances hydrogen yield, reduces energy consumption, and facilitates CO2 capture and utilization, optimizing resource use and addressing environmental concerns.
Smart Images

Figure CN116004275B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing hydrogen and enriching carbon dioxide. Background Art
[0002] Hydrogen energy is an ideal new energy source. As a green energy with abundant reserves, high calorific value, high energy density and diverse sources, hydrogen energy is known as the "ultimate energy" of the 21st century. Hydrogen is produced through clean energy such as wind and light, and hydrogen is combined with fuel cells to generate electricity, thus forming a hydrogen energy industry ecosystem, which will help accelerate the construction of a clean and low-carbon hydrogen energy supply system.
[0003] There are three relatively mature technical routes for the main hydrogen production methods, namely, the use of fossil energy such as coal and natural gas to reform hydrogen, the high-temperature decomposition and reforming of chemical raw materials represented by alcohol cracking hydrogen production technology, and the electrolysis of water to produce hydrogen. Technical routes such as photolysis of water and biomass gasification to produce hydrogen are still in the experimental and development stage. It is difficult to make breakthroughs in related technologies and has not yet met the needs of large-scale hydrogen production. At present, domestic natural gas reforming hydrogen production and high-temperature cracking hydrogen production are mainly used in large-scale hydrogen production industry. The raw gas in the natural gas hydrogen production process is also fuel gas and does not need to be transported, but the investment in natural gas hydrogen production is relatively high and is suitable for large-scale industrial production. The general hydrogen production scale is 5000m 3 / h or more, it is more economical to choose the natural gas hydrogen production process. In addition, natural gas raw materials account for more than 70% of the cost of hydrogen production, and the price of natural gas is an important factor in determining the price of hydrogen. Coal gasification hydrogen production is the first choice for large-scale industrial hydrogen production, and it is also the mainstream fossil energy hydrogen production method in my country. This hydrogen production process converts coal into synthesis gas (CO, CH4, H2, CO2, N2, etc.) through gasification technology, and then separates and treats it through water-gas shift to extract high-purity hydrogen. It is the raw material for preparing synthetic ammonia, methanol, liquid fuel, natural gas and other products, and is widely used in petrochemical, steel and other fields. The coal-to-hydrogen technology route is mature and efficient, and can be produced on a large scale and stably, but the fuel power energy consumption of coal-to-hydrogen is higher than that of natural gas-to-hydrogen, and the system steam and electricity requirements are high, and enterprises need matching boilers. In addition, environmental protection issues are prominent, the existing urban refineries have harsh environmental requirements, and coal transportation is subject to many factors, which also limits the application of this technology in modern refineries.
[0004] With the development of oil refining technology, especially the trend of heavy / low-quality crude oil and the improvement of oil product quality, the hydrogenation process has been more widely used, which has greatly promoted the demand for hydrogen. According to statistics, the annual growth rate of global refinery hydrogen demand exceeds 4%. Hydrogen from refineries mainly comes from process unit by-products, refinery gas recovery, and existing refinery hydrogen production units. Refinery self-produced hydrogen will be difficult to meet the future growth demand for hydrogen. Therefore, it is necessary to explore more flexible and feasible hydrogen supply strategies. It is an inevitable trend for oil refining enterprises to transform from "fuel type" to "chemical type". For oil refining enterprises, it is necessary to significantly reduce the yield of oil products, especially the poor quality gasoline and diesel produced by some secondary processing units. For example, catalytic cracking diesel has always been relatively poor, with high density, high aromatic content and low cetane number. The existing utilization method is to first perform hydrogenation and then catalytic cracking to produce high-octane gasoline. As the demand for gasoline slows down, the outlet of catalytic cracking diesel has become a difficult problem faced by refineries. If these low-quality and low-value distillate oils can be converted into hydrogen energy, it will undoubtedly have good economic and social benefits. However, hydrogen production from hydrocarbon raw materials is a decarbonization process. In order to meet the needs of hydrogen production, low-hydrogen coke is not only inevitable, but also charcoal burning will bring CO2 emissions. Therefore, compared with emission reduction, CO2 capture is the key to the problem. Summary of the invention
[0005] The object of the present invention is to provide a method for catalytically producing hydrogen and enriching carbon dioxide.
[0006] The method for catalytically producing hydrogen and enriching carbon dioxide from hydrocarbon raw materials provided by the present invention comprises the following steps:
[0007] After the hydrocarbon raw material is mixed with water vapor, it is introduced into a fluidized reactor to contact with the regenerated catalyst and undergo a catalytic decomposition reaction to obtain a reactant stream and a deactivated catalyst with carbon, and the reaction oil gas obtained by the catalytic cracking reaction and the deactivated catalyst are separated into gas and solid;
[0008] The separated reaction oil and gas enters the separation unit for further separation into products including hydrogen, carbon monoxide, carbon dioxide, methane and other hydrocarbons;
[0009] The obtained deactivated catalyst is sent to the regenerator, contacted with oxygen-containing gas and water vapor for high-temperature gasification and regeneration. After regeneration, the deactivated catalyst is returned to the fluidized bed reactor for recycling; the regenerated flue gas is sent to the separation unit to obtain carbon monoxide and carbon dioxide.
[0010] Preferably, the other hydrocarbon products are returned to the reactor as feedstock for further conversion.
[0011] The catalyst comprises the following components by weight percentage: 15% to 65% of natural minerals, 20% to 60% of oxides, and 5% to 30% of metal active components. The metal active components are selected from one or more compounds of transition metal elements.
[0012] The present invention adopts a fluidized reactor to produce hydrogen, and the catalyst circulates between the reactor and the regenerator, which not only achieves the regeneration of the deactivated catalyst, but also transfers a large amount of heat for the reaction, greatly reducing the energy required for the hydrogen production process and achieving process economy.
[0013] The present invention uses hydrocarbon raw materials as raw materials, which not only reduces the raw material cost of natural gas hydrogen production, but also helps to ease the tight supply situation in my country's natural gas market, which is of strategic significance to the stable development of my country's energy structure.
[0014] The present invention uses high-temperature gasification technology to regenerate the deactivated catalyst with carbon, which not only restores the catalyst activity, but also produces CO and H2, further improving the hydrogen production, and also provides high-quality and cheap raw gas for the water-gas shift process, achieving optimal utilization of resources. At the same time, it greatly increases the concentration of CO2 in the flue gas, achieves CO2 enrichment, and can reduce carbon emissions through capture, utilization, and storage technology.
[0015] The present invention uses fluidized bed technology to convert hydrocarbon raw materials into hydrogen and enrich CO2 resources, with a high hydrogen yield. The present invention not only realizes the high-value utilization of low-value hydrocarbon raw materials, but also enriches the CO2 generated in the process, which not only brings hydrogen energy, but also facilitates carbon capture, and can bring greater economic and social benefits to the petrochemical industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A process flow chart of a specific implementation method of producing hydrogen and enriching CO2 from hydrocarbon raw materials provided by the present invention. DETAILED DESCRIPTION
[0017] A method for catalytically producing hydrogen from hydrocarbon feedstock while simultaneously enriching CO2, the method comprising the following steps:
[0018] After the hydrocarbon raw material is mixed with water vapor, it is introduced into a fluidized reactor to contact with the regenerated catalyst and undergo a catalytic decomposition reaction to obtain a reactant stream and a deactivated catalyst with carbon; the reaction oil gas obtained by the catalytic cracking reaction and the deactivated catalyst with carbon are separated into gas and solid;
[0019] The separated reaction oil and gas enters a separation unit and is further separated into products including hydrogen, carbon monoxide, carbon dioxide, methane and other hydrocarbons;
[0020] The obtained deactivated catalyst with carbon is sent to the regenerator, contacted with oxygen-containing gas and water vapor for high-temperature gasification and regeneration. After regeneration, the deactivated catalyst with carbon is returned to the fluidized bed reactor for recycling; the regenerated flue gas is sent to the separation unit to obtain carbon monoxide and carbon dioxide; the separated carbon monoxide can be used as a raw material for water-gas shift to further produce hydrogen and carbon dioxide.
[0021] The hydrocarbon oil is various animal and plant oils rich in hydrocarbons, and the hydrocarbon is selected from one or more mixtures of hydrocarbon raw materials, mineral oils and synthetic oils. Hydrocarbon raw materials are well known to those skilled in the art, for example, can be one or more mixtures of straight-run gasoline, straight-run diesel, vacuum wax oil, atmospheric residue, vacuum residue or hydrocarbon oils obtained by secondary processing of a primary processing device. The hydrocarbon oil obtained by secondary processing is one or more of coker gasoline, catalytic diesel, hydrogenated diesel, coker diesel, coker wax oil, deasphalted oil, furfural refined raffinate oil. Mineral oil is selected from one or more mixtures of coal liquefaction oil, oil sand oil and shale oil. Synthetic oil is a distillate obtained by FT synthesis of coal, natural gas or asphalt.
[0022] The hydrocarbon feedstock meets one or two indicators selected from the group consisting of a hydrogen content of less than 12 wt% and an aromatic hydrocarbon content of greater than 30 wt%.
[0023] The catalyst comprises the following components by weight percentage:
[0024] A) 15% to 65% natural minerals,
[0025] B) 20% to 60% oxide,
[0026] C) 5% to 30% metal active components.
[0027] The method provided by the present invention can be carried out in various existing fluidized reactors, wherein the fluidized reactor is selected from one or a combination of a turbulent bed, a fast bed and a dilute phase transport bed. The fluidized reactor includes a pre-lifting section and at least one reaction zone fluidized reactor from bottom to top. In order to allow the crude oil to react fully and according to different quality requirements of the target product, the reaction zones can be 2-8, preferably 2-3.
[0028] The conditions of the catalytic decomposition reaction include: the reaction temperature of the fluidized reactor is 450-800°C, preferably 550-700°C, the reaction time is 0.1-10 seconds, preferably 1-8 seconds, the weight ratio of the catalyst to the hydrocarbon feedstock is 5-100, preferably 20-50; the weight ratio of water vapor to the hydrocarbon feedstock is 0.1-20, preferably 1-10.
[0029] According to the method provided by the present invention, the deactivated catalyst with carbon is generally first separated from the reaction oil and gas to obtain the deactivated catalyst with carbon and reaction oil and gas, and then the obtained reaction oil and gas are separated by a subsequent separation unit to obtain hydrogen and CO2, CO, methane, other hydrocarbons and other products. The method of separating hydrogen, CO, CO2 and the like from the reaction products is similar to the conventional technical method in the field, and the present invention is not limited to this and is not described in detail herein.
[0030] In the method provided by the present invention, preferably the deactivated catalyst enters the stripping section under the action of gravity, the hydrocarbon products adsorbed on the deactivated catalyst are stripped by water vapor, and the deactivated catalyst after stripping enters the regenerator.
[0031] In the method provided by the present invention, the deactivated catalyst with carbon can be gasified and regenerated at high temperature in a conventional regenerator, and a single regenerator or multiple regenerators can be used. During the regeneration process, oxygen-containing gas and water vapor are generally introduced from the bottom of the regenerator. After the oxygen-containing gas and water vapor are introduced into the regenerator, the deactivated catalyst with carbon contacts with oxygen and water vapor to undergo a gasification reaction to generate hydrogen, CO and, and at the same time, the coke on the catalyst is removed to regenerate the catalyst. The flue gas generated after the catalyst is regenerated is separated into gas and solid at the top of the regenerator, and the flue gas enters the separation unit for further separation to obtain hydrogen, CO and CO2.
[0032] In the method provided by the present invention, the CO obtained in the separation unit is sent to the water-gas shift unit, and further reacts with water vapor to obtain hydrogen and CO2. The water-gas shift of the CO and water vapor adopts the existing technology well known to those skilled in the art. The CO2 obtained in the separation unit can be recovered and captured using the existing technology.
[0033] In the method provided by the present invention, the oxygen concentration in the oxygen-containing gas at the bottom of the regenerator is 22-100% by volume, preferably 25-80% by volume, and the volume ratio of the water vapor to the oxygen-containing gas is 1-10, preferably 1-5. In the method provided by the present invention, the operating conditions of the high-temperature regeneration-gasification in the regenerator are preferably: the temperature is 550-1000°C, preferably 700-950°C; the gas superficial linear velocity is 0.2-1.0 m / s, preferably 0.3-0.8 m / s, and the average residence time of the catalyst is 0.5-10 minutes, preferably 1-5 minutes.
[0034] In the method provided by the present invention, the natural minerals in the catalyst are selected from one or more of kaolin, halloysite, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite, and the content of the natural minerals on a dry basis is 15% to 65% by weight, preferably 20% to 60% by weight; the oxides are one or more of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, and amorphous silicon aluminum, and the content of the oxides is 20% to 60% by weight, preferably 20% to 40% by weight, and more preferably 25% to 35% by weight, based on the total amount of the catalyst and in terms of oxide weight percentage.
[0035] Based on the weight of the catalyst, the metal active component content is 5% to 30% by weight, preferably 8-25% by weight. The metal active component is selected from one or more compounds of transition metal elements, preferably one or more of nickel, cobalt, iron, tungsten, molybdenum, manganese, copper, zirconium and chromium.
[0036] In the method provided by the present invention, the catalyst preparation method adopts the preparation method of conventional catalytic cracking catalyst, which is a method well known to those skilled in the art. The metal can be loaded on the catalyst by impregnation method or slurry method, preferably impregnation method, which are well known to those skilled in the art.
[0037] The accompanying drawings are used to provide further understanding of the present disclosure and constitute a part of the specification. They are used to explain the present disclosure together with the following detailed description, but do not constitute a limitation of the present disclosure.
[0038] like Figure 1 As shown, the regenerated catalyst from pipeline 7 enters the fluidized reactor 1 and accelerates upward along the reactor. The hydrocarbon feedstock is mixed with the water vapor from pipeline 6 through pipeline 5 and then injected into the fluidized reactor 1 to contact the regenerated catalyst. The hydrocarbon feedstock undergoes a catalytic reaction on the hot catalyst and accelerates upward. After the generated reaction products and the deactivated catalyst with carbon are separated, the reaction products enter the separation unit 3 through pipeline 8 and are separated into hydrogen 9, carbon dioxide 10, carbon monoxide 15, methane 11 and other hydrocarbons 4. The other separated hydrocarbons 4 can be sent back to the fluidized reactor 1 alone, or mixed with the hydrocarbon feedstock 5 and sent to the fluidized reactor 1 together.
[0039] The catalyst with carbon passes through the inclined pipe 12 and enters the regenerator 2, and contacts with the oxygen-containing gas 13 and water vapor 16 entering from the bottom of the regenerator to undergo a gasification reaction, and burns off the coke on the catalyst to regenerate the catalyst with carbon. The regenerated flue gas enters the separation unit 3 through the flue gas pipeline 14, and hydrogen 9, carbon dioxide 10 and carbon monoxide 15 are separated in the separation unit. The regenerated catalyst is circulated to the bottom of the fluidized reactor 1 through the pipeline 7.
[0040] The present invention will be further described in the following examples, but the present invention is not limited thereto.
[0041] The raw materials used in the examples and comparative examples are all catalytic diesel, and the properties are shown in Table 1. The catalyst used in the comparative example is an industrial catalyst, the trade name is DMMC-1, and the properties are shown in Table 2.
[0042] The catalyst preparation method used in the examples is briefly described as follows:
[0043] 1) 75.4 kg of kaolin (solid content 71.6 wt%) was slurried with 250 kg of decationized water, and then 54.8 kg of pseudo-boehmite (solid content 63 wt%) was added, and the pH was adjusted to 2-4 with hydrochloric acid, and stirred evenly. The mixture was allowed to stand and age at 60-70°C for 1 hour, and the pH was maintained at 2-4. The temperature was lowered to below 60°C, and 41.5 kg of aluminum sol (Al2O3 content of 21.7 wt%) was added, and stirred for 40 minutes to obtain a mixed slurry, which was spray-dried and calcined to obtain a matrix sample.
[0044] 2) 3 kg of Ni(NO3)2 was dissolved in 5.5 kg of water to prepare a Ni(NO3)2·6H2O aqueous solution, 10 kg of the molecular sieve catalyst sample was immersed in the Ni(NO3)2·6H2O aqueous solution, and the obtained mixture was dried at 180°C for 4 hours and calcined at 600°C for 2 hours. After repeated immersion, drying and calcination, the content of Ni loaded on the catalyst sample reached 15%, and the catalyst A of the embodiment was obtained.
[0045] Example 1
[0046] according to Figure 1 The catalytic decomposition reaction test of catalytic diesel was carried out on the riser reactor. The catalytic diesel entered the lower part of the riser reactor, contacted with the hot regenerated catalyst and underwent catalytic decomposition reaction. The reaction products and the regenerated catalyst entered the closed cyclone separator from the reactor outlet. The reaction products and the regenerated catalyst were quickly separated, and the reaction products were separated into cracked gas and liquid products in the separation system.
[0047] The regenerated catalyst enters the stripping section under the action of gravity, and the hydrocarbon products adsorbed on the regenerated catalyst are stripped by water vapor. The stripped regenerated catalyst enters the regenerator, and contacts with oxygen-rich air and water vapor for gasification and regeneration reaction; the regenerated catalyst is then returned to the riser reactor for recycling, and the regenerated flue gas enters the separation system. The operating conditions and product distribution are listed in Table 3.
[0048] From the results in Table 3, it can be seen that the hydrogen yield is as high as 21.03%, the CO yield in the reaction product is 27.69%, and the CO2 yield is 24.58%. The CO concentration in the regenerated flue gas is 50.59% by volume, the CO2 concentration is 5.01% by volume, and the hydrogen concentration in the flue gas is 10.23% by volume.
[0049] Comparative Example 1
[0050] The test was carried out on a medium-sized device of a riser, the catalytic diesel feedstock was the same as in Example 1, and the catalyst was DMMC-1.
[0051] The catalytic diesel enters the riser reactor and contacts the hot DMMC-1 catalyst to undergo a catalytic decomposition reaction. The reaction products and the spent catalyst enter the closed cyclone separator from the reactor outlet. The reaction products and the spent catalyst are quickly separated. The reaction products are separated into gas and liquid products according to the distillation range in the separation system.
[0052] The spent catalyst enters the stripping section under the action of gravity, and the hydrocarbon products adsorbed on the spent catalyst are stripped by water vapor. The spent catalyst after stripping enters the regenerator and is regenerated by contact with air; the regenerated catalyst is then returned to the riser reactor for recycling; the operating conditions and product distribution are listed in Table 3.
[0053] From the results in Table 3, it can be seen that the hydrogen yield is 1.35%, the ethylene yield is 3.01%, the propylene yield is 9.35%, and the CO and CO2 yields in the reaction products are low. No CO was detected in the regeneration flue gas, the CO2 concentration was 15.01% by volume, and the O2 concentration was 3.55% by volume.
[0054] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0055] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0056] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the content of the present invention.
[0057] Table 1
[0058] project Catalytic diesel <![CDATA[Density (20 °C) / (kg / m 3 )]]> 948.9 <![CDATA[Kinematic viscosity (20 °C) / (mm 2 / s)]]> 3.754 Total acid value / (mg KOH / g) <0.05 Freezing point / ℃ -27 Closed cup flash point / ℃ 66 Distillation range / ℃ Initial distillation point 197.9 5% 220.4 10% 228.4 50% 262.5 70% 283.1 90% 308.6 95% 319.5 Final distillation point 329.9
[0059] Table 2
[0060] Comparative Example 1 Example 1 DMMC-1 Catalyst A Physical properties <![CDATA[Specific surface area, m 2 / g]]> 106 118 <![CDATA[Matrix specific surface area, m 2 / g]]> 64 95 <![CDATA[Pore volume, cm 3 / g]]> 0.13 0.106 Sieve composition, weight % 0~40 microns 30.9 20.7 0~80 microns 75.0 76.1 0~105 microns 89.1 84.3 0~149 microns 98.4 97.5 Average particle size / micron 55.6 54.9 Micro-anti-activity, % 65 40 Metal content, weight % Ni 0.06 15.0
[0061] Table 3
[0062] Example 1 Comparative Example 1 Riser reaction conditions Reaction temperature, °C 650 650 Reaction time, seconds 2 2 Water to oil weight ratio 0.2 0.2 Weight ratio of catalyst to catalytic diesel 20 20 Regeneration conditions Regeneration temperature, °C 650 850 Oxygen concentration in regeneration air, volume % 50 50 Gas superficial velocity, m / s 0.8 0.8 Average stay time, minutes 5 5 Product distribution, weight % CO 27.69 0.23 <![CDATA[CO2]]> 24.58 0.9 <![CDATA[H2]]> 21.03 1.35 Methane 5.36 3.36 Other hydrocarbons 9.82 84.53 Coke 11.52 9.63 total 100.00 100.00 Regeneration flue gas composition, volume % CO 50.59 0 <![CDATA[CO2]]> 5.01 15.01 <![CDATA[N2]]> 34.17 81.44 <![CDATA[O2]]> 0 3.55 <![CDATA[H2]]> 10.23 0
Claims
1. A method for catalytically producing hydrogen and enriching carbon dioxide, the method comprising the following steps: After mixing the hydrocarbon raw material with water vapor, the mixture is introduced into a fluidized reactor to contact with the regenerated catalyst and perform a catalytic decomposition reaction, wherein the reaction temperature of the fluidized reactor is 450-800°C, the reaction time is 0.1-10 seconds, the weight ratio of the catalyst to the hydrocarbon raw material is 5-100, and the weight ratio of the water vapor to the hydrocarbon raw material is 0.1-20, to obtain a reactant stream and a carbon-bearing catalyst; the reaction oil gas obtained by the catalytic cracking reaction and the deactivated catalyst are subjected to gas-solid separation; the hydrocarbon raw material is diesel; based on the dry weight of the catalyst, the catalyst comprises 15%-65% of natural minerals, 20%-60% of oxides, and 5%-30% of metal active components, wherein the natural minerals are selected from one or more of kaolin, montmorillonite, diatomaceous earth, attapulgite, sepiolite, halloysite, hydrotalcite, bentonite and rectorite, the oxides are one or more of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, and amorphous silicon aluminum, and the metal active components are selected from one or more of compounds of transition metal elements; The separated reaction oil and gas enters a separation unit and is further separated into products including hydrogen, carbon monoxide, carbon dioxide, methane and other hydrocarbons; The obtained deactivated catalyst is sent to the regenerator, contacted with oxygen-containing gas and water vapor for high-temperature gasification and regeneration. The volume ratio of water vapor to oxygen-containing gas is 1-5, the temperature is 550-1000°C, and the average residence time of the catalyst is 0.5-10 minutes. After the deactivated catalyst is regenerated, it is returned to the fluidized bed reactor for recycling; the regenerated flue gas is sent to the separation unit to obtain carbon monoxide and carbon dioxide.
2. The method according to claim 1, wherein the diesel is selected from one or more of catalytic diesel, hydrogenated diesel, and coker diesel.
3. The method according to claim 1, characterized in that The content of the metal active component is 8% to 25% by weight, and the metal active component is selected from one or more of nickel, cobalt, iron, tungsten, molybdenum, manganese, copper, zirconium and chromium.
4. The method according to claim 1, characterized in that The reaction temperature of the fluidized bed reactor is 550-700°C, the reaction time is 1-8 seconds, the weight ratio of the catalyst to the hydrocarbon raw material is 20-50; the weight ratio of water vapor to the hydrocarbon raw material is 1-10.
5. The method according to claim 1, characterized in that The fluidized reactor is selected from one or a combination of a riser reactor, a fast bed and a dense phase fluidized bed.
6. The method according to claim 5, characterized in that The fluidized bed reactor includes a pre-lifting section and at least one reaction zone from bottom to top. In order to allow the crude oil to react fully and according to different quality requirements of the target product, the number of reaction zones is 2-8.
7. The method according to claim 6, characterized in that The number of the reaction zones is 2-3.
8. The method according to claim 1, characterized in that The oxygen concentration in the oxygen-containing gas at the bottom of the regenerator is 22 volume % to 100 volume %.
9. The method according to claim 1, characterized in that: The oxygen concentration in the oxygen-containing gas at the bottom of the regenerator is 25 volume % to 80 volume %.
10. The method according to claim 1, characterized in that The operating conditions of high-temperature regeneration-gasification in the regenerator are: the gas superficial linear velocity is 0.2-1.0 m / s.
11. The method according to claim 1, characterized in that: The operating conditions of high temperature-gasification in the regenerator are: temperature of 700-950°C; gas superficial linear velocity of 0.3-0.8 m / s; and average residence time of the catalyst of 1-5 minutes.