A kind of high-toughness impregnated film paper and its preparation method and application

By optimizing flexible paper substrates and modified phenolic resins, combined with improved impregnation liquid formula, the cracking problem of wood composite materials in the immersed paper is solved, the flexibility and crack resistance are improved, and the application range is broadened.

CN116005490BActive Publication Date: 2024-12-06DYNEA GUANGDONG
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
CN202211597046.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-12-06
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Existing adhesive paper-decorated wood composite materials are prone to cracking, resulting in a decrease in surface appearance quality and loss of protective function, limiting its use environment and scope.

Method used

By preferring flexible paper substrates and modified phenolic resins, combined with improved impregnation liquid formulations, the flexibility of the impregnation film paper is improved, including the use of high toughness phenolic resins, flexible agents, wetting agents, moisture-repellents and mold release agents, Form high toughness impregnated film paper.

Benefits of technology

It significantly improves the flexibility and crack resistance of the adhesive film paper, extends its service life, and broadens its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116005490B_ABST
    Figure CN116005490B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-toughness impregnated film paper and a preparation method and application thereof, which belong to the field of decorative paper. The preparation method of high-toughness impregnated film paper comprises the following steps: impregnating a flexible paper substrate with a high-toughness phenolic resin impregnated adhesive, and then drying to obtain the high-toughness impregnated film paper; the high-toughness phenolic resin impregnated adhesive comprises the following components in parts by weight: 85-95 parts of high-toughness phenolic resin, 5-15 parts of flexibilizer, 0.1-0.6 parts of wetting agent, 1-3 parts of moisture-proof agent and 0.2-0.8 parts of release agent. The present invention synergistically toughens the impregnated film paper by toughening the phenolic resin, the impregnated adhesive and the substrate, thereby significantly improving the flexibility of the impregnated film paper, thereby providing a new technical solution for solving the problem of cracking on the surface of the wood composite material of the impregnated paper veneer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of decorative paper, and in particular to a high-toughness dipped film paper and a preparation method and application thereof. Background Art

[0002] Wood composite materials (commonly known as artificial boards) are a kind of wood materials made of artificial forest wood as the main raw material through composite or recombinant processing technology. They can be used in flooring, furniture and other home furnishing fields. They are an indispensable livelihood industry for improving people's quality of life and have a very important basic position in the national economy and social development. At present, most wood composite materials such as plywood, fiberboard, particleboard, joinery, etc. need to be surface-finished before they can be used in the manufacture and application of home products. The wood composite materials with impregnated paper veneer (commonly known as ecological boards) are widely used in furniture, flooring, cabinets, doors and windows and other home manufacturing and decorative materials due to their beautiful and generous surface, harmonious color, heat resistance, wear resistance, waterproof and other characteristics.

[0003] Most of the resins used in existing impregnated facing papers are melamine resins, and some are impregnated (modified) with urea-formaldehyde resins or phenol-formaldehyde resins. Cracking is a common defect of wood composite materials with impregnated paper facings, which not only reduces the surface appearance quality of the material, but also loses its protective function in severe cases, severely limiting the use environment and scope of the facing wood composite materials. The main reason for the cracking of wood composite materials with impregnated paper facings is that the shrinkage and swelling coefficients of the wood substrate and the surface impregnated film paper are different. The wood substrate is anisotropic, and the shrinkage performance of the transverse grain is greater than that of the longitudinal grain, while the impregnated film paper is isotropic. When the wood composite material with impregnated paper facings absorbs or desorbs moisture, internal stress will be generated at the interface between the wood substrate and the impregnated film paper. When the internal stress is greater than the strength of the paper, cracks will occur on the paper surface. The patent (CN201811140359) of high-toughness polyurethane amine-formaldehyde resin glue, high-toughness adhesive film paper and preparation method proposes adding modified polyurethane to amine-formaldehyde resin to increase the flexibility of amine-formaldehyde resin, thereby improving the flexibility of adhesive film paper and thus improving the anti-cracking ability of veneer. However, it is difficult to completely solve the cracking problem of adhesive film paper by only toughening the adhesive layer. Summary of the invention

[0004] The purpose of the present invention is to provide a high-toughness impregnated film paper and a preparation method and application thereof to solve the problems existing in the prior art. The present invention synergistically toughens the impregnated film paper by optimizing a flexible paper substrate, preparing a high-toughness phenolic resin, and then improving the formulation of the impregnating liquid. The flexibility of the impregnated film paper is improved, and a new solution is provided for solving the problem of cracking on the surface of the impregnated paper veneer wood composite material.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention: a method for preparing high-toughness impregnated film paper, comprising the following steps:

[0007] The flexible paper substrate is impregnated with a high-toughness phenolic resin to perform a dipping treatment, and then dried to obtain the high-toughness impregnated film paper;

[0008] The high-toughness phenolic resin impregnated rubber material comprises the following components in parts by weight: 85-95 parts of high-toughness phenolic resin, 5-15 parts of flexibilizer, 0.1-0.6 parts of wetting agent, 1-3 parts of moisture-proof agent and 0.2-0.8 parts of release agent.

[0009] Furthermore, the finished product of the high-toughness impregnated film paper has a basis weight of 150 to 300 g / m 2 .

[0010] Furthermore, the preparation of the high-toughness phenolic resin impregnated rubber material specifically includes: weighing various raw materials according to weight proportions, stirring and mixing them evenly, and obtaining the high-toughness phenolic resin impregnated rubber material.

[0011] Furthermore, the high-toughness phenolic resin impregnation rubber has a viscosity of 80-400 cps, a pH value of 8.5-10.0, and a non-volatile component content of 40-60 wt.%.

[0012] Furthermore, the high-toughness phenolic resin comprises the following raw materials in parts by weight: 100 parts of phenol, 110-150 parts of 50wt.% formaldehyde aqueous solution, 3-8 parts of alkaline compounds, 15-20 parts of glycol compounds, 10-15 parts of urea and 4-8 parts of ethylene urea.

[0013] Furthermore, the alkaline compound is sodium hydroxide and / or potassium hydroxide.

[0014] Furthermore, the preparation of the high-toughness phenolic resin comprises the following steps:

[0015] Weigh each raw material by weight, mix 60-80% by weight of phenol, diol compounds and part of 50wt.% formaldehyde aqueous solution, control the molar ratio of formaldehyde to phenol to be 0.5-1.0, then adjust the pH to 3.0-4.0, and react at 85-105°C; after the reaction is completed, add the remaining 50wt.% formaldehyde aqueous solution, adjust the pH to 8.0-8.5, then add urea and water, and keep warm at 85-95°C; after the insulation is completed, adjust the pH to 4.5-5.0, react at 85-95°C, add alkaline compounds and remaining phenol, react at 70-80°C until the product viscosity reaches 50-200cps, add ethylene urea, cool to room temperature, and obtain the high-toughness phenolic resin.

[0016] Modification of phenolic resin can improve the flexibility of phenolic resin. The modification principle is as follows: a linear phenolic resin intermediate modified by diol compounds is obtained by reacting low-ratio phenol and formaldehyde (the molar ratio of formaldehyde to phenol is 0.5-1.0) and diol compounds under acidic conditions at high temperature. Phenol and formaldehyde react under this condition to form a flexible linear thermoplastic phenolic resin; the addition of diol compounds forms a steric hindrance by reacting with the phenolic hydroxyl group to form an etherification reaction, making it difficult for the two ortho-hydrogens on the ether bond to participate in the reaction, thereby reducing the crosslinking density; at the same time, the diol compounds can also react with the hydroxymethyl in the intermediate hydroxymethylphenol to make Flexible diol compounds are bonded to phenolic resins to reduce the crosslinking density of the resin after curing and improve the flexibility of the resin; secondly, after obtaining a flexible phenolic resin intermediate modified by diol compounds, formaldehyde and urea are added, and through a process of first alkali and then acid, the length of the urea-formaldehyde resin chain segment is increased to improve flexibility; finally, phenol is added for further polycondensation reaction to ensure that the product has good bonding strength; after the polycondensation is completed, ethylene urea is added to ensure that the product has lower free formaldehyde while retaining good bonding strength, so that the prepared modified phenolic resin not only has good flexibility, but also has the advantages of environmental protection, light color and high bonding strength.

[0017] Furthermore, the high-toughness phenolic resin has a viscosity of 50 to 200 cps, a pH value of 9.0 to 10.0, and a non-volatile component content of 45 to 60 wt.%.

[0018] Furthermore, the diol compound includes one or more of ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, dibutylene glycol, polyethylene glycol and polypropylene glycol.

[0019] Furthermore, the flexible paper substrate is selected from any one of cotton paper, pure wood pulp paper, straw pulp paper or bamboo pulp paper; the water absorption rate of the flexible paper substrate is 50-100 mm / 10 min, the tensile strength is 0.5-5.0 KN / m, the air permeability is 60-500 μm / Pa·s, and the elongation at break is 2-5%.

[0020] Furthermore, the flexibilizer includes a polyvinyl alcohol aqueous solution and / or a polyvinyl acetate emulsion; the wetting agent includes one or more of silanol, glycol ether, polyoxyethylene alkylphenol ether and polyoxyethylene fatty alcohol ether; the moisture-proof agent is an emulsified paraffin solution; the release agent includes one or more of stearic acid, emulsified methyl silicone oil, polysiloxane, alkyl polyglycerol compounds and fatty acids; the drying is regional segmented drying, the drying temperature is 110 to 160°C, and the operating speed is 25 to 50 m / min.

[0021] The flexibilizer selected by the invention has moderate viscosity, good toughening effect and good process applicability, and when mixed with high-toughness phenolic resin, the obtained dipping material has good stability.

[0022] Furthermore, the degree of polymerization of the polyvinyl alcohol aqueous solution is 800-2000, the degree of alcoholysis is 85-100%, and the mass concentration is 10-35%; the content of non-volatile components in the polyvinyl acetate emulsion is 40-60wt.%, the viscosity is 1000-15000cps, and the pH is 5-9.

[0023] The second technical solution of the present invention: a high-toughness impregnated film paper prepared by the above-mentioned preparation method of the high-toughness impregnated film paper.

[0024] The third technical solution of the present invention: an application of the above-mentioned high-toughness impregnated film paper in material surface finishing and bonding between materials.

[0025] The present invention discloses the following technical effects:

[0026] (1) The maximum axial diameter of the film paper prepared by the present invention is small, the maximum bending force does not decrease significantly, the fracture disturbance is large, and it has good flexibility and anti-cracking ability.

[0027] (2) The present invention synergistically toughens the impregnated film paper by toughening the phenolic resin, the impregnating material and the substrate, thereby significantly improving the flexibility of the impregnated film paper, thereby providing a new technical solution to the problem of cracking on the surface of the impregnated paper veneer wood composite material.

[0028] (3) The high-toughness impregnated film paper prepared by the present invention can be used as a bonding material, thereby broadening the application range of the film paper. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 This is the appearance of the membrane paper sample prepared in Example 1 of the present invention;

[0031] Figure 2 This is a test result diagram of the maximum shaft diameter of the membrane paper prepared in Example 1 of the present invention, wherein the left figure shows the state of the membrane paper, and the right figure shows the state of the membrane paper after being tested by a 2mm cylindrical shaft;

[0032] Figure 3This is a test result diagram of the maximum shaft diameter of the membrane paper prepared in Comparative Example 3 of the present invention, wherein the left figure shows the state of the membrane paper, and the right figure shows the state of the membrane paper after being tested by a 5mm cylindrical shaft.

[0033] Figure 4 This is a sample picture of a bamboo board and an aluminum board bonded together using the film paper prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0035] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0036] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0037] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0038] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0039] The “parts” described in the following examples are all “parts by weight”.

[0040] Example 1

[0041] A method for preparing high-toughness impregnated film paper:

[0042] (1) Selection of flexible paper substrate

[0043] Cotton paper was selected with a water absorption rate of 100 mm / 10 min, a tensile strength of 5.0 KN / m, an air permeability of 500 μm / Pa·s, and an elongation at break of 5%.

[0044] (2) Preparation of high-toughness phenolic resin

[0045] 60 parts of phenol, 17 parts of diethylene glycol and 30 parts of 50wt.% formaldehyde aqueous solution were mixed and added into a reactor, the pH was adjusted to 3.3, and the mixture was reacted at 100°C for 2h; after the reaction, 90 parts of 50wt.% formaldehyde aqueous solution were added, the pH was adjusted to 8.2, and then 15 parts of urea and 30 parts of water were added, and the mixture was kept warm at 85°C for 30min; after the insulation was completed, the pH was adjusted to 4.7 with acid, and the mixture was reacted at 85°C for 2h, 3.5 parts of sodium hydroxide and 40 parts of phenol were added, and the mixture was reacted at 80°C until the viscosity of the product reached 110cps, 4 parts of ethylene urea were added, and the mixture was cooled to room temperature to obtain a high-toughness phenolic resin with a viscosity of 105cps, a pH of 9.3, and a non-volatile component content of 51wt.%.

[0046] (3) Preparation of high-toughness phenolic resin impregnation

[0047] 90 parts of high-toughness phenolic resin, 5 parts of polyvinyl acetate emulsion (non-volatile component content is 48wt.%, viscosity is 5000cps, pH is 8), 0.2 parts of glycol ether, 2 parts of emulsified paraffin solution, 0.5 parts of stearic acid, are stirred and mixed to obtain a high-toughness phenolic resin impregnated rubber material with a viscosity of 180cps, a pH value of 9.25, and a non-volatile component content of 50wt.%.

[0048] (4) Impregnation with high-toughness phenolic resin (coated paper impregnation)

[0049] The high-toughness phenolic resin impregnation material prepared in step (3) is placed in a special impregnation glue tank to form a flow cycle. The cotton paper runs under the traction of mechanical equipment and passes through the high-toughness phenolic resin impregnation glue material. The temperature of the glue material is 28-33°C to obtain the impregnated coated paper.

[0050] (5) Drying of impregnated coated paper

[0051] The coated paper after impregnation is dried in sections. The drying area is divided into four controlled temperature sections: low temperature (110℃), medium temperature (120℃), medium high temperature (135℃), medium low temperature (115℃). The running speed is 25m / min. After drying, the finished product of high-toughness impregnated film paper is obtained (see the appearance picture). Figure 1 ), basis weight is 250g / m 2 .

[0052] Example 2

[0053] A method for preparing high-toughness impregnated film paper:

[0054] (1) Selection of flexible paper substrate

[0055] Pure wood pulp paper is selected, with a water absorption rate of 60mm / 10min, a tensile strength of 3.0KN / m, an air permeability of 60μm / Pa·s, and an elongation at break of 3%.

[0056] (2) Preparation of high-toughness phenolic resin

[0057] 70 parts of phenol, 20 parts of propylene glycol and 45 parts of 50wt.% formaldehyde aqueous solution were mixed and added into a reactor, the pH was adjusted to 3.8, and the mixture was reacted at 85°C for 4 hours; after the reaction, 95 parts of 50wt.% formaldehyde aqueous solution were added, the pH was adjusted to 8.5, and then 12 parts of urea and 5 parts of water were added, and the mixture was kept warm at 90°C for 20 minutes; after the insulation was completed, the pH was adjusted to 4.8 with acid, and the mixture was reacted at 90°C for 1.5 hours, 6 parts of sodium hydroxide and 30 parts of phenol were added, and the mixture was reacted at 80°C until the viscosity of the product reached 200cps, 8 parts of ethylene urea were added, and the mixture was cooled to room temperature to obtain a high-toughness phenolic resin with a viscosity of 200cps, a pH of 9.6, and a non-volatile component content of 58wt.%.

[0058] (3) Preparation of high-toughness phenolic resin impregnation

[0059] 85 parts of high-toughness phenolic resin, 10 parts of polyvinyl alcohol aqueous solution (polymerization degree of 1700, alcoholysis degree of 88%, mass concentration of 15%), 0.2 parts of glycol ether, 2 parts of emulsified paraffin solution, and 0.5 parts of stearic acid were stirred and mixed to obtain a high-toughness phenolic resin impregnated rubber material with a viscosity of 320 cps, a pH value of 9.5, and a non-volatile component content of 54 wt.%.

[0060] (4) Impregnation with high-toughness phenolic resin (coated paper impregnation)

[0061] The high-toughness phenolic resin impregnation material prepared in step (3) is placed in a special impregnation glue tank to form a flow cycle. The pure wood pulp paper runs under the traction of mechanical equipment and passes through the high-toughness phenolic resin impregnation glue material. The temperature of the glue material is 28-33°C to obtain the impregnated coated paper.

[0062] (5) Drying of impregnated coated paper

[0063] The coated paper after impregnation is dried in sections. The drying area is divided into four controlled temperature sections: low temperature (120℃), medium temperature (130℃), medium high temperature (145℃), medium low temperature (125℃). The running speed is 30m / min. After drying, the finished product of high-toughness impregnated paper is obtained, with a basis weight of 300g / m 2 .

[0064] Example 3

[0065] A method for preparing high-toughness impregnated film paper:

[0066] (1) Selection of flexible paper substrate

[0067] Straw pulp paper is selected, with a water absorption rate of 70 mm / 10 min, a tensile strength of 3.0 KN / m, an air permeability of 150 μm / Pa·s, and an elongation at break of 4%.

[0068] (2) Preparation of high-toughness phenolic resin

[0069] 80 parts of phenol, 15 parts of butanediol and 35 parts of 50wt.% formaldehyde aqueous solution were mixed and added into a reactor, the pH was adjusted to 3.0, and the mixture was reacted at 90°C for 3h; after the reaction, 100 parts of 50wt.% formaldehyde aqueous solution were added, the pH was adjusted to 8.0, and then 10 parts of urea and 90 parts of water were added, and the mixture was kept warm at 90°C for 10min; after the insulation, the pH was adjusted to 5.0 with acid, and the mixture was reacted at 90°C for 1h, 5 parts of sodium hydroxide and 20 parts of phenol were added, and the mixture was reacted at 75°C until the viscosity of the product reached 60cps, 6 parts of ethylene urea were added, and the mixture was cooled to room temperature to obtain a high-toughness phenolic resin having a viscosity of 55cps, a pH of 9.5, and a non-volatile component content of 46wt.%.

[0070] (3) Preparation of high-toughness phenolic resin impregnation

[0071] 88 parts of high-toughness phenolic resin, 7 parts of polyvinyl acetate emulsion (non-volatile component content is 60wt.%, viscosity is 10000cps, pH is 5), 0.2 parts of glycol ether, 2 parts of emulsified paraffin solution, 0.5 parts of stearic acid, are stirred and mixed uniformly to obtain a high-toughness phenolic resin impregnated rubber material with a viscosity of 130cps, a pH value of 9.3, and a non-volatile component content of 47wt.%.

[0072] (4) Impregnation with high-toughness phenolic resin (coated paper impregnation)

[0073] The high-toughness phenolic resin impregnation material prepared in step (3) is placed in a special impregnation glue tank to form a flow circulation. The straw pulp paper runs under the traction of mechanical equipment and passes through the high-toughness phenolic resin impregnation glue material. The temperature of the glue material is 28-33°C to obtain the impregnated coated paper.

[0074] (5) Drying of impregnated coated paper

[0075] The coated paper after impregnation is dried in sections. The drying area is divided into four controlled temperature sections: low temperature (130℃), medium temperature (140℃), medium high temperature (155℃), medium low temperature (135℃). The running speed is 40m / min. After drying, the finished product of high-toughness impregnated film paper is obtained, with a basis weight of 120g / m 2 .

[0076] Example 4

[0077] A method for preparing high-toughness impregnated film paper:

[0078] (1) Selection of flexible paper substrate

[0079] Bamboo pulp paper is selected, with a water absorption rate of 50mm / 10min, a tensile strength of 3.0KN / m, an air permeability of 400μm / Pa·s, and an elongation at break of 5%.

[0080] (2) Preparation of high-toughness phenolic resin

[0081] 70 parts of phenol, 15 parts of ethylene glycol and 40 parts of 50wt.% formaldehyde aqueous solution were mixed and added into a reactor, the pH was adjusted to 3.5, and the mixture was reacted at 95°C for 3h; after the reaction, 100 parts of 50wt.% formaldehyde aqueous solution were added, the pH was adjusted to 8.4, and then 11 parts of urea and 40 parts of water were added, and the mixture was kept warm at 95°C for 10min; after the insulation, the pH was adjusted to 4.7 with acid, and the mixture was reacted at 90°C for 1h, 8 parts of potassium hydroxide and 30 parts of phenol were added, and the mixture was reacted at 75°C until the product viscosity reached 60cps, 5 parts of ethylene urea were added, and the mixture was cooled to room temperature to obtain a high-toughness phenolic resin with a viscosity of 130cps, a pH of 9.7, and a non-volatile component content of 45wt.%.

[0082] (3) Preparation of high-toughness phenolic resin impregnation

[0083] 90 parts of high-toughness phenolic resin, 5 parts of polyvinyl acetate emulsion (non-volatile component content is 48wt.%, viscosity is 12000cps, pH is 7), 0.2 parts of glycol ether, 2 parts of emulsified paraffin solution, 0.5 parts of stearic acid, are stirred and mixed to obtain a high-toughness phenolic resin impregnated rubber material with a viscosity of 200cps, a pH value of 9.5, and a non-volatile component content of 45wt.%.

[0084] (4) Impregnation with high-toughness phenolic resin (coated paper impregnation)

[0085] The high-toughness phenolic resin impregnation material prepared in step (3) is placed in a special impregnation glue tank to form a flow circulation. The straw pulp paper runs under the traction of mechanical equipment and passes through the high-toughness phenolic resin impregnation glue material. The temperature of the glue material is 28-33°C to obtain the impregnated coated paper.

[0086] (5) Drying of impregnated coated paper

[0087] The coated paper after impregnation is dried in sections. The drying area is divided into four controlled temperature sections: low temperature (125℃), medium temperature (135℃), medium high temperature (160℃), medium low temperature (130℃). The running speed is 50m / min. After drying, the finished product of high-toughness impregnated paper is obtained, with a basis weight of 150g / m 2 .

[0088] Example 5

[0089] A method for preparing high-toughness impregnated film paper:

[0090] (1) Selection of flexible paper substrate

[0091] Cotton paper was selected with a water absorption rate of 100 mm / 10 min, a tensile strength of 0.5 KN / m, an air permeability of 500 μm / Pa·s, and an elongation at break of 2%.

[0092] (2) Preparation of high-toughness phenolic resin

[0093] 70 parts of phenol, 17 parts of diethylene glycol and 30 parts of 50wt.% formaldehyde aqueous solution were mixed and added to a reactor, the pH was adjusted to 3.0, and the mixture was reacted at 105°C for 2h; after the reaction, 80 parts of 50wt.% formaldehyde aqueous solution were added, the pH was adjusted to 8.5 with caustic soda, and then 15 parts of urea and 30 parts of water were added, and the mixture was kept warm at 85°C for 30min; after the insulation was completed, the pH was adjusted to 5.0 with acid, and the mixture was reacted at 85°C for 2h, 3.5 parts of sodium hydroxide and 30 parts of phenol were added, and the mixture was reacted at 70°C until the viscosity of the product reached 150cps, 4 parts of ethylene urea were added, and the mixture was cooled to room temperature to obtain a high-toughness phenolic resin with a viscosity of 145cps, a pH of 9.3, and a non-volatile component content of 52wt.%.

[0094] (3) Preparation of high-toughness phenolic resin impregnation

[0095] 95 parts of high-toughness phenolic resin, 15 parts of polyvinyl acetate emulsion (non-volatile component content is 40wt.%, viscosity is 1000cps, pH is 6), 0.1 parts of polyoxyethylene alkylphenol ether, 1 part of emulsified paraffin solution, 0.2 parts of emulsified methyl silicone oil are stirred and mixed to obtain a high-toughness phenolic resin impregnated rubber material with a viscosity of 180cps, a pH value of 9.1, and a non-volatile component content of 50wt.%.

[0096] (4) Impregnation with high-toughness phenolic resin (coated paper impregnation)

[0097] The high-toughness phenolic resin impregnation material prepared in step (3) is placed in a special impregnation glue tank to form a flow cycle. The cotton paper runs under the traction of mechanical equipment and passes through the high-toughness phenolic resin impregnation glue material. The temperature of the glue material is 28-33°C to obtain the impregnated coated paper.

[0098] (5) Drying of impregnated coated paper

[0099] The coated paper after impregnation is dried in sections. The drying area is divided into four controlled temperature sections: low temperature (130℃), medium temperature (140℃), medium high temperature (155℃), and medium low temperature (135℃). The running speed is 40m / min. After drying, a high-toughness impregnated film paper product is obtained with a basis weight of 200g / m 2 .

[0100] Example 6

[0101] Same as Example 5, except that step (3) is specifically as follows:

[0102] 95 parts of high-toughness phenolic resin, 12 parts of polyvinyl alcohol aqueous solution (polymerization degree 800, alcoholysis degree 85%, mass concentration 10%), 0.6 parts of polyoxyethylene fatty alcohol ether, 3 parts of emulsified paraffin solution, and 0.8 parts of polysiloxane were stirred and mixed to obtain a high-toughness phenolic resin impregnated rubber material with a viscosity of 160 cps, a pH value of 9.2, and a non-volatile component content of 47 wt.%.

[0103] After drying, the finished product of high-toughness impregnated film paper is obtained, with a basis weight of 180g / m 2 .

[0104] Comparative Example 1

[0105] The same as Example 1, except that the high-toughness phenolic resin is replaced by ordinary pure phenolic resin, with a viscosity of 110 cps, a pH value of 9.6, and a non-volatile component content of 52 wt.%.

[0106] Comparative Example 2

[0107] The same as Example 1, except that no polyvinyl acetate emulsion is added in step (3).

[0108] Comparative Example 3

[0109] The same as Example 1, except that the cotton paper in step (1) is replaced by ordinary kraft paper with a water absorption rate of 30 mm / 10 min, a tensile strength of 4.1 KN / m, an air permeability of 50.3 μm / Pa·s, and an elongation at break of 2.0%.

[0110] Effect Example 1

[0111] The properties of the membrane papers prepared in the examples and comparative examples were measured, and the results are shown in Table 1.

[0112] The performance test method is as follows:

[0113] (1) Maximum axial diameter of film paper at break: The film paper was cut into strips of 15 mm × 250 mm and baked at 135 °C for 10 min to completely cure the resin. According to the standard GB / T 6742-2007 Paint and varnish bending test (cylindrical axis), the maximum axial diameter of the film paper at break after curing was tested using a QTY-32 paint film bending tester to characterize the film paper's anti-cracking ability and flexibility during hot pressing. The smaller the axial diameter, the better the film paper's anti-cracking ability and flexibility.

[0114] (2) Maximum bending force and fracture disturbance: Twenty sheets of 25 mm × 1500 mm film paper were stacked together and hot pressed on a press at 140°C for 8 min. After the hot pressing, the obtained samples were polished with 180-mesh sandpaper and tested for maximum bending force and fracture disturbance using a universal testing machine according to the standard GB / T 9341-2008 Determination of Flexural Properties of Plastics.

[0115] Figure 2 The maximum shaft diameter test for film paper fracture: the film paper sample of Example 1 (left) and the sample after being tested by a 2 mm cylindrical shaft (right);

[0116] Figure 3 The maximum shaft diameter test for film paper breakage: the state of the sample of comparative example 3 (left) and the sample after being tested with a 5mm cylindrical shaft (right).

[0117] Table 1 Performance data of the embodiments and comparative examples

[0118]

[0119]

[0120] From the comparison between Example 1 and Comparative Examples 1 to 3, it can be seen that the maximum axial diameter of the membrane paper prepared in Example 1 is small, the maximum bending force does not decrease significantly, and the fracture disturbance is large, which means that the membrane paper prepared in Example 1 has good flexibility and anti-cracking ability.

[0121] Effect Example 2

[0122] The adhesive properties of the film paper prepared in Example 1 were measured by using the impregnated film paper to bond eucalyptus veneers, eucalyptus veneers and aluminum plates, bamboo plates and aluminum plates, non-woven fabrics and aluminum plates, and non-woven fabrics and eucalyptus veneers, with a hot pressing temperature of 140°C and a hot pressing time of 8 minutes. According to the standard GB / T17657-2013 Test methods for physical and chemical properties of artificial boards and veneer artificial boards 4.19.4.1.

[0123] The immersion peeling strength of the test board is tested. The test results are shown in Table 2 and Figure 4 .

[0124] Figure 4 This is a sample picture of a bamboo board and an aluminum board bonded together using the film paper prepared in Example 1 of the present invention.

[0125] Table 2 Performance test results of bonding various substrates using the film paper prepared in Example 1

[0126] Substrate Immersion peel strength Test Results Eucalyptus-Eucalyptus No peeling qualified Eucalyptus-Aluminum Plate No peeling qualified Bamboo board-aluminum board No peeling qualified Non-woven fabric-aluminum sheet No peeling qualified Non-woven fabric-Eucalyptus No peeling qualified

[0127] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing high-toughness impregnated film paper, It is characterized in that The following steps are involved: The flexible paper substrate is impregnated with a high-toughness phenolic resin to perform a dipping treatment, and then dried to obtain the high-toughness impregnated film paper; The high-toughness phenolic resin impregnated rubber material comprises the following components in parts by weight: 85-95 parts of high-toughness phenolic resin, 5-15 parts of flexibilizer, 0.1-0.6 parts of wetting agent, 1-3 parts of moisture-proof agent and 0.2-0.8 parts of release agent; The high-toughness phenolic resin comprises the following raw materials in parts by weight: 100 parts of phenol, 110-150 parts of 50wt.% formaldehyde aqueous solution, 3-8 parts of alkaline compounds, 15-20 parts of glycol compounds, 10-15 parts of urea and 4-8 parts of ethylene urea; The flexible paper substrate is selected from any one of cotton paper, pure wood pulp paper, straw pulp paper or bamboo pulp paper; the flexible paper substrate has a water absorption rate of 50-100 mm / 10 min, a tensile strength of 0.5-5.0 KN / m, an air permeability of 60-500 μm / Pa·s, and an elongation at break of 2-5%; The flexibilizer includes polyvinyl alcohol aqueous solution and / or polyvinyl acetate emulsion.

2. The method for preparing the high-toughness impregnated film paper according to claim 1, It is characterized in that The alkaline compound is sodium hydroxide and / or potassium hydroxide.

3. The method for preparing the high-toughness impregnated film paper according to claim 1, It is characterized in that The preparation of the high-toughness phenolic resin comprises the following steps: Weigh each raw material by weight, mix 60-80% by weight of phenol, diol compounds and part of 50wt.% formaldehyde aqueous solution, control the molar ratio of formaldehyde to phenol to be 0.5-1.0, then adjust the pH to 3.0-4.0, and react at 85-105°C; after the reaction is completed, add the remaining 50wt.% formaldehyde aqueous solution, adjust the pH to 8.0-8.5, then add urea and water, and keep warm at 85-95°C; after the insulation is completed, adjust the pH to 4.5-5.0, react at 85-95°C, add alkaline compounds and remaining phenol, react at 70-80°C until the product viscosity reaches 50-200cps, add ethylene urea, cool to room temperature, and obtain the high-toughness phenolic resin.

4. The method for preparing the high-toughness phenolic resin according to claim 3, It is characterized in that The diol compound includes one or more of ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, dibutylene glycol, polyethylene glycol and polypropylene glycol.

5. The method for preparing the high-toughness impregnated film paper according to claim 1, It is characterized in that The wetting agent includes one or more of silanol, glycol ether, polyoxyethylene alkylphenol ether and polyoxyethylene fatty alcohol ether; the moisture-proof agent is an emulsified paraffin solution; the release agent includes one or more of stearic acid, emulsified methyl silicone oil, polysiloxane, alkyl polyglycerol compounds and fatty acids; the viscosity of the high-toughness phenolic resin impregnation rubber is 80-400cps, the pH is 8.5-10.0, and the non-volatile content is 40-60wt.%; the drying is regional segmented drying, the drying temperature is 110-160°C, and the operating speed is 25-50m / min.

6. The method for preparing the high-toughness impregnated film paper according to claim 1, It is characterized in that The degree of polymerization of the polyvinyl alcohol aqueous solution is 800-2000, the degree of alcoholysis is 85-100%, and the mass concentration is 10-35%; the content of non-volatile components in the polyvinyl acetate emulsion is 40-60wt.%, the viscosity is 1000-15000cps, and the pH is 5-9.

7. A high-toughness impregnated film paper prepared by the method for preparing high-toughness impregnated film paper according to any one of claims 1 to 6.

8. Use of the high-toughness impregnated film paper according to claim 7 in material surface finishing and bonding between materials.

Citation Information

Patent Citations

  • High toughness polyurethane amine-aldehyde resin glue, high toughness film adhesive and preparation method

    CN109321180A

  • Flame-proof floor and processing technique thereof

    CN101195231A

  • Method for preparing toughening agent modified phenolic fiber

    CN101709516A

  • Phenolic aldehyde foam material

    CN103073840A

  • Modified phenolic foam

    CN103694625A