Method for preparing hydrogenation catalyst, catalyst prepared by the method and application thereof

By mixing pseudo-boehmite containing phosphorus and magnesium with hydrogenation active metal components, the preparation process of the hydrogenation catalyst is simplified, the problem of insufficient catalyst activity and stability in the existing technology is solved, and a catalyst with excellent performance is obtained. High performance catalyst suitable for hydrocarbon oil hydrogenation reaction.

CN116020498BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111255180.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-10-15
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

The preparation process of existing hydrogenation catalysts is cumbersome, it is difficult to improve the activity and stability of the catalyst, and it is difficult to obtain an alumina carrier with both large mesopore volume and total pore volume, resulting in insufficient catalyst performance.

Method used

The pseudo-boehmite containing phosphorus and magnesium is mixed with the precursor of the hydrogenation active metal component to form. It only needs one drying and roasting. The process of drying and roasting the pseudo-boehmite to prepare the carrier is omitted, and a specific activation process is adopted. conditions to obtain an excellent hydrogenation catalyst.

Benefits of technology

The preparation process is simplified, the hydrogenation activity and stability of the catalyst are improved, the cost is reduced, the operating cycle of the catalyst is extended, and the economic benefits of the refinery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003323900590000131
    Figure BDA0003323900590000131
  • Figure BDA0003323900590000141
    Figure BDA0003323900590000141
Patent Text Reader

Abstract

The present invention discloses a method for preparing a hydrogenation catalyst, a catalyst prepared by the method and application, the method comprising the following steps: (1) preparing pseudo-boehmite containing phosphorus and magnesium; (2) mixing and molding the pseudo-boehmite containing phosphorus and magnesium with a precursor of a hydrogenation active metal component, and then drying and activating in sequence to obtain the hydrogenation catalyst; the activation conditions include: a heating rate of 50-600°C / hour, a temperature of 400-1000°C, and a time of 1-10 hours. The preparation method provided by the present invention directly mixes and molds the pseudo-boehmite with a precursor of a hydrogenation active metal component, and only needs to be dried and calcined once to obtain a hydrogenation catalyst, thereby omitting the process of drying and calcining the pseudo-boehmite to prepare a carrier, simplifying the preparation process, and making the obtained catalyst have excellent hydrogenation activity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of hydrogenation catalysts, and in particular to a method for preparing a hydrogenation catalyst, a catalyst prepared by the method and applications thereof. Background Art

[0002] The hydrogenation catalyst is the core of the full hydrogen refinery, and the hydrogenation catalyst is mainly composed of a carrier and an active metal component. Alumina, especially γ-alumina, is often used as a carrier for the preparation of catalysts because of its good pore structure, specific surface area and heat stability. In particular, the pore structure of the alumina carrier is particularly critical to the performance of the catalyst. The raw material of the alumina carrier is generally pseudo-boehmite. The prior art discloses a variety of different methods for preparing phosphorus-containing pseudo-boehmite, which controls the pore distribution and pore volume of alumina by different methods. The performance of pseudo-boehmite and alumina described in the prior art is superior in some aspects, but it is difficult to obtain phosphorus-containing alumina with bimodal pores and large pore volume and total pore volume in both pore distributions.

[0003] A large number of hydrogenation catalysts and preparation methods are disclosed in the prior art, and there are also many reports on the influence of carrier characteristics on catalyst performance, including the influence of pore size, pore distribution, acidity, additives, etc. on the final catalyst performance. However, in the solutions in the prior art, it is difficult to obtain an alumina carrier with a large mesopore volume, a macropore volume and a total pore volume, and thus it is impossible to obtain a corresponding hydrogenation catalyst. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art that the catalyst preparation process is complicated and the activity and stability of the catalyst need to be further improved, and to provide a preparation method of a hydrogenation catalyst and a hydrogenation catalyst and application. The method simplifies the preparation process, and the prepared catalyst has excellent hydrogenation activity and stability.

[0005] The inventors of the present invention discovered during the course of research that, in the preparation process of the hydrogenation catalyst, a pseudo-boehmite containing phosphorus and magnesium is directly mixed with a precursor of a hydrogenation active metal component and formed, and then the hydrogenation catalyst can be obtained after only one drying and calcination. Compared with the prior art, the process of drying and calcining the pseudo-boehmite to prepare the carrier is omitted, the preparation process is simplified, and the obtained catalyst has excellent hydrogenation activity and stability.

[0006] In order to achieve the above object, the present invention provides a method for preparing a hydrogenation catalyst, which comprises the following steps:

[0007] (1) preparing pseudo-boehmite containing phosphorus and magnesium;

[0008] (2) mixing the phosphorus- and magnesium-containing pseudo-boehmite with a precursor of a hydrogenation-active metal component, forming the mixture, and then drying and activating the mixture in sequence to obtain the hydrogenation catalyst;

[0009] The activation conditions include: a heating rate of 50-600°C / hour, a temperature of 400-1000°C, and a time of 1-10 hours;

[0010] The hydrogenation active metal component contains at least one Group VIB metal component and at least one Group VIII

[0011] The amount of each component is such that the final catalyst, calculated as oxide, the content of the VIB Group metal component is 0.5-50% by weight, the content of the VIII Group metal component is 0.5-20% by weight.

[0012] The present invention also provides a hydrogenation catalyst prepared by the method and application of the hydrogenation catalyst in hydrocarbon oil hydrogenation reaction.

[0013] Compared with the prior art, the preparation method provided by the present invention directly mixes and shapes the pseudo-boehmite with the precursor of the hydrogenation active metal component, and then only needs to be dried and calcined once to obtain a hydrogenation catalyst, thereby omitting the process of drying and calcining the pseudo-boehmite to prepare the carrier, simplifying the preparation process, and making the prepared catalyst have excellent hydrogenation activity and stability, and have better demetallization, desulfurization and carbon removal activities under the same other conditions, which is beneficial to reducing the catalyst cost and increasing the catalyst operation cycle, thereby benefiting the improvement of the overall economic benefits of the refinery. DETAILED DESCRIPTION

[0014] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0015] In the present invention, unless otherwise specified, the pore distribution refers to the distribution of pore diameters. The pore size refers to the pore diameter.

[0016] According to the method for preparing the catalyst provided by the present invention, there is no special requirement for the pseudo-boehmite containing phosphorus and magnesium. When the pseudo-boehmite containing phosphorus and magnesium in step (1) meets the following requirements, the prepared hydrogenation catalyst has better performance. Specifically, based on the total dry weight of the pseudo-boehmite containing phosphorus and magnesium, the content of Al2O3 is 84-99.8% by weight, and more preferably 84-99.7% by weight; the content of P2O5 is 0.1-6% by weight, the content of MgO is 0.1-5% by weight, and the content of the auxiliary element is 0-5% by weight, and more preferably 0.1-5% by weight; preferably, the phosphorus and magnesium-containing alumina obtained by calcining the pseudo-boehmite containing phosphorus and magnesium at 600°C for 3 hours has a bimodal pore structure, and the bimodal pore structure is measured by mercury intrusion, and the pore distribution is located at a mesopore volume V of 3-100nm. 中孔 The pore volume V of the macropores is 0.7-1.7 mL / g and the pore distribution is between 100-5000 nm. 大孔 1.7-4.7 mL / g, total pore volume V 总 2.4-6.4 mL / g; further preferably, the pore distribution of the phosphorus and magnesium-containing alumina is located in the mesopore volume V of 3-100 nm. 中孔 The pore volume V of the macropores is 0.9-1.5 mL / g and the pore distribution is between 100-5000 nm. 大孔 1.8-3.2mL / g, total pore volume V 总 It is 2.7-4.7mL / g.

[0017] In order to further improve the performance of the catalyst, the phosphorus and magnesium-containing pseudo-boehmite may also contain optional auxiliary elements, wherein the auxiliary elements include metal auxiliary elements and / or non-metal auxiliary elements; the metal auxiliary elements are selected from at least one of lithium, sodium, potassium, rubidium, cesium, francium, beryllium, calcium, zirconium and titanium; the non-metal auxiliary elements are selected from at least one of boron, fluorine and silicon.

[0018] The catalyst prepared according to the preparation method of the present invention preferably has a peak height P of a low-temperature reduction peak at 300-500° C. when measured by a hydrogen temperature-programmed reduction method (H2-TPR). 低温峰 The peak height P of the high temperature reduction peak at 650-850℃ 高温峰 The ratio S = P 低温峰 / P 高温峰 is 0.5-2.0; further preferably, the peak height P of the low temperature reduction peak 低温峰 The peak height P 高温峰 The ratio S = P 低温峰 / P 高温峰 It is 0.7-1.9, preferably 0.8-1.8.

[0019] According to the preparation method of the present invention, the purpose of the activation in step (2) is to convert pseudo-boehmite into alumina, convert the hydrogenation active metal into an oxidized state, and enhance the interaction between the hydrogenation active metal component and the carrier. Preferably, the activation conditions include: a heating rate of 100-550°C / hour, a temperature of 410-880°C, preferably 430-850°C, and most preferably 450-830°C.

[0020] The type and content of the hydrogenation metal active component are conventionally selected in the art, for example, the VIB group metal component is Mo and / or W, and the VIII group metal component is Co and / or Ni; the amount of each component is such that in the final catalyst, based on the total amount of the catalyst and calculated as oxide, the content of the VIB group metal component is 5-45% by weight, and the content of the VIII group metal component is 1-15% by weight.

[0021] The present invention does not particularly limit the specific preparation method of the pseudo-boehmite containing phosphorus and magnesium. In order to obtain an alumina carrier having large mesopore volume, macropore volume and total pore volume, the pseudo-boehmite containing phosphorus and magnesium can be prepared by the following steps:

[0022] (a) contacting a solution of a phosphorus-containing compound, a magnesium-containing compound, or an inorganic aluminum-containing compound with an acid or a base to carry out a precipitation reaction, or contacting an organic aluminum-containing compound with a solution of a magnesium-containing compound or a phosphorus-containing compound to carry out a hydrolysis reaction, thereby obtaining a hydrated aluminum oxide containing phosphorus and magnesium;

[0023] (b) aging the phosphorus- and magnesium-containing hydrated aluminum oxide obtained above at a pH of 7-10.5, and then drying the aged solid product to obtain pseudo-boehmite containing phosphorus and magnesium;

[0024] The precipitation reaction or the hydrolysis reaction in step (a) is carried out at a pH of 4-7.

[0025] Further preferably, the precipitation reaction or the hydrolysis reaction in step (a) is carried out at a pH of 4-6.5; the temperatures of the precipitation reaction and the hydrolysis reaction are each independently 30-90°C; the conditions of the precipitation reaction include: the reaction temperature is 40-90°C, preferably 45-80°C, and the reaction time is 10-60 minutes, preferably 10-30 minutes; the conditions of the hydrolysis reaction include: the reaction temperature is 40-90°C, preferably 45-80°C, and the reaction time is 2-30 hours, preferably 2-20 hours.

[0026] The inorganic aluminum-containing compound, phosphorus-containing compound, magnesium-containing compound, organic aluminum-containing compound, acid and base in the preparation step are all conventionally selected in the art. For example, the inorganic aluminum compound is an aluminum salt and / or aluminate; the organic aluminum-containing compound is at least one of alkoxy aluminums that can undergo hydrolysis reaction with water to produce hydrated aluminum oxide precipitation; the phosphorus-containing compound is selected from at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate, diammonium hydrogen phosphate, sodium phosphate and potassium phosphate; the magnesium-containing compound is an inorganic magnesium salt, selected from one or more of magnesium chloride, magnesium nitrate, magnesium sulfate and magnesium acetate; the acid is at least one of sulfuric acid, hydrochloric acid, nitric acid, carbonic acid, phosphoric acid, formic acid, acetic acid, citric acid and oxalic acid; the base is at least one of sodium aluminate, potassium aluminate, sodium hydroxide, potassium hydroxide and ammonia water.

[0027] In the present invention, there is no particular limitation on the manner of adding the phosphorus-containing compound and the magnesium-containing compound. The phosphorus-containing compound (or an aqueous solution of the phosphorus-containing compound) and the magnesium-containing compound (or an aqueous solution of the magnesium-containing compound) can be added separately, or the phosphorus-containing compound (or its aqueous solution) and the magnesium-containing compound (or its aqueous solution) can be mixed with one or more of the raw materials in advance, and then the raw materials containing the phosphorus-containing compound and the magnesium-containing compound are reacted, as long as the precipitation reaction or the hydrolysis reaction is carried out in the presence of the phosphorus-containing compound and the magnesium-containing compound.

[0028] The pH of the aging step in preparing pseudo-boehmite is preferably 8-10, and the remaining operations are conventional steps in the art, for example, the aging conditions include: temperature of 50-95°C, preferably 55-90°C; time of 0.5-8 hours, preferably 2-6 hours. The drying conditions in step (b) can be: temperature of 50-350°C, preferably 80-250°C, and drying time of 1-12 hours, preferably 2-8 hours.

[0029] In order to introduce a promoter that is beneficial to improving the performance of the catalyst, when preparing pseudo-boehmite containing phosphorus and magnesium, an optional compound containing a promoter element is also added in the precipitation reaction or hydrolysis reaction of step (a), and the promoter element includes a metal promoter element and / or a non-metal promoter element; the metal promoter element is selected from at least one of lithium, sodium, potassium, rubidium, cesium, francium, beryllium, calcium, zirconium and titanium, and is more preferably selected from at least one of lithium, sodium, potassium, beryllium, calcium, zirconium and titanium; the non-metal promoter element is selected from at least one of boron, fluorine and silicon. In order to further improve the performance of the catalyst, the amount of each component is such that the content of Al2O3 in the prepared pseudo-boehmite containing phosphorus and magnesium is 85-99.8% by weight, more preferably 85-99.7% by weight, the content of P2O5 is 0.1-5% by weight, the content of MgO is 0.1-5% by weight, and the content of auxiliary elements is 0-5% by weight, more preferably 0.1-5% by weight, based on the total dry amount of the pseudo-boehmite containing phosphorus and magnesium.

[0030] The step of preparing pseudo-boehmite containing phosphorus and magnesium in the present invention also includes separating, washing and drying the aged product after the aging reaction. According to the method provided by the present invention, the separation can be a well-known technology in the art, such as a method of filtering or centrifugal separation. The washing and drying methods can be methods commonly used in preparing pseudo-boehmite, for example, the washing agent can be water, and the drying can be at least one of oven drying, forced air drying, spray drying and flash drying. The drying temperature can be 100-350°C, preferably 120-300°C.

[0031] According to the preparation method provided by the present invention, in the catalyst preparation process, when the pseudo-boehmite is kneaded with the active metal component, an organic additive can also be introduced. The present invention has no special restrictions on the type of the organic additive, the organic additive is selected from at least one of oxygen-containing and / or nitrogen-containing organic matter, the oxygen-containing organic matter is selected from organic alcohols and / or organic acids, and the nitrogen-containing organic matter is selected from at least one of organic amines and organic amine salts; specifically, the oxygen-containing organic matter is selected from at least one of ethylene glycol, glycerol, polyethylene glycol (molecular weight 200-1500), diethylene glycol, butanediol, acetic acid, maleic acid, oxalic acid, aminotriacetic acid, 1,2-cyclohexanediaminetetraacetic acid, citric acid, tartaric acid, and malic acid, preferably at least one of ethylene glycol, glycerol, polyethylene glycol and citric acid; the nitrogen-containing organic matter is selected from at least one of ethylenediamine, diethylenetriamine, cyclohexanediaminetetraacetic acid, aminoacetic acid, nitrilotriacetic acid, EDTA and its amine salts, preferably EDTA and / or nitrilotriacetic acid.

[0032] According to the preparation method provided by the present invention, there is no particular limitation on the drying conditions after kneading the hydrogenation active metal group with pseudo-boehmite containing phosphorus and magnesium. Preferably, the drying conditions include: a drying temperature of 80-200°C, preferably 100-150°C; a drying time of 1-8 hours, preferably 2-6 hours. The present invention does not particularly limit the drying method, and the drying can be at least one of oven drying, blast drying, spray drying and flash drying. According to the preparation method provided by the present invention, there is no particular limitation on the activation and drying atmospheres, which can be at least one of air, oxygen and nitrogen, preferably air.

[0033] The present invention also provides the use of the hydrogenation catalyst prepared by the above preparation method in the hydrocarbon oil hydrogenation reaction. According to the present invention, the hydrogenation catalyst can be pre-sulfurized according to the conventional method in the art before use, so that the active metal component supported on it is converted into a metal sulfide component; the pre-sulfurization method can be: the hydrogenation catalyst is pre-sulfurized with sulfur, hydrogen sulfide or sulfur-containing raw materials under the condition of 140-400°C in the presence of hydrogen. This pre-sulfurization can be carried out outside the device or in-situ in the device.

[0034] The present invention has no particular limitation on the hydrogenation conditions when the hydrogenation catalyst is used, and the common reaction conditions in the art can be adopted; preferably, the reaction temperature is 200-420°C, more preferably 220-400°C, the pressure is 2-18MPa, more preferably 2-16MPa, and the liquid hourly volume space velocity is 0.1-10 hours. -1 , more preferably 0.15-6 hours -1 , the hydrogen-to-oil volume ratio is 50-5000, and more preferably 50-4000. The present invention has no particular restrictions on the hydroprocessing reaction device when the hydrogenation catalyst is applied, and can be any reactor sufficient to allow the feedstock oil to contact and react with the hydrogenation catalyst under the hydroprocessing reaction conditions, such as a fixed bed reactor, a slurry bed reactor, a moving bed reactor or an ebullating bed reactor. The present invention has no particular restrictions on the application object of the hydrogenation catalyst, and can be directly used to process various types of hydrocarbon oil feedstocks to carry out hydrogenation modification or hydrocracking. The hydrocarbon oil feedstock can be various heavy mineral oils or synthetic oils or their mixed distillate oils, for example, it can be selected from at least one of crude oil, distillate oil, solvent refined oil, wax paste, wax oil, Fischer-Tropsch synthetic oil, coal liquefaction oil, light deasphalted oil and heavy deasphalted oil; it is particularly suitable for the hydroprocessing of at least one of gasoline, diesel, wax oil, lubricating oil, kerosene, naphtha, atmospheric residue oil, vacuum residue oil, petroleum wax and Fischer-Tropsch synthetic oil.

[0035] The present invention will be described in detail below by way of examples. In the following examples, the raw materials involved are all commercially available unless otherwise specified.

[0036] The pore volumes in different pore size ranges in alumina containing phosphorus and magnesium were determined by mercury intrusion porosimetry.

[0037] The H2-TPR (programmed temperature reduction) experiment of the oxidized catalyst was measured on the AutoChemⅡ2920 multifunctional adsorption instrument of Micromeritics, USA. The experimental steps are as follows: 0.20g of 40-60 mesh catalyst was loaded into a U-shaped quartz tube, heated to 50℃ at a rate of 2℃ / min in 50mL / min argon, pretreated the sample for 10min, and then switched to Ar carrier gas containing 10% H2 volume fraction, with a gas flow rate of 50mL / min. After the baseline is stable, the temperature is raised to 1000℃ at a rate of 10℃ / min. The carrier gas passes through the reactor and enters the cold trap to condense the water generated during the reduction process. At the same time, the signal is detected by a thermal conductivity cell detector to obtain the TPR spectrum of the sample.

[0038] Example 1

[0039] This example is used to illustrate the hydrogenation catalyst and its preparation method provided by the present invention.

[0040] (1) Preparation of pseudo-boehmite PA1:

[0041] In a 2-liter reaction tank, 5000 ml of aluminum sulfate solution with a concentration of 60 g aluminum oxide / liter, 40 g magnesium nitrate, 8.0 mL of 85 wt% concentrated phosphoric acid and 6 wt% ammonia solution were added in parallel for precipitation reaction. The reaction temperature was 50°C and the reaction time was 30 minutes. The flow rate of ammonia solution was controlled to make the pH of the reaction system 5.0. After the precipitation reaction was completed, an appropriate amount of ammonia solution was added to the slurry to make the pH value of the slurry 8.7. The slurry was aged at 70°C for 120 minutes and then filtered. The filter cake was washed twice with deionized water. The filter cake was dried at 120°C for 24 hours to obtain PA1. The structure and composition of PA1 were characterized by XRD. PA1 has a pseudo-boehmite structure. The contents of phosphorus, magnesium and auxiliary elements in PA1 are listed in Table 1. PA1 was then calcined at 600°C for 3 hours, and the pore structure of the obtained alumina was measured. The results are listed in Table 1.

[0042] (2) Preparation of hydrogenation catalyst C1:

[0043] 1000 g of PA1, 30 g of sesbania powder (produced by Jiangsu Fengxian Runshun Trading Co., Ltd.), 317 g of ammonium molybdate, 218 g of nickel nitrate and 25 g of nitric acid, and 1200 g of water were mixed evenly, and then extruded into butterfly-shaped wet strips with an outer diameter of 1.7 mm on a plunger extruder, and the butterfly-shaped wet strips were dried at 130° C. for 4 hours, heated to 620° C. at a heating rate of 180° C. / h, and activated for 3 hours to obtain hydrogenation catalyst C1. The content of the metal oxide in the hydrogenation catalyst is shown in Table 2.

[0044] Comparative Example 1

[0045] Pseudo-boehmite and catalyst were prepared according to the method of Example 1, except that only 8.0 mL of phosphoric acid with a concentration of 85 wt% was added to the aluminum sulfate solution without magnesium nitrate, to obtain CPA1. XRD characterization was performed according to the method of Example 1, and CPA1 had a pseudo-boehmite structure. The composition of CPA1 calculated by XRD characterization is listed in Table 1. DC1 was prepared according to the method of preparing catalyst C1 in Example 1, and the pore structure of alumina obtained after CPA1 was calcined at 600°C for 3 hours was measured. The results are listed in Table 1. The content of metal oxides in DC1 is shown in Table 2.

[0046] Comparative Example 2

[0047] Pseudo-boehmite and catalyst were prepared according to the method of Example 1, except that the aluminum sulfate solution did not contain magnesium nitrate, and the flow rate of the ammonia solution was directly controlled to make the pH of the reaction system 8.7. After the precipitation reaction was completed, it was not necessary to add ammonia solution to the slurry to adjust the pH value, thereby obtaining CPA2. According to the method of Example 1, CPA2 was characterized by XRD, and it was found that CPA2 had a pseudo-boehmite structure. The composition of CPA2 calculated by XRD characterization is listed in Table 1. DC2 was prepared according to the method of preparing catalyst C1 in Example 1, and the pore structure of alumina obtained after CPA2 was calcined at 600°C for 3 hours was measured. The results are listed in Table 1, and the content of metal oxides in DC2 is shown in Table 2.

[0048] Comparative Example 3

[0049] The hydrogenation catalyst was prepared by the method in Example 1, except that the activation conditions were different, specifically, calcination at 350° C. for 3 hours to obtain the hydrogenation catalyst DC3. The content of the metal oxide in the hydrogenation catalyst is shown in Table 2.

[0050] Example 2

[0051] This example is used to illustrate the hydrogenation catalyst and its preparation method provided by the present invention.

[0052] Preparation of pseudo-boehmite PA2:

[0053] In a 2-liter reaction tank, 4000 ml of aluminum chloride solution containing 22.1 mL of 85 wt% concentrated phosphoric acid and 20 g of magnesium nitrate and 1000 ml of sodium aluminate solution containing 210 g of aluminum oxide / liter and a caustic coefficient of 1.58 were added in parallel to carry out precipitation reaction, the reaction temperature was 80°C, the reactant flow was adjusted so that the neutralization pH value was 4.0, and the reaction residence time was 15 minutes; 5 wt% dilute ammonia water was added to the obtained slurry to adjust the slurry pH to 9.0, and the temperature was raised to 85°C, aged for 3 hours, and then filtered with a vacuum filter. After the filtration was completed, 20 liters of deionized water (temperature 85°C) were added to the filter cake to rinse the filter cake for about 30 minutes. The washed qualified filter cake was added to 3 liters of deionized water and stirred into slurry, and the slurry was pumped into a spray dryer for drying, and the outlet temperature of the spray dryer was controlled in the range of 100-110°C. The material drying time was about 2 minutes, and PA2 was obtained after drying. According to the method of Example 1, XRD characterization was performed and PA2 had a pseudo-boehmite structure. The composition of PA2 calculated by XRD characterization is listed in Table 1.

[0054] The pore structure of alumina obtained by calcining PA2 at 600°C for 3 hours was measured according to the method of Example 1, and the results are listed in Table 1.

[0055] Catalyst C2 was prepared according to the method of Example 1, except that the activation heating rate was 150°C / hour and the activation temperature was 650°C. The content of metal oxides in C2 is shown in Table 2.

[0056] Example 3

[0057] This example is used to illustrate the hydrogenation catalyst and its preparation method provided by the present invention.

[0058] (1) Preparation of pseudo-boehmite PA3:

[0059] In a 2-liter three-necked flask with a stirrer and a reflux condenser, 1000 g of an azeotrope of isopropanol-water (water content is 15 wt%), 4.6 mL of 85% concentrated phosphoric acid, 8 g of magnesium nitrate, and ammonia water are added to adjust the pH to 5.1, and then heated to 60°C, 500 g of molten aluminum isopropoxide is slowly dripped into the flask through a separatory funnel, reacted for 2 hours, ammonia water is added to adjust the pH to 8.5, refluxed for 20 hours, dehydrated isopropanol is evaporated, aged at 80°C for 6 hours, and water-containing isopropanol is evaporated while aging. After aging, the hydrated alumina is filtered and dried at 120°C for 24 hours to obtain PA3. According to the method of Example 1, PA3 has a pseudo-boehmite structure, and the composition of PA3 calculated by XRD characterization is listed in Table 1.

[0060] (2) PA3 was used to prepare C3 according to the method of Example 1; the pore structure of alumina obtained after PA3 was calcined at 600°C for 3 hours was measured. The results are listed in Table 1. The content of metal oxides in C3 is shown in Table 2.

[0061] Comparative Example 4

[0062] Phosphorus-containing pseudo-boehmite was prepared according to the typical method in "Research on Heavy Oil Hydrogenation Catalyst Support Materials". 8.8 mL of 85% concentrated phosphoric acid was added to a concentration of 57 g·L -1 3000mL of aluminum sulfate solution and 64g·L -1 2500mL of sodium aluminate solution was used for precipitation reaction, the neutralization pH was 8.0, the reaction time was 70min, and then aging was performed, the aging temperature was 90°C, the aging pH was 8.5, and after aging, the filter cake was slurried and washed twice with deionized water, and the filter cake was dried at 120°C for 24 hours to prepare phosphorus-containing pseudo-boehmite CPA4. According to the method of Example 1, XRD characterization was performed, and CPA4 had a pseudo-boehmite structure. The composition of CPA4 calculated by XRD characterization is listed in Table 1.

[0063] The CPA4 was used to prepare DC4 according to the method of Example 1. The pore structure of alumina obtained by calcining CPA4 at 600° C. for 3 hours was measured, and the results are listed in Table 1. The content of metal oxides in DC4 is shown in Table 2.

[0064] Example 4

[0065] Pseudo-boehmite and alumina carriers were prepared according to the method of Example 1, except that 2 grams of sodium acetate was also added to the aluminum sulfate solution to obtain PA4. According to the method of Example 1, XRD characterization was performed, and PA4 had a pseudo-boehmite structure. The composition of PA4 calculated by XRD characterization is listed in Table 1. PA4 was used to prepare C4 according to the method of Example 1. The pore structure of alumina obtained after PA4 was calcined at 600°C for 3 hours was measured, and the results are listed in Table 1. The content of metal oxides in C4 is shown in Table 2.

[0066] Example 5

[0067] Pseudo-boehmite and alumina carriers were prepared according to the method of Example 1, except that 4 g of ammonium fluoride was also added to the aluminum sulfate solution to obtain PA5.

[0068] According to the method of Example 1, PA5 was characterized by XRD, and it was found that the structure of PA5 was pseudo-boehmite. The composition of PA5 calculated by XRD characterization was listed in Table 1. PA5 was used to prepare C5 according to the method of Example 1. The pore structure of alumina obtained by calcining PA5 at 600°C for 3 hours was measured, and the results were listed in Table 1. The content of metal oxides in C5 is shown in Table 2.

[0069] Comparative Example 5

[0070] The method of Example 1 was followed, except that PA1 was calcined at 350°C for 3 hours before being kneaded with the hydrogenation active metal. The catalyst DC5 was obtained. The content of the catalyst metal components is shown in Table 2.

[0071] Comparative Example 6

[0072] Catalyst DC6 was prepared according to the method of Example 1, except that the hydrogenation active metal component was introduced by impregnation, specifically:

[0073] Take 1000 grams of PA1 and 30 grams of sesbania powder (produced by Jiangsu Fengxian Runshun Trading Co., Ltd.) and mix them evenly, then add 1320 milliliters of an aqueous solution containing 25g of nitric acid to mix, and then extrude into butterfly-shaped wet strips with an outer diameter of 1.7mm on a plunger extruder, and dry the butterfly-shaped wet strips at 130°C for 4 hours to obtain a molded material carrier. Take 130 grams of the carrier, and impregnate the carrier with 140 milliliters of a mixed aqueous solution composed of ammonium molybdate, nickel nitrate and citric acid (the mixed aqueous solution contains 250 grams / liter of MoO3 and 60 grams / liter of NiO), the impregnation time is 3 hours, and the carrier is dried at 110°C for 4 hours, and the temperature is raised to 620°C at a heating rate of 180°C / h, and activated for 3 hours to obtain a hydrogenation catalyst DC6. The content of the metal oxide of the hydrogenation catalyst is shown in Table 2.

[0074] Table 1

[0075]

[0076] Note: V 中孔 Refers to the volume of mesopores with a pore distribution of 3-100 nm, in mL / g; V 大孔 Refers to the volume of macropores with pore distribution between 100-5000nm, in mL / g; V 总 Refers to the total pore volume in mL / g.

[0077] From the results in Table 1, it can be seen that the pseudo-boehmite containing phosphorus and magnesium prepared by the method of the present invention has a bimodal pore structure. The bimodal pore structure is measured by mercury intrusion, and the pore volume V of the mesopore is 3-100 nm. 中孔 The pore volume V of the macropores is 0.9-1.4 mL / g and the pore distribution is between 100-5000 nm. 大孔 1.8-2.5mL / g, total pore volume V 总 2.7-3.9 mL / g, while various pseudo-boehmite V prepared by the prior art method and the comparative example method 中孔 All below 0.7, V 大孔All are below 1, and the total pore volume V 总 All below 2.

[0078] Table 2

[0079]

[0080] Example 6

[0081] 100 mL of the hydrogenation catalysts prepared in Examples 1-5 and Comparative Examples 1-5 were crushed into particles with a diameter of 2-3 mm and then pre-sulfurized. The pre-sulfurization conditions included: the sulfiding oil used was Shanghai Changer Line diesel containing 5 w% dimethyl disulfide, and the liquid hourly volume space velocity of the sulfided oil was 1.2 h -1 , hydrogen partial pressure 14.0MPa, hydrogen-oil volume ratio 600, constant temperature vulcanization at 360℃ for 3 hours.

[0082] Then, a low-quality heavy oil (Ni content of 11 ppm, V content of 31 ppm, density of 0.973, residual carbon value of 11.9%, S content of 3.5%, N content of 0.21%) was used as raw material to evaluate the hydrogenation activity and stability of the catalyst in a 100 ml small fixed-bed reactor at a reaction temperature of 380°C, a hydrogen partial pressure of 15 MPa, and a liquid hourly space velocity of 0.6 h. -1 , the sample was taken and analyzed after 200 hours of reaction under the condition of hydrogen-to-oil volume ratio of 600. The results are shown in Table 3.

[0083] Among them, the calculation methods of the removal (Ni+V) rate, desulfurization rate and residual carbon removal rate are the same; the present invention takes the removal (Ni+V) rate as an example to exemplify the calculation method, and the removal (Ni+V) rate = ((Ni+V) content in the raw material - (Ni+V) content in the product after hydrogenation) / (Ni+V) content in the raw material.

[0084] The nickel and vanadium contents in the oil samples were determined by inductively coupled plasma emission spectrometer (ICP-AES) (the instrument used was PE-5300 plasma photometer produced by PE Company of the United States, for specific methods, see petrochemical analysis method RIPP124-90); the sulfur content in the oil samples was determined by the coulometric method (for specific methods, see petrochemical analysis method RIPP62-90); the residual carbon content in the oil samples was determined by the trace method (for specific methods, see petrochemical analysis method RIPP149-90).

[0085] Table 3

[0086] Example No. Sample name De-(Ni+V) rate / % Desulfurization rate / % Residual carbon removal rate / % Example 1 C1 80 85 60 Comparative Example 1 DC1 59 51 49 Comparative Example 2 DC2 57 61 41 Comparative Example 3 DC3 63 58 39 Example 2 C2 82 86 58 Example 3 C3 79 83 59 Comparative Example 4 DC4 61 53 40 Example 4 C4 82 84 56 Example 5 C5 83 82 59 Comparative Example 5 DC5 71 69 52 Comparative Example 6 DC6 79 84 61

[0087] It can be seen from Table 3 that the catalyst provided by the present invention has better demetallization, desulfurization and carbon removal activities under the same other conditions, and the catalyst has excellent activity and stability.

[0088] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a hydrogenation catalyst, the method comprising the following steps: (1) Preparation of pseudo-boehmite containing phosphorus and magnesium; (2) mixing the phosphorus- and magnesium-containing pseudo-boehmite with a precursor of a hydrogenation-active metal component, forming the mixture, and then drying and activating the mixture in sequence to obtain the hydrogenation catalyst; The activation conditions include: The heating rate is 50-600℃ / hour, the temperature is 400-1000℃, and the time is 1-10 hours; The hydrogenation active metal component contains at least one VIB group metal component and at least one VIII group metal component; the amount of each component is such that in the final catalyst, the content of the VIB group metal component is 0.5-50% by weight, and the content of the VIII group metal component is 0.5-20% by weight, calculated as oxide; Based on the total dry weight of the pseudo-boehmite containing phosphorus and magnesium, the content of Al2O3 is 84-99.8% by weight; the content of P2O5 is 0.1-6% by weight, and the content of MgO is 0.1-5% by weight; the pseudo-boehmite containing phosphorus and magnesium further contains optional auxiliary elements, and the auxiliary elements include metal auxiliary elements and / or non-metal auxiliary elements; the metal auxiliary elements are selected from at least one of lithium, sodium, potassium, rubidium, cesium, francium, beryllium, calcium, zirconium and titanium; the non-metal auxiliary elements are selected from at least one of boron, fluorine and silicon; the content of the auxiliary elements is 0-5% by weight; The phosphorus- and magnesium-containing alumina obtained by calcining the pseudo-boehmite at 600°C for 3 hours has a bimodal pore structure, and the bimodal pore structure is measured by mercury intrusion, and the pore distribution is located in the mesopore volume V of 3-100 nm. 中孔 The pore volume V of the macropores is 0.7-1.7 mL / g and the pore distribution is between 100-5000 nm. 大孔 The total pore volume V 总 2.4-6.4mL / g; When the catalyst is measured by a hydrogen temperature programmed reduction method (H2-TPR), the peak height P of the low temperature reduction peak at 300-500°C is 低温峰 The peak height P of the high temperature reduction peak at 650-850℃ 高温峰 The ratio S=P 低温峰 / P 高温峰 It is 0.5-2.

0.

2. The preparation method according to claim 1, wherein Based on the total dry weight of the pseudo-boehmite containing phosphorus and magnesium, the content of Al2O3 is 84-99.7% by weight; the content of the auxiliary element is 0.1-5% by weight; The pore distribution of the phosphorus and magnesium-containing aluminum oxide is located in the mesopore volume V of 3-100 nm. 中孔 The pore volume V of the macropores is 0.9-1.5 mL / g and the pore distribution is between 100-5000 nm. 大孔 1.8-3.2mL / g, total pore volume V 总 It is 2.7-4.7mL / g.

3. The preparation method according to claim 1, wherein: The peak height P of the low temperature reduction peak 低温峰 The peak height P 高温峰 The ratio S=P 低温峰 / P 高温峰 It is 0.7-1.

9.

4. The preparation method according to claim 3, wherein: The peak height P of the low temperature reduction peak 低温峰 The peak height P 高温峰 The ratio S=P 低温峰 / P 高温峰 It is 0.8-1.

8.

5. The preparation method according to claim 1, wherein: The activation conditions include: a heating rate of 100-550°C / hour and a temperature of 410-880°C; The VIB group metal component is Mo and / or W, and the VIII group metal component is Co and / or Ni; the dosage of each component is such that in the final catalyst, based on the total amount of the catalyst and calculated as oxide, the content of the VIB group metal component is 5-45% by weight, and the content of the VIII group metal component is 1-15% by weight.

6. The preparation method according to claim 5, wherein: The activation conditions include: a temperature of 430-850°C.

7. The preparation method according to claim 1, wherein: The steps of preparing the pseudo-boehmite containing phosphorus and magnesium are as follows: (a) contacting a solution of a phosphorus-containing compound, a magnesium-containing compound, or an inorganic aluminum-containing compound with an acid or a base to carry out a precipitation reaction, or contacting an organic aluminum-containing compound with a solution of a magnesium-containing compound or a phosphorus-containing compound to carry out a hydrolysis reaction, thereby obtaining a hydrated aluminum oxide containing phosphorus and magnesium; (b) aging the above-obtained phosphorus- and magnesium-containing hydrated aluminum oxide at a pH of 7-10.5, and then drying the aged solid product to obtain pseudo-boehmite containing phosphorus and magnesium; The precipitation reaction or the hydrolysis reaction in step (a) is carried out at a pH of 4-7.

8. The preparation method according to claim 7, wherein: The precipitation reaction or the hydrolysis reaction in step (a) is carried out at a pH of 4-6.5; the temperature of the precipitation reaction and the hydrolysis reaction is independently 30-90° C.; The conditions of the precipitation reaction include: the reaction temperature is 40-90°C, and the reaction time is 10-60 minutes; the conditions of the hydrolysis reaction include: the reaction temperature is 40-90°C, and the reaction time is 2-30 hours; The inorganic aluminum-containing compound is an aluminum salt and / or an aluminate; The organic aluminum-containing compound is at least one of alkoxy aluminums that can undergo a hydrolysis reaction with water to produce hydrated aluminum oxide precipitation; The phosphorus-containing compound is selected from at least one of phosphoric acid, ammonium phosphate, ammonium hydrogen phosphate, diammonium hydrogen phosphate, sodium phosphate and potassium phosphate; The magnesium-containing compound is one or more selected from magnesium chloride, magnesium nitrate, magnesium sulfate, and magnesium acetate; The acid is at least one of sulfuric acid, hydrochloric acid, nitric acid, carbonic acid, phosphoric acid, formic acid, acetic acid, citric acid and oxalic acid; The alkali is at least one of sodium aluminate, potassium aluminate, sodium hydroxide, potassium hydroxide and ammonia water.

9. The preparation method according to claim 8, wherein: The conditions of the precipitation reaction include: the reaction temperature is 45-80° C., and the reaction time is 10-30 minutes; the conditions of the hydrolysis reaction include: the reaction temperature is 45-80° C., and the reaction time is 2-20 hours.

10. The preparation method according to claim 7, wherein: The aging in step (b) is carried out at a pH of 8-10; the aging conditions include: a temperature of 50-95° C.; and a time of 0.5-8 hours; The drying conditions in step (b) include: a temperature of 50-350° C. and a drying time of 1-12 hours.

11. The preparation method according to claim 10, wherein: The aging conditions include: temperature of 55-90°C; time of 2-6 hours; The drying conditions in step (b) include: a temperature of 80-250° C. and a drying time of 2-8 hours.

12. The preparation method according to claim 7, wherein: The precipitation reaction or the hydrolysis reaction in step (a) further comprises adding a compound containing an optional auxiliary element, wherein the auxiliary element comprises a metal auxiliary element and / or a non-metal auxiliary element; The metal auxiliary element is selected from at least one of lithium, sodium, potassium, rubidium, cesium, francium, beryllium, calcium, zirconium and titanium; The non-metallic auxiliary element is selected from at least one of boron, fluorine and silicon; The amount of each component used is such that the content of Al2O3 in the obtained pseudo-boehmite containing phosphorus and magnesium is 85-99.8% by weight, the content of P2O5 is 0.1-5% by weight, the content of MgO is 0.1-5% by weight, and the content of auxiliary elements is 0-5% by weight, based on the total dry amount of the pseudo-boehmite containing phosphorus and magnesium.

13. The preparation method according to claim 12, wherein: The metal auxiliary element is selected from at least one of lithium, sodium, potassium, beryllium, calcium, zirconium and titanium; Based on the total dry weight of pseudo-boehmite containing phosphorus and magnesium, the content of Al2O3 is 85-99.7% by weight, and the content of the auxiliary element is 0.1-5% by weight.

14. A hydrogenation catalyst prepared by the method according to any one of claims 1 to 13.

15. Use of the hydrogenation catalyst according to claim 14 in hydrocarbon oil hydrogenation reaction.