A precursor material and its preparation method and application

By controlling the temperature and pH value of the co-precipitation reaction, a fluffy precursor material is prepared to form a cross-linked network cathode material, which solves the performance problems caused by the structural changes of the battery cathode material during cycling and achieves high rate and cycle stability. properties, simplifying the production process and reducing manufacturing costs.

CN116022863BActive Publication Date: 2024-10-11WUHU JIANA ENERGY TECHNOLOGY CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310153300.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-17
Publication Date
2024-10-11
Estimated Expiration
2043-02-17

AI Technical Summary

Technical Problem

Existing lithium-ion or sodium-ion battery cathode materials suffer from mechanical strain and micro-cracks due to structural changes during cycling, which affects battery performance. Single-crystal materials have weak performance at high rates and high manufacturing costs. It is difficult to balance single-crystal particles with porous structures. strength and high rate performance of polycrystalline particles.

Method used

By controlling the temperature and pH value of the co-precipitation reaction, a fluffy precursor material is prepared. The fusion of fine particles during calcination is used to form a cathode material with a cross-linked network porous structure, combining the strength of single crystal particles and polycrystalline High rate capability of particles.

Benefits of technology

It achieves excellent cycle stability and high-rate performance of the cathode material, simplifies the production process, reduces manufacturing costs, and effectively alleviates the negative impact of structural changes on battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116022863B_ABST
    Figure CN116022863B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of new energy battery materials, and specifically, to a precursor material and a preparation method and application thereof. The preparation method of the precursor material comprises: adding a mixed metal salt solution, a precipitant solution and a complexing agent solution to a base liquid to carry out a coprecipitation reaction; after the coprecipitation reaction is completed, the solid and liquid are separated to obtain a precursor material; during the coprecipitation reaction, the mixture is first reacted at a certain temperature and pH for 2 to 20 hours, and then the temperature of the mixture is reduced at a rate of ≤10°C / h, and / or the pH of the mixture is reduced at a rate of ≤2 / h. By adopting the means of cooling or lowering the pH, a precursor material with primary particles in the form of fluff is prepared, and the obtained positive electrode material has a porous structure in the form of a cross-linked network, which has the high rate performance of polycrystalline particles while having the strong structure of single crystal particles, and the porous structure can effectively alleviate the damage to the structure caused by strain, and has excellent electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy battery materials, and specifically, to a precursor material and a preparation method and application thereof; more specifically, to a precursor material and a preparation method thereof, a positive electrode material, a positive electrode sheet and a battery. Background Art

[0002] The positive electrode material determines the energy density, power and life of lithium-ion batteries or sodium-ion batteries, but the repeated ion insertion or extraction in the positive electrode particles leads to serious structural changes, which seriously affects the performance of the battery. The common polycrystalline positive electrode materials are filled with a large number of grain boundaries between the primary particles, which helps to achieve high-rate battery performance, but the material is prone to phase change during long-term cycles, resulting in anisotropic shrinkage / expansion of the layered structure, causing severe mechanical strain in the crystal, inducing the formation of microcracks, and causing the breakage of the positive electrode material particles. The structure of single-crystal positive electrode materials is stable, but the large single-crystal particles of micron size increase the transmission distance of lithium / sodium ions, resulting in weaker rate performance, and the calcination temperature is usually very high, which makes the manufacturing cost high, all of which seriously restrict its application in more large-scale areas.

[0003] Therefore, in order to develop layered cathode materials with excellent performance and high crystal structure strength for lithium or sodium ion batteries, researchers have proposed to improve the battery performance by ion doping / replacing the cathode materials to modify the lattice and surface coating to strengthen the peripheral structure. However, the current modification methods do not combine the strong particle structure characteristics of single crystal cathode materials, the advantages of porous structures that effectively suppress microcracks, and the advantages of high-rate battery performance of polycrystalline particles to prepare high-performance cathode materials.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The first purpose of the present invention is to provide a method for preparing a precursor material. Based on the growth control of the precursor material, a precursor material with fluffy primary particles is prepared by cooling or lowering the growth pH. The mutual fusion and shrinkage of the fluffy primary particles during calcination are utilized. Without the need for excessively high temperature calcination of conventional single crystal positive electrode materials or additional molten salt-assisted calcination, a positive electrode material with no obvious grain boundaries and a porous structure with a cross-linked network inside can be obtained. The positive electrode material has the strong structure of single crystal particles and the high rate performance of polycrystalline particles. The porous structure can effectively alleviate the damage to the structure caused by strain, thereby exhibiting excellent battery performance.

[0006] The second object of the present invention is to provide a precursor material having excellent cycle stability and high rate performance.

[0007] The third object of the present invention is to provide a positive electrode material having good cycle stability.

[0008] The fourth object of the present invention is to provide a positive electrode plate.

[0009] A fifth object of the present invention is to provide a battery.

[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0011] In a first aspect, the present invention provides a method for preparing a precursor material, comprising the following steps:

[0012] A mixed metal salt solution, a precipitant solution and a complexing agent solution are added to the base solution to carry out a coprecipitation reaction; after the coprecipitation reaction is completed, the solid and the liquid are separated to obtain the precursor material.

[0013] Among them, the metal elements in the mixed metal salt solution include at least two of Ni element, Co element, Mn element and doped metal elements, such as a mixture of Ni element and doped metal elements, a mixture of Co element and doped metal elements, a mixture of Mn element and doped metal elements, a mixture of Ni element and Mn element, a mixture of Ni element and Co element, or a mixture of Ni element, Mn element and doped metal elements, etc., but not limited to these.

[0014] The doping metal elements include at least one of La, Al, Ti, Ta, Mg, Mo, W, Ca, Zn, Nb, Cr, Zr and Fe elements, and two, three or five elements may also be selected.

[0015] During the coprecipitation reaction, the mixture is first reacted at a certain temperature and pH for 2 to 20 hours (including but not limited to any one of 5 hours, 8 hours, 10 hours, 13 hours, 15 hours, and 18 hours or a range between any two of them), and then the temperature of the mixture is reduced at a cooling rate of ≤10°C / h (including but not limited to any one of 9°C / h, 8°C / h, 5°C / h, 4°C / h, 3°C / h, 2°C / h, 1°C / h, 0.8°C / h, 0.6°C / h, 0.5°C / h, 0.3°C / h, 0.4°C / h, 0.2°C / h, 0.1°C / h, and 0.01°C / h or a range between any two of them), preferably at a cooling rate of 0.1°C / h to 1°C / h, until the coprecipitation reaction is completed or the temperature reaches the lower limit (e.g., 20°C).

[0016] And / or, the pH of the mixed material is reduced at a rate of ≤2 / h (including but not limited to any point value of 1.7 / h, 1.5 / h, 1.0 / h, 0.8 / h, 0.5 / h, 0.3 / h, 0.1 / h, 0.08 / h, 0.06 / h, 0.05 / h, 0.03 / h, 0.02 / h, 0.01 / h or any range value between two thereof), preferably at a pH reduction rate of 0.01 / h to 1 / h, until the coprecipitation reaction is completed or the pH reaches the lower limit value (e.g. 9.5).

[0017] That is, the coprecipitation reaction is first carried out while keeping the temperature and pH of the reaction system unchanged. After a period of time, the temperature of the reaction system (i.e., the temperature of the mixed material) is reduced at a rate of ≤10°C per hour, and / or the pH of the reaction system (i.e., the pH of the mixed material) is reduced at a rate of ≤2°C per hour.

[0018] The present invention is based on the growth control of the precursor material, and adopts the means of cooling at a specific rate or lowering the growth pH to prepare a precursor material with primary particles in the form of fluff. The positive electrode material prepared by using the precursor material has a cross-linked network-like porous structure inside, which has both the strong structure of single crystal particles and the high rate performance of polycrystalline particles. The porous structure can effectively alleviate the damage to the structure caused by strain, and exhibits excellent electrochemical performance.

[0019] Compared with the prior art, the present invention only needs to simply and skillfully control the temperature and pH value of the coprecipitation reaction system, so that the growth of the precursor material is always in the process of becoming thinner, making it difficult for the primary particles on the surface to aggregate and grow into coarser primary particles, thereby preparing a precursor material with fluffy primary particles.

[0020] Therefore, the preparation method of the precursor material provided by the present invention is simple, and the temperature setting, pH value change and the detection operation of the two are simpler. The problems of complex detection and reduced production capacity caused by changing the reaction conditions by limiting the particle size can be eliminated, thereby improving production efficiency and facilitating mass production.

[0021] In addition, the precursor material prepared by the present invention is used for the back-end preparation of high-performance lithium battery positive electrode materials or sodium battery positive electrode materials, and the unique structure exhibited can effectively alleviate the negative impact of serious structural changes in particles during the use of positive electrode materials on battery performance.

[0022] Preferably, during the coprecipitation reaction, the temperature of the mixed material is 20-75°C, including but not limited to any point value of 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C or a range value between any two of them.

[0023] And / or, during the coprecipitation reaction, the pH of the mixed material is 9.5-12.3, including but not limited to any point value of 9.8, 10.0, 10.3, 10.5, 10.8, 11.0, 11.3, 11.5, 11.8, 12.0 or a range between any two of them.

[0024] Preferably, the coprecipitation reaction is carried out to a solid particle size of D50 = 3-17 μm, including but not limited to any point value of 5 μm, 7 μm, 9 μm, 10 μm, 12 μm, 14 μm, 15 μm or a range value between any two of them; or, the total reaction time of the coprecipitation reaction is 25-90 h, including but not limited to any point value of 30 h, 35 h, 40 h, 45 h, 50 h, 55 h, 60 h, 65 h, 70 h, 75 h, 80 h, 85 h or a range value between any two of them.

[0025] Preferably, the precipitant solution comprises potassium hydroxide solution and / or sodium hydroxide solution.

[0026] Preferably, the complexing agent solution includes at least one of a sodium oxalate solution, an ammonia solution, a citric acid solution and a disodium ethylenediaminetetraacetic acid solution.

[0027] The base liquid is mainly prepared from at least one of water, the precipitant solution and the complexing agent solution. For example, the base liquid can be made of pure water alone, or a precipitant solution alone, or a complexing agent solution alone, or can be prepared by mixing water, a precipitant solution and a complexing agent solution at the same time.

[0028] In some specific embodiments of the present invention, the anions in the mixed metal salt solution include at least one of nitrate ions, sulfate ions and chloride ions.

[0029] In some specific embodiments of the present invention, after the solid-liquid separation, the steps of washing and drying are further included.

[0030] In a second aspect, the present invention provides a precursor material, which is mainly prepared by the preparation method of the precursor material as described above.

[0031] Wherein, the chemical formula of the precursor material is Ni x Co y Mn z M e (OH)2; wherein 0≤x<1, 0≤y<1, 0≤z<1, 0≤e<1, and x+y+z+e=1.

[0032] M refers to a doping metal element, and M includes at least one of La, Al, Ti, Ta, Mg, Mo, W, Ca, Zn, Nb, Cr, Zr and Fe.

[0033] The precursor material prepared by the present invention can effectively alleviate the negative impact of serious structural changes in particles of the positive electrode material during use on battery performance, so it has excellent electrochemical properties, especially excellent cycle stability.

[0034] Preferably, the shape of the primary particles of the precursor material includes villi (or filaments); wherein the precursor material includes secondary particles formed by aggregation of primary particles.

[0035] Preferably, the length of the primary particles of the precursor material is less than 1 μm, including but not limited to any point value of 0.8 μm, 0.5 μm, 0.3 μm, 0.1 μm, 0.05 μm, 0.01 μm or a range value between any two of them.

[0036] The thickness of the primary particles of the precursor material is less than 100 nm, including but not limited to any point value of 80 nm, 60 nm, 50 nm, 30 nm, 10 nm, 5 nm, 1 nm, or a range value between any two of them.

[0037] The primary particles of the precursor material prepared by the present invention are relatively fine, so the positive electrode material prepared therefrom has a porous structure in the form of a cross-linked network, thereby exhibiting excellent electrochemical performance.

[0038] In a third aspect, the present invention provides a positive electrode material, which is mainly obtained by uniformly mixing the precursor material as described above with a sodium source or a lithium source and then calcining the mixture.

[0039] That is, the preparation method of the positive electrode material includes: uniformly mixing the precursor material with the sodium source or the lithium source, and then calcining to obtain the positive electrode material.

[0040] In some specific embodiments of the present invention, the molar ratio of the precursor material to the sodium element in the sodium source is 1:0.65-1.18, including but not limited to any point value of 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1 or a range value between any two of them.

[0041] In some specific embodiments of the present invention, the molar ratio of the precursor material to the lithium element in the lithium source is 1:1.0-1.6, including but not limited to any point value of 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5 or a range value between any two of them.

[0042] The positive electrode material includes secondary particles in a cross-linked network formed by aggregation of primary particles; the interior of the secondary particles has a honeycomb porous structure.

[0043] A simple and effective high-temperature calcination is used to supplement lithium or sodium. The precursor material is used so that the tiny primary particles are more easily fused and cross-linked into a network during calcination. While the primary particles are fused, they are away from each other to form a unique void structure. Finally, a honeycomb positive electrode material is obtained in which the internal primary particles are cross-linked, the particles are rich in porous buffer layers to isolate crack extension, and the grain boundaries between the grains are not obvious. The honeycomb positive electrode material exhibits excellent cycle performance as a lithium battery positive electrode material or a sodium battery positive electrode material, and exhibits high capacity at a high rate of 5C.

[0044] Preferably, the sodium source includes at least one of sodium oxide, sodium carbonate, sodium sulfate, sodium nitrate, sodium acetate, sodium hydroxide, sodium oxalate and sodium chloride.

[0045] Preferably, the lithium source includes at least one of lithium oxide, lithium carbonate, lithium sulfate, lithium nitrate, lithium acetate, lithium hydroxide, lithium oxalate and lithium chloride.

[0046] Preferably, the calcination temperature is 400-1000°C, including but not limited to any one of 500°C, 600°C, 700°C, 800°C, 900°C or a range between any two of them.

[0047] The calcination holding (total) time is 4 to 22 hours, including but not limited to any one of 5 hours, 7 hours, 9 hours, 10 hours, 13 hours, 15 hours, 18 hours, and 20 hours, or a range between any two of them.

[0048] In some specific embodiments of the present invention, the calcination may be performed in one stage or in multiple stages.

[0049] In a fourth aspect, the present invention provides a positive electrode plate, which is mainly made of the positive electrode material as described above.

[0050] In a fifth aspect, the present invention provides a battery comprising the positive electrode plate as described above; wherein the battery comprises a lithium ion battery and / or a sodium ion battery.

[0051] The battery has excellent electrochemical performance, especially good cycle performance.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] (1) The method for preparing the precursor material provided by the present invention controls the temperature and pH value of the coprecipitation reaction system so that the growth of the precursor material is always in the process of becoming thinner. The primary particles of the obtained precursor material are in a fluffy shape. The precursor material is used for the back-end preparation of high-performance lithium battery positive electrode materials or sodium battery positive electrode materials. The unique structure exhibited can effectively alleviate the negative impact of serious structural changes in the particles during the use of the positive electrode material on the battery performance, and has excellent electrochemical properties.

[0054] (2) The present invention provides a special precursor material, whose primary particles are in a fluffy state. The primary particles are porous and have a higher specific surface area. When mixed with Li / Na salt and calcined, the fluffy primary particles fuse with each other to form a cross-linked state and shrink with each other to easily form a porous form. This primary particle morphology is the key to preparing special structure positive electrode materials.

[0055] (3) The cathode material provided by the present invention has a honeycomb porous structure inside the secondary particles, which has both the strong structure of single crystal particles and the high rate performance of polycrystalline particles. As a cathode material for lithium batteries or sodium batteries, it exhibits excellent cycling performance and high capacity at a high rate of 5C. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0057] Figure 1 Ni prepared in Example 1 of the present invention 0.6 Co 0.1 Mn 0.3 FESEM image of (OH)2 precursor material;

[0058] Figure 2 LiNi prepared in Example 1 of the present invention 0.6 Co 0.1 Mn 0.3 FESEM image of the outer surface of the O2 cathode material;

[0059] Figure 3 LiNi prepared in Example 1 of the present invention 0.6 Co 0.1 Mn 0.3 FESEM image of the cross section of the O2 cathode material;

[0060] Figure 4Ni prepared in Example 2 of the present invention 0.38 Mn 0.62 FESEM image of (OH)2 precursor material;

[0061] Figure 5 The Na obtained in Example 2 of the present invention 0.9 Ni 0.38 Mn 0.62 FESEM image of the outer surface of the O2 cathode material;

[0062] Figure 6 The Na obtained in Example 2 of the present invention 0.9 Ni 0.38 Mn 0.62 FESEM image of the cross section of the O2 cathode material;

[0063] Figure 7 Ni prepared in Comparative Example 1 of the present invention 0.6 Co 0.1 Mn 0.3 FESEM image of (OH)2 precursor material;

[0064] Figure 8 LiNi prepared in Comparative Example 1 of the present invention 0.6 Co 0.1 Mn 0.3 FESEM image of the outer surface of the O2 cathode material;

[0065] Fig. 9 LiNi prepared in Comparative Example 1 of the present invention 0.6 Co 0.1 Mn 0.3 FESEM image of the cross section of O2 positive electrode material. DETAILED DESCRIPTION

[0066] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0067] Example 1

[0068] The Ni provided in this embodiment 0.6 Co 0.1 Mn 0.3(OH)2 Precursor Materials and LiNi 0.6 Co 0.1 Mn 0.3 The preparation method of O2 positive electrode material comprises the following steps:

[0069] (1) nickel sulfate, cobalt sulfate, and manganese sulfate were weighed in a molar ratio of Ni:Co:Mn=60:10:30, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 2.4 mol / L; sodium hydroxide was dissolved in pure water to prepare a sodium hydroxide solution with a molar concentration of 10.2 mol / L (as a precipitant solution); and an ammonia solution with a mass fraction of 23% was prepared as a complexing agent solution;

[0070] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, ammonia solution and sodium hydroxide solution are fed in parallel, wherein the feeding rate of the sodium hydroxide solution is based on the stable pH at 11.7, and the stability of the feeding of the ammonia solution and the mixed metal salt solution is maintained, and the flow rate ratio of the ammonia solution and the mixed metal salt solution is maintained at 1:58, and they are added in parallel to the coprecipitation kettle containing a 55°C bottom liquid (pure water), and the coprecipitation kettle is stirred continuously, and the temperature of the mixed material is controlled at 55°C to carry out precipitation reaction; after the coprecipitation reaction is carried out for 9 hours, the feeding rate of the sodium hydroxide solution is changed to ensure that the pH value decreases by 0.1 every 3 hours (that is, the rate of reducing the pH is 0.033 / h); at the same time, the temperature of the mixed material in the reactor is adjusted to ensure that the temperature of the mixed material decreases by 1°C every 3 hours (that is, the cooling rate is 0.33°C / h).

[0071] (3) When the total reaction time reaches 65 h, the D50 particle size of the solid particles in the reactor reaches 10 μm, the feed is stopped, the reaction is completed, and then the solid and liquid are separated to obtain very fine primary particles of Ni in the form of fluff. 0.6 Co 0.1 Mn 0.3 (OH)2 precursor material.

[0072] (4) The above Ni 0.6 Co 0.1 Mn 0.3 The (OH)2 precursor material and lithium hydroxide were weighed and mixed in a molar ratio of 1:1.03, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 450°C at a rate of 2°C / min and kept for 5 hours, then continued to be heated to 800°C and kept for 15 hours. Finally, the furnace was cooled to room temperature to obtain secondary particles in the form of a cross-linked network formed by aggregation of primary particles, and the secondary particles had a honeycomb porous structure of LiNi 0.6 Co 0.1 Mn 0.3 O2 positive electrode material.

[0073] like Figure 1 Shown is the FESEM image of the precursor material prepared in Example 1; Figure 2 This is a FESEM image of the outer surface of the positive electrode material prepared in Example 1. Figure 3 This is a FESEM image of the cross section of the positive electrode material obtained in Example 1. Figure 1 It can be seen that the primary particles of the precursor are relatively fine and closely connected, with a primary particle length of about 500 nm and a thickness of about 30 nm. Figure 2 The primary particle size of the positive electrode material surface obtained by calcination is also relatively small, which is conducive to the rapid diffusion of lithium ions; Figure 3 From the cross-sectional view in the figure, we can see that the primary particles are cross-linked to form a network structure, no obvious independent grain boundaries are generated, and there are abundant pore structures inside.

[0074] Example 2

[0075] The Ni provided in this embodiment 0.38 Mn 0.62 (OH)2 precursor materials and Na 0.9 Ni 0.38 Mn 0.62 The preparation method of O2 positive electrode material comprises the following steps:

[0076] (1) nickel sulfate and manganese sulfate were weighed in a molar ratio of Ni:Mn=38:62, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 2.5 mol / L; sodium hydroxide was dissolved in pure water to prepare a sodium hydroxide solution with a molar concentration of 9.5 mol / L; and an ammonia solution with a concentration of 20% was prepared as a complexing agent solution;

[0077] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, ammonia solution and sodium hydroxide solution are fed in parallel. The feeding rate of the sodium hydroxide solution is based on the stable pH at 10.9, and the stability of the feeding of the ammonia solution and the mixed metal salt solution is maintained. The flow rate ratio of the ammonia solution and the mixed metal salt solution is maintained at 1:70, and the mixed metal salt solution is added in parallel to the coprecipitation kettle containing a 35°C bottom liquid, wherein the bottom liquid is a mixed solution of ammonia solution and sodium hydroxide solution (pH is 10.9, wherein the ammonia concentration is 0.23 mol / L), the coprecipitation kettle is stirred continuously, the temperature of the mixed material is controlled at 35°C, and a precipitation reaction is carried out; after the coprecipitation reaction is carried out for 20 hours, the feeding rate of the sodium hydroxide solution is changed to ensure that the pH decreases by 0.07 every 3 hours (i.e., the rate of reducing the pH is 0.023 / h).

[0078] (3) When the total reaction time reaches 63 h, the D50 particle size of the solid particles in the reactor reaches 10 μm, the feed is stopped, the reaction is completed, and then the solid and liquid are separated to obtain very fine primary particles of Ni in the form of fluff. 0.38 Mn 0.62 (OH)2 precursor material.

[0079] (4) The above Ni 0.38 Mn 0.62 The (OH)2 precursor material and sodium carbonate were weighed and mixed in a molar ratio of 1:0.452, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 500°C at a rate of 2°C / min and kept for 5 hours, then continued to be heated to 900°C and kept for 16 hours. Finally, the furnace was cooled to room temperature to obtain secondary particles in the form of a cross-linked network formed by aggregation of primary particles, and the secondary particles had a honeycomb porous structure of Na 0.9 Ni 0.38 Mn 0.62 O2 positive electrode material.

[0080] like Figure 4 Shown is the FESEM image of the precursor material prepared in Example 2; Figure 5 This is a FESEM image of the outer surface of the positive electrode material prepared in Example 2. Figure 6 This is a FESEM image of the cross section of the positive electrode material obtained in Example 2. Figure 4 It can be seen that the primary particles of the precursor are relatively fine and the particles are closely connected. The length of the primary particles is about 360nm and the thickness is about 21nm. Figure 5 It can be seen that the primary particle size of the positive electrode material obtained by calcination is small, which is conducive to the rapid diffusion of sodium ions; from the cross-section of the positive electrode material ( Figure 6 ) It can be observed that the primary particles are cross-linked to form a network honeycomb structure, the grain boundaries between the primary particles are not obvious, and the internal pores are abundant.

[0081] Example 3

[0082] The Ni provided in this embodiment 0.25 Mn 0.75 (OH)2 precursor materials and Li 1.2 Ni 0.2 Mn 0.6 The preparation method of O2 positive electrode material comprises the following steps:

[0083] (1) nickel sulfate and manganese sulfate were weighed in a molar ratio of Ni:Mn=25:75, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 1.5 mol / L; sodium hydroxide was dissolved in pure water to prepare a sodium hydroxide solution with a molar concentration of 7.9 mol / L; and a sodium oxalate solution with a concentration of 1.8 mol / L was prepared as a complexing agent solution;

[0084] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, sodium oxalate solution, and sodium hydroxide solution are fed in parallel. The feeding rate of the sodium hydroxide solution is based on the stable pH at 9.8, and the stability of the sodium oxalate solution and the mixed metal salt solution is maintained. The flow rate ratio of the sodium oxalate solution to the mixed metal salt solution is maintained at 1:50, and they are added in parallel to the coprecipitation kettle containing a 70°C bottom liquid, wherein the bottom liquid is a mixed solution of sodium oxalate solution and sodium hydroxide solution (pH is 9.8, wherein the molar concentration of sodium oxalate is 0.5 mol / L), and the coprecipitation kettle is continuously stirred, and the temperature of the mixed material is controlled at 70°C to carry out a precipitation reaction; after the coprecipitation reaction is carried out for 2 hours, the temperature of the mixed material is changed to ensure that the temperature of the mixed material decreases by 3°C every 5 hours (i.e., the cooling rate is 0.6°C / h), while maintaining the pH stability.

[0085] (3) When the total reaction time reaches 67 h, the D50 particle size of the solid particles in the reactor reaches 10 μm, the feed is stopped, the reaction is completed, and then the solid and liquid are separated to obtain very fine primary particles of Ni in the form of fluff. 0.25 Mn 0.75 (OH)2 precursor material.

[0086] (4) The above Ni 0.25 Mn 0.75 The (OH)2 precursor material and lithium carbonate were weighed and mixed in a molar ratio of 0.8:0.615, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 500°C at a rate of 2°C / min and kept at this temperature for 5 hours, and then continued to be heated to 880°C and kept at this temperature for 15 hours. Finally, the mixture was cooled to room temperature with the furnace to obtain secondary particles in the form of a cross-linked network formed by the aggregation of primary particles, and the secondary particles had a honeycomb porous structure of Li 1.2 Ni 0.2 Mn 0.6 O2 positive electrode material.

[0087] Example 4

[0088] The Ni provided in this embodiment 0.9 Co 0.1 (OH)2 Precursor Materials and LiNi 0.9 Co 0.1 The preparation method of O2 positive electrode material comprises the following steps:

[0089] (1) nickel acetate and cobalt sulfate crystals are weighed at a molar ratio of Ni:Co=90:10, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 2.5 mol / L; potassium hydroxide is dissolved in pure water to prepare a potassium hydroxide solution with a molar concentration of 9.5 mol / L; and a citric acid solution with a concentration of 0.9 mol / L is prepared as a complexing agent solution;

[0090] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, citric acid solution, and potassium hydroxide solution are fed in parallel. The feeding rate of the potassium hydroxide solution is based on the stable pH at 11.0, and the stability of the feeding of the citric acid solution and the mixed metal salt solution is maintained. The flow rate ratio of the citric acid solution to the mixed metal salt solution is maintained at 1:43, and the mixed metal salt solution is added in parallel to the coprecipitation kettle containing a 50°C bottom liquid, wherein the bottom liquid is a mixed solution of citric acid solution and sodium hydroxide solution (pH is 11.0, wherein the molar concentration of citric acid is 0.3 mol / L). The coprecipitation kettle is stirred continuously, and the temperature of the mixed material is controlled at 50°C to carry out a precipitation reaction; after the coprecipitation reaction is carried out for 7 hours, the feeding rate of the potassium hydroxide solution is changed to ensure that the pH decreases by 0.1 every 7 hours (i.e., the pH reduction rate is 0.014 / h); at the same time, the temperature of the mixed material is changed to ensure that the temperature of the mixed material decreases by 0.5°C every 5 hours (i.e., the cooling rate is 0.1°C / h).

[0091] (3) When the total reaction time reaches 86 h, the D50 particle size of the solid particles in the reactor reaches 10 μm, the feed is stopped, the reaction is completed, and then the solid and liquid are separated to obtain a very fine, fluffy Ni 0.9 Co 0.1 (OH)2 precursor material.

[0092] (4) The above Ni 0.9 Co 0.1 The (OH)2 precursor material and lithium hydroxide were weighed and mixed in a molar ratio of 1:1.05, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 500°C at a rate of 3°C / min and kept for 5 hours, then continued to be heated to 730°C and kept for 14 hours. Finally, the furnace was cooled to room temperature to obtain secondary particles in the form of a cross-linked network formed by aggregation of primary particles, and the secondary particles had a honeycomb porous structure of LiNi 0.9 Co 0.1 O2 positive electrode material.

[0093] Example 5

[0094] The Ni provided in this embodiment 0.79 Mn 0.2 Al 0.01(OH)2 Precursor Materials and LiNi 0.79 Mn 0.2 Al 0.01 The preparation method of O2 positive electrode material comprises the following steps:

[0095] (1) Nickel sulfate, manganese nitrate, and ammonium tungstate crystals are weighed according to a molar ratio of Ni:Mn:Al=79:20:1, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 1.3 mol / L; sodium hydroxide is dissolved in pure water to prepare a sodium hydroxide solution with a molar concentration of 7.5 mol / L; and an ammonia solution with a mass fraction of 15% is prepared as a complexing agent solution.

[0096] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, ammonia solution and sodium hydroxide solution are fed in parallel. The feeding rate of the sodium hydroxide solution is based on the stable pH at 10.9, and the stability of the feeding of the ammonia solution and the mixed metal salt solution is maintained. The flow rate ratio of the ammonia solution and the mixed metal salt solution is maintained at 1:36, and they are added in parallel to the coprecipitation kettle containing a 55°C bottom liquid, wherein the bottom liquid is an ammonia solution with a molar concentration of 0.1 mol / L. The coprecipitation kettle is stirred continuously, and the temperature of the mixed material is controlled at 55°C to carry out a precipitation reaction; after the coprecipitation reaction is carried out for 7 hours, the temperature of the mixed material is adjusted to decrease by 2°C every 6 hours (i.e., the cooling rate is 0.33°C / h).

[0097] (3) When the total reaction time reaches 78 h, the D50 particle size of the solid particles in the reactor reaches 10 μm, the feed is stopped, the reaction is completed, and then the solid and liquid are separated to obtain a very fine, fluffy Ni 0.79 Mn 0.2 Al 0.01 (OH)2 precursor material.

[0098] (4) The above Ni 0.79 Mn 0.2 Al 0.01 The (OH)2 precursor material and lithium hydroxide were weighed and mixed in a molar ratio of 1:1.06, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 460°C at a rate of 4°C / min and kept for 4 hours, then continued to be heated to 750°C and kept for 16 hours. Finally, the furnace was cooled to room temperature to obtain secondary particles in the form of a cross-linked network formed by aggregation of primary particles, and the secondary particles had a honeycomb porous structure of LiNi 0.79 Mn 0.2 Al 0.01 O2 positive electrode material.

[0099] Example 6

[0100] The Ni provided in this embodiment0.33 Mg 0.17 Mn 0.5 (OH)2 precursor materials and NaNi 0.33 Mg 0.17 Mn 0.5 The preparation method of O2 positive electrode material comprises the following steps:

[0101] (1) Nickel sulfate, manganese nitrate, and magnesium sulfate crystals are weighed in a molar ratio of Ni:Mn:Mg=33:50:17, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 1.7 mol / L; sodium hydroxide is dissolved in pure water to prepare a sodium hydroxide solution with a molar concentration of 6.5 mol / L; and a disodium ethylenediaminetetraacetic acid solution with a concentration of 0.9 mol / L is prepared as a complexing agent solution.

[0102] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, disodium ethylenediaminetetraacetic acid solution, and sodium hydroxide solution are fed in parallel, the feeding rate of the sodium hydroxide solution is based on the stable pH at 9.9, and the stability of the feeding of disodium ethylenediaminetetraacetic acid solution and the mixed metal salt solution is maintained, and the flow rate ratio of the disodium ethylenediaminetetraacetic acid solution to the mixed metal salt solution is maintained at 1:38, and they are added in parallel to the coprecipitation kettle containing a 60°C bottom liquid, wherein the bottom liquid is a disodium ethylenediaminetetraacetic acid solution with a molar concentration of 0.7 mol / L, and the coprecipitation kettle is stirred continuously, and the temperature of the mixed material is controlled at 60°C to carry out a precipitation reaction; after the coprecipitation reaction is carried out for 5 hours, the temperature of the mixed material is set to decrease by 3°C every 5 hours (i.e., the cooling rate is 0.6°C / h) until the temperature drops to 29°C, and the cooling is stopped to continue the reaction.

[0103] (3) When the total reaction time reaches 58 h, when the D50 particle size of the solid particles in the reactor reaches 5.5 μm, the feed is stopped, the reaction is completed, and then the solid-liquid separation is performed to obtain a very fine, fluffy Ni 0.33 Mg 0.17 Mn 0.5 (OH)2 precursor material.

[0104] (4) The above Ni 0.33 Mg 0.17 Mn 0.5 The (OH)2 precursor material and sodium carbonate were weighed and mixed in a molar ratio of 1:0.53, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 460°C at a rate of 4°C / min and kept for 6 hours, then continued to be heated to 870°C and kept for 14 hours. Finally, the furnace was cooled to room temperature to obtain secondary particles in the form of a cross-linked network formed by aggregation of primary particles, and the secondary particles had a honeycomb porous structure of NaNi 0.33 Mg 0.17Mn 0.5 O2 positive electrode material.

[0105] Example 7

[0106] The Ni provided in this embodiment 0.334 Fe 0.333 Mn 0.333 (OH)2 precursor materials and Na 0.7 Ni 0.334 Fe 0.333 Mn 0.333 The preparation method of O2 positive electrode material comprises the following steps:

[0107] (1) Nickel sulfate, ferrous sulfate, and manganese sulfate were weighed in a molar ratio of Ni:Fe:Mn=33.4:33.3:33.3, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 1.8 mol / L; sodium hydroxide was dissolved in pure water to prepare a sodium hydroxide solution with a molar concentration of 7.5 mol / L; and an ammonium oxalate solution with a concentration of 1.2 mol / L was prepared as a complexing agent solution.

[0108] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, ammonium oxalate solution, and sodium hydroxide solution are fed in parallel. The feeding rate of the sodium hydroxide solution is based on the stable pH at 10.7, and the stability of the feeding of the ammonium oxalate solution and the mixed metal salt solution is maintained. The flow rate ratio of the ammonium oxalate solution to the mixed metal salt solution is maintained at 1:21, and they are added in parallel to the coprecipitation kettle containing a 70°C bottom liquid, wherein the bottom liquid is an ammonium oxalate solution with a molar concentration of 0.4 mol / L. The coprecipitation kettle is stirred continuously, and the temperature of the mixed material is controlled at 70°C to carry out a precipitation reaction; after the coprecipitation reaction is carried out for 5 hours, the temperature of the mixed material is set to decrease by 2°C every 5 hours (i.e., the cooling rate is 0.4°C / h) until the temperature drops to 40°C, and the cooling is stopped to continue the reaction.

[0109] (3) When the D50 particle size of the solid particles in the reactor reaches 7.5 μm, the feed is stopped, the reaction ends, and then the solid and liquid are separated to obtain very fine, fluffy Ni 0.334 Fe 0.333 Mn 0.333 (OH)2 precursor material.

[0110] (4) The above Ni 0.334 Fe 0.333 Mn 0.333The (OH)2 precursor material and sodium carbonate were weighed and mixed in a molar ratio of 1:0.361, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 450°C at a rate of 4°C / min and kept for 6 hours, then continued to be heated to 880°C and kept for 14 hours. Finally, the furnace was cooled to room temperature to obtain secondary particles in the form of a cross-linked network formed by aggregation of primary particles, and the secondary particles had a honeycomb porous structure of Na 0.7 Ni 0.334 Fe 0.333 Mn 0.333 O2 positive electrode material.

[0111] Example 8

[0112] The Ni provided in this embodiment 0.5 Mn 1.5 (OH)4 Precursor Materials and LiNi 0.5 Mn 1.5 The preparation method of O4 positive electrode material comprises the following steps:

[0113] (1) nickel acetate and manganese sulfate crystals are weighed in a molar ratio of Ni:Mn=5:15, and dissolved in a batching tank to prepare a mixed metal salt solution with a total metal concentration of 2.0 mol / L; potassium hydroxide is dissolved in pure water to prepare a potassium hydroxide solution with a molar concentration of 10 mol / L; and an ammonia solution with a mass fraction of 20% is prepared as a complexing agent solution;

[0114] (2) nitrogen is continuously introduced into the coprecipitation kettle, and the mixed metal salt solution, ammonia solution and potassium hydroxide solution are fed in parallel, the feeding rate of potassium hydroxide solution is based on the stable pH at 11.5, and the stability of the feeding of ammonia solution and mixed metal salt solution is maintained, and the flow rate ratio of ammonia solution and mixed metal salt solution is maintained at 1:78, and they are added in parallel to the coprecipitation kettle containing a 65°C bottom liquid, wherein the bottom liquid is an ammonia solution with a molar concentration of 0.15 mol / L, and the coprecipitation kettle is stirred continuously, and the temperature of the mixed material is controlled at 65°C to carry out precipitation reaction; after the coprecipitation reaction is carried out for 17 hours, the feeding rate of potassium hydroxide solution is changed to ensure that the pH of the mixed material decreases by 0.1 every 5 hours (i.e., the pH reduction rate is 0.02 / h), and the temperature of the mixed material decreases by 1°C every 2 hours (i.e., the cooling rate is 0.5°C / h); wherein, when the pH of the mixed material decreases to 10.3, the pH no longer changes, and the temperature is ensured to be not lower than 35°C.

[0115] (3) When the D50 particle size of the solid particles in the reactor reaches 5.5 μm, the feed is stopped, the reaction ends, and then the solid and liquid are separated to obtain very fine, fluffy Ni 0.5 Mn 1.5 (OH)4 precursor material.

[0116] (4) The above Ni 0.5 Mn 1.5 The (OH)4 precursor material and lithium carbonate were weighed and mixed in a molar ratio of 1:0.536, and then heated and calcined in an air atmosphere. The temperature was raised from room temperature to 600°C at a rate of 5°C / min and kept for 5 hours, then continued to be heated to 910°C and kept for 17 hours. Finally, the furnace was cooled to room temperature to obtain secondary particles in the form of a cross-linked network formed by aggregation of primary particles, and the secondary particles had a honeycomb porous structure of LiNi 0.5 Mn 1.5 O4 positive electrode material.

[0117] Comparative Example 1

[0118] The Ni provided in this comparative example 0.6 Co 0.1 Mn 0.3 (OH)2 Precursor Materials and LiNi 0.6 Co 0.1 Mn 0.3 The preparation method of the O2 positive electrode material is basically the same as that in Example 1, with the only difference being that in step (2), during the coprecipitation reaction, the temperature (55°C) and pH (11.7) of the mixed material are kept unchanged (until the D50 particle size of the solid particles in the reactor reaches 10 μm).

[0119] like Figure 7 Shown is the FESEM image of the precursor material prepared in this comparative example 1; Figure 8 This is a FESEM image of the outer surface of the positive electrode material prepared in this comparative example 1. Fig. 9 This is a FESEM image of the cross section of the positive electrode material obtained in this comparative example 1. Figure 7 It can be seen that the primary particles of the precursor prepared in this comparative example are relatively coarse, and the gaps between the primary particles are obvious. The length of the primary particles is about 1050nm and the thickness is about 320nm. Figure 8 It can be seen that the primary particles of the calcined positive electrode material are larger in size, which is due to the fact that the positive electrode material particles inherit the characteristics of the precursor primary particles. Fig. 9 From the cross-sectional diagram in the figure, we can see that the primary particles are closely packed together, the internal space has a small number of pores that are too large, and the distribution is extremely uneven. After multiple lithium ion insertion / removal, it is easy to form uneven stress between the primary particles, causing the particles to break.

[0120] Comparative Example 2

[0121] The Ni provided in this comparative example 0.6 Co 0.1 Mn 0.3 (OH)2 Precursor Materials and LiNi0.6 Co 0.1 Mn 0.3 The preparation method of O2 positive electrode material is basically the same as that in Example 1, with the only difference being that in step (2), after the coprecipitation reaction is carried out for 9 hours, the feeding rate of the sodium hydroxide solution is changed to ensure that the pH value decreases by 0.1 every 3 hours (i.e., the rate of reducing the pH is 0.033 / h); and at the same time, the temperature of the mixed material in the reactor is adjusted to ensure that the temperature of the mixed material increases by 1°C every 3 hours (i.e., the heating rate is 0.33°C / h).

[0122] Comparative Example 3

[0123] The Ni provided in this comparative example 0.6 Co 0.1 Mn 0.3 (OH)2 Precursor Materials and LiNi 0.6 Co 0.1 Mn 0.3 The preparation method of the O2 positive electrode material is basically the same as that in Example 1, with the only difference being that in step (2), after the coprecipitation reaction is carried out for 9 hours, the feeding rate of the sodium hydroxide solution is changed to ensure that the pH value increases by 0.1 every 3 hours (i.e., the rate of increasing the pH is 0.033 / h) until the pH reaches 12.3; at the same time, the temperature of the mixed material in the reactor is adjusted to ensure that the temperature of the mixed material increases by 1°C every 3 hours (i.e., the heating rate is 0.33°C / h).

[0124] Experimental example

[0125] The positive electrode materials prepared in the above embodiments and comparative examples were dispersed in NMP solvent with conductive carbon black and polyvinylidene fluoride binder at a mass ratio of 88:6:6 for slurry preparation, and then the slurry was coated on an aluminum foil substrate, dried, rolled, and cut into discs with a diameter of 1.2 cm as positive electrode sheets. The positive electrode, diaphragm, and lithium / sodium sheet electrodes were assembled into 2016 button cells in a glove box, and their performance was tested on an electrochemical tester. The results are shown in Table 1 (1C current density) and Table 2 (5C current density).

[0126] Table 1 Electrical performance test results of the positive electrode materials prepared in each group at 1C

[0127]

[0128] Table 2 Electrical performance test results of the cathode materials prepared in each group at 5C

[0129]

[0130]

[0131] It can be seen from Table 1 that the internal particle cross-linked LiNi prepared in Example 1 0.6 Co 0.1 Mn 0.3 The first discharge capacity of the O2 positive electrode material at 1C current density reached 168mAh / g, and the capacity was maintained at 145mAh / g after 150 cycles, reaching a capacity retention rate of 86.3%. 0.6 Co 0.1 Mn 0.3 The first discharge capacity of the O2 positive electrode material at 1C current density is 157 mAh / g, and the capacity is maintained at 128 mAh / g after 150 cycles, with a corresponding capacity retention rate of 81.5%; the LiNi prepared in Example 2-3 0.6 Co 0.1 Mn 0.3 The capacity of O2 cathode material at 1C current density is also relatively low. These cycle performance data show that cathode materials with abundant internal pores, interconnected primary particles, and fewer grain boundaries have unique advantages as battery materials. Their special primary particle microstructure is very helpful for the diffusion of Li, because the interconnected primary particles and abundant voids provide a fast diffusion path for lithium / sodium ions and effective transmission from the inside of the particles to the surface.

[0132] It can be seen from Table 2 that the internal particle cross-linked LiNi prepared in Example 1 0.6 Co 0.1 Mn 0.3 The first discharge capacity of the O2 positive electrode material reached 137 mAh / g at a current density of 5C, and the capacity remained at 116 mAh / g after 150 cycles, reaching a capacity retention rate of 84.7%. 0.6 Co 0.1 Mn 0.3 The first discharge capacity of the O2 positive electrode material at 5C current density is 126 mAh / g, and the capacity is maintained at 99 mAh / g after 150 cycles, with a corresponding capacity retention rate of 78.6%. 0.6 Co 0.1 Mn 0.3 The capacity of O2 cathode material at 5C current density is also low.

[0133] These battery data show that the positive electrode material prepared by the present invention with abundant internal pores, cross-linked primary particles and fewer grain boundaries has better high-rate performance, because its special cross-linked primary particles and abundant voids can provide a fast transmission pathway for lithium / sodium ions and effective migration from the core of the particles to the surface.

[0134] In addition, the above tests show that the internal particle morphology of the positive electrode materials prepared in the other embodiments is all cross-linked, and has a higher discharge specific capacity and excellent cycle stability.

[0135] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A method for preparing a precursor material, characterized in that: The steps include: A mixed metal salt solution, a precipitant solution and a complexing agent solution are added to the base solution to perform a coprecipitation reaction; after the coprecipitation reaction is completed, the solid and liquid are separated to obtain the precursor material; Wherein, the metal elements in the mixed metal salt solution include at least two of Ni, Co, Mn and doped metal elements; The doping metal element includes at least one of La, Al, Ti, Ta, Mg, Mo, W, Ca, Zn, Nb, Cr, Zr and Fe; During the coprecipitation reaction, the mixture is first reacted at a certain temperature and pH for 2 to 20 hours, and then the temperature of the mixture is reduced at a rate of 0.1 to 1°C / h until the coprecipitation reaction is completed or the temperature reaches a lower limit, and the pH of the mixture is reduced at a rate of 0.01 to 0.1 / h until the coprecipitation reaction is completed or the pH reaches a lower limit; The chemical formula of the precursor material is Ni x Co y Mn z M e (OH)2; wherein, 0 < x < 1, 0 ≤ y < 1, 0 < z < 1, 0 ≤ e ≤ 0.333, and x + y + z + e = 1; M includes at least one of La, Al, Ti, Ta, Mg, Mo, W, Ca, Zn, Nb, Cr, Zr, and Fe; The shape of the primary particles of the precursor material includes a villi-like shape; The length of the primary particles of the precursor material is less than 1 μm, and the thickness of the primary particles of the precursor material is less than 100 nm; During the coprecipitation reaction, the temperature of the mixed material is 20-75° C., and the pH of the mixed material is 9.5-12.3; The coprecipitation reaction is carried out until the D50 particle size of the solid particles is 3-17 μm, and the total reaction time of the coprecipitation reaction is 25-90 hours.

2. The method for preparing a precursor material according to claim 1, characterized in that: The precipitant solution includes potassium hydroxide solution and / or sodium hydroxide solution.

3. The method for preparing a precursor material according to claim 1, characterized in that: The complexing agent solution includes at least one of a sodium oxalate solution, an ammonia solution, a citric acid solution and a disodium ethylenediaminetetraacetic acid solution.