A flame retardant PBT composite material and its preparation method and application

By using the coordinated combination of ethylene-sodium methacrylate polymer, disodium dihydrogen pyrophosphate and chain extender in PBT materials, the problem of insufficient welding strength and insufficient fluidity in ultrasonic welding is solved. , achieving high flowability and 0.4mm V-0 flame retardant level ultra-thin materials, improving welding strength and flame retardant performance.

CN116023769BActive Publication Date: 2024-11-05KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211689796.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-05
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The existing halogen-free flame-retardant PBT materials cannot be melt-plasticized during ultrasonic welding, resulting in insufficient welding strength and difficulty in obtaining ultra-thin halogen-free flame-retardant (0.4mm V-0) materials. The main reasons are insufficient fluidity and flame-retardant The agent decomposes during injection molding, reducing the flame retardant efficiency.

Method used

Using the coordinated cooperation of ethylene-sodium methacrylate polymer, disodium dihydrogen pyrophosphate and chain extender, the extrusion and granulation are carried out through a twin-screw extruder to improve the fluidity and welding strength of the material and ensure the flame retardant performance reaching 0.4. mm V-0 level.

Benefits of technology

It significantly improves the strength and fluidity of ultrasonic welding, ensures the 0.4mm V-0 flame retardant level of the material, and reduces the decomposition of flame retardant during injection molding, and improves welding strength and fluidity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a flame retardant PBT composite material, which comprises the following components by weight: 50 parts of PBT; 7-14 parts of hypophosphite flame retardant; 0.5-2 parts of solid phosphate flame retardant; 1-4 parts of ethylene-sodium methacrylate polymer; 0.1-1 parts of disodium dihydrogen pyrophosphate; and 0.1-0.3 parts of chain extender. The invention can improve the defect of poor ultrasonic welding effect of the flame retardant PBT composite material, improve fluidity and reduce the decomposition of the flame retardant during the injection molding process, and has a flame retardant level of 0.4mm V-0 by selecting the synergy of ethylene-sodium methacrylate polymer / disodium dihydrogen pyrophosphate / chain extender.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a flame retardant PBT composite material and a preparation method and application thereof. Background Art

[0002] Ultrasonic welding is a reliable, efficient and pollution-free welding technology, which is widely used in plastic and metal connections. In the electrical and electronic industry, plastic parts such as charger housings, USB connectors, and low-voltage electrical appliance housings all require ultrasonic welding. With the development trend of miniaturization, thin-walling, halogen-free, environmentally friendly, and high-performance in the electrical and electronic industry, the requirements for the weldability, flame retardancy, and material fluidity of modified PBT materials are becoming higher and higher.

[0003] At present, the mature flame retardant system of halogen-free flame retardant PBT is the hypophosphite compound melamine polyphosphate system. The compound of the two flame retardants can improve the mechanical properties of the material. However, the above-mentioned halogen-free flame retardants are inorganic fillers and cannot be melted and plasticized during ultrasonic welding, which seriously affects the ultrasonic welding strength. In addition, it is difficult to obtain ultra-thin halogen-free flame retardant (0.4mm V-0) using the hypophosphite compound melamine polyphosphate system. The main reason is that the fluidity is insufficient. The flame retardant decomposes due to high shear during the injection molding process, which reduces the flame retardant efficiency. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and provide an ultra-thin halogen-free flame-retardant (0.4mm V-0), high-flowability, and ultrasonically weldable PBT composite material and a preparation method thereof.

[0005] The present invention is achieved through the following technical solutions:

[0006] A flame retardant PBT composite material, comprising the following components in parts by weight:

[0007] PBT 50 parts;

[0008] 7-14 parts of hypophosphite flame retardant;

[0009] 0.5-2 parts of solid phosphate flame retardant;

[0010] 1-4 parts of ethylene-sodium methacrylate polymer;

[0011] Disodium dihydrogen pyrophosphate 0.1-1 part;

[0012] Chain extender 0.1-0.3 parts.

[0013] Preferably, the following components are included by weight:

[0014] PBT 50 parts;

[0015] 7-14 parts of hypophosphite flame retardant;

[0016] 0.5-2 parts of solid phosphate flame retardant;

[0017] Ethylene-sodium methacrylate polymer 2-3 parts;

[0018] Disodium dihydrogen pyrophosphate 0.3-0.7 parts;

[0019] Chain extender 0.15-0.25 parts.

[0020] The melting point of the ethylene-sodium methacrylate polymer may be in the range of 65-95°C. Preferably, the melting point of the ethylene-sodium methacrylate polymer is in the range of 85-95°C.

[0021] The melting point of ethylene-sodium methacrylate polymer is lower than that of PBT resin. It can be melted and plasticized during the heating process of ultrasonic welding, and the bonding effect can be improved. After melting, it can combine the PBT melt and effectively improve the welding strength.

[0022] The chain extender is selected from at least one of bisphenol A diglycidyl ether, 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate and glycidyl methacrylate.

[0023] The intrinsic viscosity of the PBT is in the range of 0.6-1.2 dL / g, and the test condition is 25°C.

[0024] The hypophosphite flame retardant is selected from aluminum diethylphosphinate.

[0025] The solid phosphate flame retardant is selected from at least one of 1,3-phenylene (2,6-diphenylmethyl) tetraphosphate and triphenyl phosphate.

[0026] It is possible to choose whether to add 0-1 part of lubricant according to actual needs. The lubricant may be pentaerythritol phosphate.

[0027] The preparation method of the flame retardant PBT composite material comprises the following steps: uniformly mixing the components, extruding and granulating through a twin-screw extruder, wherein the screw speed ranges from 200 to 450 rpm and the screw temperature ranges from 200 to 260° C., to obtain the flame retardant PBT composite material.

[0028] The application of flame-retardant PBT composite materials is used to prepare ultrasonic welding parts, such as motor housings, car light housings and other parts.

[0029] The present invention has the following beneficial effects:

[0030] The present invention can improve the defect of poor ultrasonic welding effect of flame-retardant PBT composite material (pull-off force is greater than or equal to 148N, spiral line length is greater than or equal to 236mm) by selecting ethylene-sodium methacrylate polymer / disodium dihydrogen pyrophosphate / chain extender, improve fluidity and reduce flame retardant decomposition during injection molding, and has a flame retardant level of 0.4mm V-0. DETAILED DESCRIPTION

[0031] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0032] The raw materials used in the examples and comparative examples of the present invention are as follows:

[0033] PBT-A: PBT GX110, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 0.6 dL / g.

[0034] PBT-B: PBT GX112, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 0.8 dL / g.

[0035] PBT-C: PBT GX121, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 1.0 dL / g.

[0036] PBT-D: PBT GL236, Yizheng Chemical Fiber, intrinsic viscosity at 25°C is 1.2 dL / g;

[0037] Diethylaluminum hypophosphite: Clariant, Germany, Exolit OP1230.

[0038] 1,3-Phenylene (2,6-diphenylmethyl) tetraphosphate: Daihachi Chemical Industry Co., Ltd., PX-200.

[0039] Triphenyl phosphate: Suzhou Dongtuo Chemical Co., Ltd., DTZR-TPP.

[0040] Disodium dihydrogen pyrophosphate: Taihei Chemical Industry Co., Ltd., DHPP.

[0041] Chain extender A: bisphenol A diglycidyl ether, Guodu Chemical Co., Ltd., YD-019.

[0042] Chain extender B: 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, Wuhan Chengtian Fine Chemical Co., Ltd., CT0961.

[0043] Chain extender C: Glycidyl methacrylate, BASF, ADR 4468.

[0044] Ethylene-sodium methacrylate polymer A: Surlyn 8920, DuPont, USA, melting point 88°C;

[0045] Ethylene-sodium methacrylate polymer B: Surlyn 8940, DuPont, USA, melting point 94°C;

[0046] Ethylene-sodium methacrylate polymer C: Surlyn 9910, DuPont, USA, melting point 86°C;

[0047] Ethylene-sodium methacrylate polymer D: Surlyn 9320, DuPont, USA, melting point 70°C;

[0048] Pentaerythritol phosphate: Hubei Zhenbo Chemical Co., Ltd.

[0049] Embodiment and comparative example Preparation method of flame-retardant PBT composite material: The components are mixed uniformly, and extruded into granules through a twin-screw extruder. The screw speed range is 200-450 rpm, and the screw temperature is set as follows: the temperature of zone 1 from the feed port to the die is 200-230°C, the temperature of zone 2 is 240-260°C, the temperature of zone 3 is 235-255°C, the temperature of zone 4 is 235-255°C, the temperature of zone 5 is 235-255°C, the temperature of zone 6 is 240-260°C, the temperature of zone 7 is 240-260°C, the temperature of zone 8 is 220-240°C, the temperature of zone 9 is 220-240°C, and the temperature of zone 10 is 240-260°C to obtain a flame-retardant PBT composite material.

[0050] Various test methods:

[0051] (1) Flame retardancy: UL94, vertical burning strip, strip size 127*13*0.8mm and 127*13*0.4mm.

[0052] (2) Fluidity test: The spiral length of each sample was injection molded at a temperature of 260°C and a pressure of 80 MPa. 51 films were continuously injected and the spiral length of the last mold product was tested. The longer the length, the better the fluidity of the product.

[0053] (3) Ultrasonic welding strength test: injection molding 80*10*4mm size specimens, ultrasonic welding area 10*10mm, pressure 20MPa, welding time 0.5s, pressure holding 1s. The surface of the specimen is melted and bonded, and the specimen pull-off force is tested using a tensile testing machine.

[0054] The fluidity test and the ultrasonic welding strength test jointly characterize the quality of ultrasonic welding characteristics. The longer the spiral wire length and the greater the pull-off force, the better the ultrasonic welding characteristics.

[0055] Table 1: Content of each component (parts by weight) and test results of flame-retardant PBT composite materials of Examples 1-7

[0056] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 PBT resin B 50 50 50 50 50 50 50 Diethylaluminum hypophosphite 10 7 10 10 10 10 10 Triphenyl phosphate 1 1 1 1 1 1 1,3-phenylene phosphate (2,6-diphenylmethyl) tetraester 2 Ethylene-sodium methacrylate polymer A 2 2 1 2 2.5 3 4 Disodium dihydrogen pyrophosphate 0.5 0.5 0.1 0.3 0.5 0.7 1 Chain Extender A 0.2 0.2 0.1 0.15 0.2 0.25 0.3 Flame retardant 0.8mm V-0 V-0 V-0 V-0 V-0 V-0 V-0 Flame retardant 0.4mm V-0 V-1 V-1 V-0 V-0 V-0 V-0 Helix length mm 252 258 258 254 250 246 236 Pull-off force N 158 159 148 155 165 174 186

[0057] It can be seen from Examples 1 / 3-7 that within the preferred content range of ethylene-sodium methacrylate polymer / disodium dihydrogen pyrophosphate / chain extender, the flame retardant performance is stable at the V-0 level, and the spiral length is greater than 245 mm and the pull-off force is greater than 150 N, indicating that the ultrasonic welding is excellent.

[0058] Table 2: Content of each component (parts by weight) and test results of flame-retardant PBT composite materials of Examples 8-12

[0059] Example 8 Example 9 Example 10 Embodiment 11 Example 12 PBT resin B 50 50 PBT Resin A 50 PBT resin C 50 PBT resin D 50 Diethylaluminum hypophosphite 14 12 10 10 10 Triphenyl phosphate 0.5 1.5 2 1 1 Ethylene-sodium methacrylate polymer A 2 2.5 3 2.5 2.5 Disodium dihydrogen pyrophosphate 0.3 0.7 0.6 0.5 0.5 Chain Extender A 0.2 0.2 0.1 Chain Extender B 0.2 Chain Extender C 0.2 Flame retardant 0.8mm V-0 V-0 V-0 V-0 V-0 Flame retardant 0.4mm V-0 V-0 V-0 V-0 V-0 Helix length mm 251 250 253 250 250 Pull-off force N 166 164 167 165 166

[0060] It can be seen from Examples 5 / 8-12 that different ethylene-sodium methacrylate polymers / chain extenders can achieve the purpose of the present invention.

[0061] Table 3: Content of each component (parts by weight) and test results of flame-retardant PBT composite materials of Examples 13-15

[0062] Embodiment 13 Embodiment 14 Embodiment 15 PBT resin B 50 50 50 Diethylaluminum hypophosphite 10 10 10 Triphenyl phosphate 1 1 1 Ethylene-sodium methacrylate polymer B 2.5 Ethylene-sodium methacrylate polymer C 2.5 Ethylene-sodium methacrylate polymer D 2.5 Disodium dihydrogen pyrophosphate 0.5 0.5 0.5 Chain Extender A 0.2 0.2 0.2 Flame retardant 0.8mm V-0 V-0 V-0 Flame retardant 0.4mm V-0 V-0 V-0 Helix length mm 253 251 247 Pull-off force N 166 162 159

[0063] It can be seen from Examples 5 / 13-15 that the preferred melting point range of ethylene-sodium methacrylate polymer is 85-95°C for better fluidity and ultrasonic welding ability.

[0064] Table 4: Content of each component (parts by weight) and test results of comparative flame-retardant PBT composite materials

[0065] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 PBT resin B 50 50 50 50 50 50 Diethylaluminum hypophosphite 10 10 10 10 10 10 Triphenyl phosphate 1 1 1 1 1 1 Ethylene-sodium methacrylate polymer A 0.5 5 2.5 2.5 2.5 2.5 Disodium dihydrogen pyrophosphate 0.5 0.5 0 1.5 0.5 0.5 Chain Extender A 0.2 0.2 0.2 0.2 0 0.4 Flame retardant 0.8mm V-0 V-2 V-1 V-0 V-0 V-0 Flame retardant 0.4mm V-0 The V-2 could not reach The V-2 could not reach V-0 V-0 V-0 Helix length mm 220 224 248 278 255 229 Pull-off force N 126 145 155 120 133 156

[0066] It can be seen from Comparative Example 1 / 2 that if the content of ethylene-sodium methacrylate polymer is too low, the ultrasonic weldability is poor; if the content of ethylene-sodium methacrylate polymer is too high, the flame retardant performance will decrease.

[0067] It can be seen from Comparative Examples 3 / 4 that the flame retardancy is poor when disodium dihydrogen pyrophosphate is not contained; however, when the content of disodium dihydrogen pyrophosphate is too high, the pull-off force after ultrasonic welding is low, indicating that the ultrasonic welding performance is poor.

[0068] It can be seen from Comparative Example 5 that the pull-off force is low when no chain extender is contained. It can be seen from Comparative Example 6 that if the content of the chain extender is too high, the helical length will be low.

Claims

1. A flame retardant PBT composite material, characterized in that: By weight, it is composed of the following components: PBT 50 parts; 7-14 parts of hypophosphite flame retardant; 0.5-2 parts of solid phosphate flame retardant; 1-4 parts of ethylene-sodium methacrylate polymer; Disodium dihydrogen pyrophosphate 0.1-1 part; Chain extender 0.1-0.3 parts; The chain extender is selected from at least one of YD-019 of Guodu Chemical Co., Ltd. and ADR 4468 of BASF.

2. The flame retardant PBT composite material according to claim 1, characterized in that: By weight, it is composed of the following components: PBT 50 parts; 7-14 parts of hypophosphite flame retardant; 0.5-2 parts of solid phosphate flame retardant; Ethylene-sodium methacrylate polymer 2-3 parts; Disodium dihydrogen pyrophosphate 0.3-0.7 parts; Chain extender 0.15-0.25 parts.

3. The flame retardant PBT composite material according to claim 1 or 2, characterized in that: The melting point of the ethylene-sodium methacrylate polymer is in the range of 85-95°C.

4. The flame retardant PBT composite material according to claim 1 or 2, characterized in that: The intrinsic viscosity of the PBT is in the range of 0.6-1.2 dL / g, and the test condition is 25°C.

5. The flame retardant PBT composite material according to claim 1 or 2, characterized in that: The hypophosphite flame retardant is selected from aluminum diethylphosphinate.

6. The flame retardant PBT composite material according to claim 1 or 2, characterized in that: The solid phosphate flame retardant is selected from at least one of 1,3-phenylene (2,6-diphenylmethyl) tetraphosphate and triphenyl phosphate.

7. The flame retardant PBT composite material according to claim 1 or 2, characterized in that: By weight, 0-1 part of lubricant is also included.

8. The method for preparing the flame retardant PBT composite material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: uniformly mixing the components, extruding and granulating the components through a twin-screw extruder, wherein the screw speed range is 200-450 rpm and the screw temperature range is 200-260° C., so as to obtain a flame-retardant PBT composite material.

9. Use of the flame retardant PBT composite material according to any one of claims 1 to 7, characterized in that: Used for preparing parts requiring ultrasonic welding, selected from at least one of motor housing and car light housing.