Catalyst for producing acrylic acid, method for producing the same, and method for producing acrylic acid
By optimizing the cooling conditions of the catalyst, the problem of insufficient catalyst performance in the existing technology was solved, and high acrylic acid selectivity and yield were improved. Specifically, by using long-term cooling and controlling oxygen concentration after calcination, the catalyst was ensured High efficiency in acrolein oxidation reaction.
Patent Information
- Application Number
- CN202180054140.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-03
- Filing Date
- 2021-08-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-08-23
AI Technical Summary
Existing acrylic acid manufacturing catalysts have insufficient performance under certain conditions and are difficult to achieve high selectivity and high yield. In particular, there is room for improvement in the optimization of the crystal structure of the catalytically active component.
By optimizing the cooling conditions after the calcination process of the catalyst, especially setting appropriate cooling time and atmosphere, ensure that the catalytically active components display specific diffraction peaks and peak intensity ratios in X-ray diffraction analysis, thereby improving the selectivity and yield of acrylic acid. . The specific method includes using a cooling time of more than 5 hours after calcination, cooling to 100°C, and cooling in an atmosphere with an oxygen concentration exceeding 5% by volume but not exceeding 21% by volume.
The catalyst achieves high acrylic acid selectivity and high acrylic acid yield in the catalytic gas phase oxidation process of acrolein, and improves the activity and selectivity of the catalyst.
Smart Images

Figure BDA0004104792870000271 
Figure BDA0004104792870000281 
Figure BDA0004104792870000291
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst for producing acrylic acid from acrolein, a method for producing the catalyst, and a method for producing acrylic acid using the catalyst. Background Art
[0002] Acrylic acid is widely used as a raw material for various industrial products. The method for producing acrylic acid is currently generally a method of gas-phase oxidation of propylene in the presence of a catalyst using a fixed bed reactor. According to this production method, propylene is catalytically gas-phase oxidized in a first-stage reaction to obtain acrolein-containing gas, and then catalytically gas-phase oxidized in a second-stage reaction to obtain acrylic acid. The catalyst used here is generally a catalyst containing molybdenum as an essential component. Among them, as a catalyst used in the second-stage reaction of producing acrylic acid from acrolein, a catalyst containing molybdenum and vanadium as catalytically active components, that is, a catalyst containing a Mo-V composite oxide is known. In general, the performance of a known catalyst depends not only on the type of metals constituting the catalytically active components and their content ratio, but also greatly depends on the crystal structure of the catalytically active components. For example, Patent Documents 1 to 5 disclose catalysts having a crystal structure that shows various X-ray diffraction profiles in X-ray diffraction analysis.
[0003] It is also known that the crystal structure of a catalytically active component generally changes greatly depending on the catalyst production method and production conditions. For example, the above-mentioned Patent Documents 1 to 5 disclose: a method of drying a mixed solution of raw materials, calcining it and coating it on a carrier (Patent Document 1); a method of blowing an oxygen-containing gas into the step of reacting the raw materials in an aqueous medium (Patent Document 2); a method of adding a nitrogen-containing compound different from the starting material in any of the steps of obtaining a mixed solution of starting materials, drying the mixed solution to obtain a dried product or further calcining the dried product to obtain a calcined product, and molding or supporting the dried product or calcined product on an inactive carrier (Patent Document 3); a method of adding an additive different from the starting material in any of the steps of obtaining a mixed solution of starting materials, drying the mixed solution to obtain a dried product, and supporting the dried product on an inactive carrier (Patent Document 4); a method of preparing a mixed solution containing molybdenum and vanadium and a mixed solution of an antimony compound and an alkaline aqueous solution, respectively, and mixing the two solutions (Patent Document 5), thereby obtaining catalysts having crystal structures showing various X-ray diffraction profiles as described above.
[0004] It is believed that the crystal structure of the catalytically active component is also affected by the conditions of the calcination process during production. In the above-mentioned Patent Documents 1 to 5, the temperature is generally appropriately adjusted within the temperature range of 250 to 660° C. On the other hand, Patent Document 6 discloses the following method: in order to produce a catalytically active multinary oxide material containing Mo, V and Cu, a uniform dry mixture containing starting materials is produced and temporarily calcined at a final temperature of 380 to 450° C., and then the uniform dry mixture is cooled to a temperature of 100° C. or less within 5 hours.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 8-299797
[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 11-285637
[0009] Patent Document 3: Japanese Patent Application Publication No. 2015-120133
[0010] Patent Document 4: Japanese Patent Application Publication No. 2016-59898
[0011] Patent Document 5: Japanese Patent Application Publication No. 2018-43197
[0012] Patent Document 6: Japanese Patent Application No. 2006-526495 Summary of the invention
[0013] Problem that the invention aims to solve
[0014] Although the catalysts having various crystal structures disclosed in the above-mentioned documents have shown high performance to some extent as practical catalysts for producing acrylic acid from acrolein, there is still room for improvement, and further performance improvement is required, specifically, high selectivity and high yield are required. The present invention has been made in view of the above circumstances, and its object is to provide a catalyst for producing acrylic acid from acrolein and showing high acrylic acid selectivity or high acrylic acid yield, and to provide a production method that can easily obtain a catalyst showing high acrylic acid selectivity or high acrylic acid yield. The present invention also provides a method for producing acrylic acid from acrolein, which uses the catalyst of the present invention or a catalyst obtained by the production method of the present invention.
[0015] Solutions for solving problems
[0016] To achieve the above object, the present inventors have focused on the optimization of the crystal structure of the catalytically active component and have conducted various studies, particularly focusing on the cooling conditions after the calcination step, as a method for obtaining a catalytically active component having an optimal crystal structure. As a result, the inventors have found that a catalyst containing a catalytically active component having a diffraction peak at a specific diffraction angle in an X-ray diffraction analysis and having a value within a predetermined range for each peak intensity ratio can be a catalyst showing a high selectivity for acrylic acid and a high yield of acrylic acid when acrylic acid is produced by catalytic gas-phase oxidation of acrolein, and that it is effective to appropriately set the cooling time and gas atmosphere during cooling after the calcination step in order to obtain a catalyst having such a catalytically active component, thereby completing the present invention.
[0017] That is, the present invention includes the following inventions.
[0018] [1] A catalyst for producing acrylic acid, which is a catalyst for producing acrylic acid from acrolein, the catalyst for producing acrylic acid containing molybdenum, vanadium and copper as catalytically active components, the catalytically active components having diffraction peaks at 2θ=22.2°±0.3°, 28.2°±0.3°, 31.5°±0.3° and 32.6°±0.3° in an X-ray diffraction analysis using Cu-Kα rays, and the peak intensity at 2θ=28.2°±0.3° and the peak intensity at 2θ=22.2°±0.3° are both equal to the peak intensity at 2θ=22.2°±0.3°. The intensity ratio I(28.2°) / I(22.2°) is greater than 0.20 and less than 0.50, the ratio of the peak intensity at 2θ=31.5°±0.3° to the peak intensity at 2θ=22.2°±0.3° I(31.5°) / I(22.2°) is greater than 0.03 and less than 0.20, and the ratio of the peak intensity at 2θ=32.6°±0.3° to the peak intensity at 2θ=22.2°±0.3° I(32.6°) / I(22.2°) is greater than 0.03 and less than 0.40.
[0019] [2] The catalyst for producing acrylic acid according to [1], wherein the catalytically active component further has a diffraction peak at 2θ=33.4°±0.3° in X-ray diffraction analysis, the ratio of the peak intensity at 2θ=33.4°±0.3° to the peak intensity at 2θ=22.2°±0.3°, I(33.4°) / I(22.2°), is 0.06 or more and 0.40 or less, and the ratio of the highest intensity in the range of 2θ=5° to 10° to the peak intensity at 2θ=22.2°±0.3°, I(5°-10°) / I(22.2°), is 0.06 or less.
[0020] [3] The catalyst for producing acrylic acid according to [1] or [2], wherein the catalytically active component further has a diffraction peak at 2θ=27.3°±0.3° in X-ray diffraction analysis, and the ratio of the peak intensity at 2θ=27.3°±0.3° to the peak intensity at 2θ=22.2°±0.3°, I(27.3°) / I(22.2°), is 0.10 or more and 0.60 or less.
[0021] [4] The catalyst for acrylic acid production according to any one of [1] to [3], wherein the catalytically active component has a composition represented by the following formula (1).
[0022] Mo a V b Cu c A d B e C f D g E h O i …(1)
[0023] (In the formula, Mo represents molybdenum, V represents vanadium, Cu represents copper, A represents at least one element selected from the group consisting of tungsten, niobium and tantalum, B represents at least one element selected from the group consisting of antimony and tin, C represents at least one element selected from the group consisting of chromium, manganese, iron, cobalt, nickel, zinc, zirconium, tellurium, cerium and bismuth, D represents at least one element selected from the group consisting of alkali metals and alkaline earth metals, E represents at least one element selected from the group consisting of silicon, aluminum and titanium, O represents oxygen, a to i represent the atomic ratios of Mo, V, Cu, A, B, C, D, E and O, respectively, when a=12, 2≤b≤14, 0<c≤5, 0<d≤10, 0<e≤5, 0≤f≤5, 0≤g≤3, 0≤h≤30, and i is a value determined according to the oxidation state of each element.)
[0024] [5] A method for producing a catalyst for producing acrylic acid from acrolein, comprising the following steps: a step of obtaining a raw material mixed solution containing molybdenum, vanadium and copper; a step of drying the raw material mixed solution to obtain a dried product; a step of molding or supporting the dried product on an inactive carrier to obtain a molded body or a supported body; a step of heating the molded body or supported body at a temperature T between 380°C and 460°C. C and, after the aforementioned calcination in an atmosphere with an oxygen concentration exceeding 5% by volume and 21% by volume or less, cooling for more than 5 hours from the aforementioned temperature T C Cooling process to 100°C.
[0025] [6] A method for producing a catalyst for producing acrylic acid, which is a method for producing a catalyst for producing acrylic acid from acrolein, comprising the following steps: a step of obtaining a raw material mixed solution containing molybdenum, vanadium and copper; a step of drying the raw material mixed solution to obtain a dried product; a step of drying the dried product at a temperature T between 380°C and 460°C; C After the aforementioned calcination in an atmosphere with an oxygen concentration exceeding 5% by volume and 21% by volume or less, a cooling time of 5 hours or more from the aforementioned temperature T C a step of cooling to 100° C.; and a step of molding or supporting the calcined product obtained through the cooling step on an inactive carrier.
[0026] [7] The method for producing a catalyst for producing acrylic acid according to [5] or [6], wherein in the cooling step, the temperature T is lowered from the temperature T to the temperature T in a cooling time of 3 hours or more. C Cool to 300°C.
[0027] [8] A method for producing acrylic acid, comprising the step of obtaining acrylic acid by catalytically oxidizing acrolein in the presence of the catalyst described in any one of [1] to [4] or the catalyst obtained by the production method described in any one of [5] to [7].
[0028] Effects of the Invention
[0029] The catalyst for producing acrylic acid of the present invention shows high acrylic acid selectivity or high acrylic acid yield. In addition, according to the method for producing the catalyst for producing acrylic acid of the present invention, the catalyst for producing acrylic acid of the present invention can be easily obtained, and the obtained catalyst shows high acrylic acid selectivity or high acrylic acid yield. DETAILED DESCRIPTION
[0030] The present invention relates to a catalyst for producing acrylic acid and a method for producing the same, and more specifically, to a catalyst for producing acrylic acid by catalyzing acrolein to undergo a gas-phase oxidation reaction, and a method for producing the same. The catalyst of the present invention contains molybdenum, vanadium and copper as catalytically active components, and more specifically, contains a composite oxide containing these elements, molybdenum, vanadium and copper. In the present invention, a composite oxide containing these elements, molybdenum, vanadium and copper, can be used as a catalyst. Hereinafter, the composite oxide containing these elements, molybdenum, vanadium and copper, will be referred to as a "Mo-V-Cu composite oxide", but this description does not exclude the inclusion of elements other than Mo, V and Cu. Mo-V composite oxide-based catalysts are widely used in industry as catalysts for oxidizing acrolein to produce acrylic acid, and the catalyst of the present invention contains a Mo-V-Cu composite oxide further containing Cu on the basis of Mo and V. By making a Mo-V-Cu composite oxide containing Cu, the selectivity of acrylic acid can be improved.
[0031] The catalyst of the present invention may contain other metal elements and semi-metal elements as catalytically active components in addition to molybdenum, vanadium and copper. Examples of other metal elements and semi-metal elements include tungsten, niobium, tantalum, antimony, tin, chromium, manganese, iron, cobalt, nickel, zinc, zirconium, tellurium, cerium, bismuth, alkali metals, alkaline earth metals, silicon, aluminum, titanium, etc., and the Mo-V-Cu composite oxide that is preferably the catalytically active component also contains at least one element selected from them. Among them, the catalyst of the present invention preferably contains tungsten and / or antimony as catalytically active components on the basis of containing molybdenum, vanadium and copper, that is, the Mo-V-Cu composite oxide preferably also contains tungsten and / or antimony.
[0032] In the catalyst of the present invention, the catalytically active component preferably has a composition represented by the following formula (1), for example.
[0033] Mo a V b Cu c A d B e C f D g E h O i …(1)
[0034] In the above formula (1), Mo represents molybdenum, V represents vanadium, Cu represents copper, A represents at least one element selected from the group consisting of tungsten, niobium and tantalum, B represents at least one element selected from the group consisting of antimony and tin, C represents at least one element selected from the group consisting of chromium, manganese, iron, cobalt, nickel, zinc, zirconium, tellurium, cerium and bismuth, D represents at least one element selected from the group consisting of alkali metals and alkaline earth metals, E represents at least one element selected from the group consisting of silicon, aluminum and titanium, O represents oxygen, a to i represent the atomic ratio of Mo, V, Cu, A, B, C, D, E and O, respectively, when a=12, 2≤b≤14, 0<c≤5, 0<d≤10, 0<e≤5, 0≤f≤5, 0≤g≤3, 0≤h≤30, and i is a value determined according to the oxidation state of each element. In the above formula (1), when a=12, the value of b is preferably 3 or more, and preferably 10 or less, and more preferably 8 or less. The value of c is preferably 0.1 or more, more preferably 0.2 or more, and preferably 4 or less. The value of d is preferably 0.1 or more, more preferably 0.3 or more, and further preferably 0.5 or more, and further preferably 6 or less, more preferably 4 or less, and further preferably 3 or less. The value of e is preferably 0.1 or more, more preferably 0.2 or more, and further preferably 3 or less, more preferably 2 or less, and further preferably 1 or less. The value of f is preferably 4 or less, more preferably 3 or less, and may be 0. The value of g is preferably 2 or less, more preferably 1 or less, and may be 0. The value of h is preferably 20 or less, more preferably 10 or less, and may be 0.
[0035] In the above formula (1), A is preferably tungsten, and B is preferably antimony. That is, the catalyst of the present invention preferably contains tungsten and antimony as catalytically active components in addition to molybdenum, vanadium and copper.
[0036] In the above formula (1), the values of f, g and h may be 0. In this case, the catalyst of the present invention preferably has a composition represented by the following formula (2) as a catalytically active component. In the following formula (2), Mo, V, Cu, A, B, O, a to e, and i have the same meanings as above.
[0037] Mo a V b Cu c A d B e O i …(2)
[0038] In the above formula (2), A is preferably tungsten and B is preferably antimony. Therefore, in the catalyst of the present invention, as a catalytically active component, it is more preferable to have a composition represented by the following formula (3). In the following formula (3), Mo, V, Cu, O, a to e, and i have the same meanings as above, W represents tungsten, and Sb represents antimony.
[0039] Mo a V b Cu c W d Sb e O i …(3)
[0040] The composition of the catalytically active components, i.e., the catalyst composition, can be determined by measuring the metal components contained in the catalyst using an ICP emission spectrometer, an atomic absorption device, or a fluorescent X-ray analyzer. Alternatively, the catalyst composition can be determined from the amount of the metal components used as raw materials when preparing the catalyst and / or the amount of the metal components actually taken into the catalyst.
[0041] The catalytically active component has diffraction peaks at 2θ=22.2°±0.3°, 28.2°±0.3°, 31.5°±0.3°, and 32.6°±0.3° in X-ray diffraction analysis using Cu-Kα rays. The catalyst of the present invention shows predetermined peak intensities at these diffraction angles, which is different from the Mo-V composite oxide catalyst known as a catalyst for acrylic acid production. Specifically, the ratio of the peak intensity of 2θ=28.2°±0.3° to the peak intensity of 2θ=22.2°±0.3°, I(28.2°) / I(22.2°), is 0.20 or more and 0.50 or less, the ratio of the peak intensity of 2θ=31.5°±0.3° to the peak intensity of 2θ=22.2°±0.3°, I(31.5°) / I(22.2°), is 0.03 or more and 0.20 or less, and the ratio of the peak intensity of 2θ=32.6°±0.3° to the peak intensity of 2θ=22.2°±0.3°, I(32.6°) / I(22.2°), is 0.03 or more and 0.40 or less. The above ratio I(28.2°) / I(22.2°) is preferably 0.22 or more, and more preferably 0.23 or more. The above ratio I(31.5°) / I(22.2°) is preferably 0.18 or less, more preferably 0.16 or less. The above ratio I(32.6°) / I(22.2°) is preferably 0.38 or less, more preferably 0.35 or less.
[0042] The catalyst of the present invention has a high selectivity for acrylic acid and a high yield for acrylic acid when producing acrylic acid by catalytically oxidizing acrolein in the gas phase, because the catalytically active component has a diffraction peak at a specific diffraction angle in X-ray diffraction analysis as described above and the intensity ratio of each peak shows a value within a predetermined range. To explain this in detail, the diffraction peak at 2θ=22.2°±0.3° can be attributed to VMo3O 11 , which is known to be an effective structure for the reaction of converting acrolein into acrylic acid. The diffraction peak at 2θ = 28.2° ± 0.3° can be mainly attributed to VMo3O 11 (However, the crystal plane is different from the diffraction peak of 2θ=22.2°±0.3°), and the diffraction peaks of 2θ=31.5°±0.3° and 2θ=32.6°±0.3° can be mainly attributed to (V 0.07 Mo 0.93 )5O 14 and V 0.95 Mo 0.97O5, the crystal structure itself is different from the crystal structure of the diffraction peak of 2θ=22.2°±0.3°. The inventors have found out through research that when the crystal planes and crystal structures different from the structure of the diffraction peak of 2θ=22.2°±0.3° exist in excess or too little in the catalytic active component, the activity in the reaction of converting acrolein to acrylic acid is reduced and / or the selectivity for acrylic acid is at a low level. However, it can be inferred that the catalyst of the present invention may improve the oxygen transfer ability and the adsorption and desorption ability of acrolein, acrylic acid, etc. in the catalytic gas phase oxidation reaction of converting acrolein to acrylic acid by making multiple crystal planes and crystal structures different from the structure of the diffraction peak of 2θ=22.2°±0.3° in the catalytic active component exist in a ratio within a specified range relative to the structure of the diffraction peak of 2θ=22.2°±0.3°, thereby improving the activity and selectivity of the catalyst. It should be noted that the attribution of the above diffraction angles is based on the Powder Diffraction / Crystal Structure Database (ICDD).
[0043] The catalyst of the present invention preferably has a diffraction peak of a specified intensity at 2θ=33.4°±0.3° in an X-ray diffraction analysis of the catalytically active component using Cu-Kα rays. Specifically, the ratio of the peak intensity at 2θ=33.4°±0.3° to the peak intensity at 2θ=22.2°±0.3°, I(33.4°) / I(22.2°), is preferably 0.06 or more and 0.40 or less. The aforementioned ratio I(33.4°) / I(22.2°) is more preferably 0.38 or less, and further preferably 0.35 or less. The catalytically active component is also preferably such that, in an X-ray diffraction analysis using Cu-Kα rays, the highest intensity in the range of 2θ=5° to 10° is less than a specified value compared to the peak intensity at 2θ=22.2°±0.3°. Specifically, the ratio of the maximum intensity in the range of 2θ=5° to 10° to the peak intensity at 2θ=22.2°±0.3°, I(5°-10°) / I(22.2°), is preferably 0.06 or less, more preferably 0.05 or less. It should be noted that the "maximum intensity in the range of 2θ=5° to 10°" here refers to the value of the maximum intensity in the range, regardless of whether a clear peak appears or does not appear in the range of the diffraction angle. By making the catalytically active component in the catalyst of the present invention show such an X-ray diffraction profile, a high acrylic acid selectivity and a high acrylic acid yield can be more reliably shown when acrylic acid is produced by catalytic gas-phase oxidation of acrolein.
[0044] The catalytically active component may also have a diffraction peak at 2θ=27.3°±0.3° in an X-ray diffraction analysis of the catalytically active component using Cu-Kα rays. For example, the ratio of the peak intensity at 2θ=27.3°±0.3° to the peak intensity at 2θ=22.2°±0.3°, I(27.3°) / I(22.2°), may be 0.10 or more and 0.60 or less. The aforementioned ratio I(27.3°) / I(22.2°) may be 0.14 or more, 0.16 or more, 0.20 or more, and 0.50 or less, or 0.40 or less. The catalyst of the present invention allows the catalytically active component to exhibit such an X-ray diffraction profile, thereby more reliably exhibiting a high acrylic acid selectivity and a high acrylic acid yield when acrylic acid is produced by catalytic gas-phase oxidation of acrolein.
[0045] The shape of the catalyst is not particularly limited, and examples thereof include granular, spherical, cylindrical, annular, saddle-shaped, honeycomb-shaped, irregular shapes, etc. The particle size of the catalyst is preferably 1.0 mm or more, more preferably 2.0 mm or more, and further preferably 2.5 mm or more, and is preferably 30.0 mm or less, more preferably 20.0 mm or less, and further preferably 15.0 mm or less.
[0046] The catalyst of the present invention may be a supported catalyst in which a catalytically active component containing a Mo-V-Cu composite oxide is supported on a carrier, or may be an unsupported catalyst in which the catalytically active component is not supported on a carrier. The carrier is preferably a carrier inactive for acrolein and acrylic acid, and may be, for example, an inorganic oxide or composite oxide such as silica, alumina, titania, or zirconia; a crystalline metal silicate such as zeolite; a metal or alloy such as stainless steel or aluminum; an inorganic carbon compound such as activated carbon or silicon carbide. Among them, as a carrier, silica, alumina, titania, zirconia, or a composite oxide thereof may be used.
[0047] The particle size of the carrier is not particularly limited. For example, when the catalyst is filled into the reaction tube of a (multi) tubular reactor, the particle size may be the desired particle size that can be filled into the reaction tube when the supported catalyst is prepared, that is, the particle size of the supported catalyst may be appropriately set in such a way that the particle size is smaller than the inner diameter of the reaction tube.
[0048] The loading rate of the supported catalyst can be appropriately adjusted from the perspective of facilitating the operation control in the reactor and / or controlling the life of the catalyst, for example, preferably 10% by mass or more, more preferably 20% by mass or more, and preferably 300% by mass or less, more preferably 200% by mass or less. The loading rate of the supported catalyst can be calculated by the following formula: Loading rate of supported catalyst (%) = mass of the supported catalytically active component / mass of the carrier × 100.
[0049] The method for producing the catalyst of the present invention is described below. The catalyst of the present invention is preferably produced by the method for producing the catalyst for producing acrylic acid of the present invention described below. The catalyst of the present invention can be easily produced by the following production method. The catalyst of the present invention may be a catalyst obtained by the method for producing the catalyst for producing acrylic acid of the present invention described below.
[0050] The method for producing a catalyst of the present invention is a method for producing a catalyst for producing acrylic acid from acrolein, comprising the following steps: a step of obtaining a raw material mixed solution containing molybdenum, vanadium and copper; a step of drying the raw material mixed solution to obtain a dried product; a step of molding or supporting the dried product on an inactive carrier to obtain a molded body or a supported body; a step of heating the molded body or the supported body at a temperature T between 380°C and 460°C. C After the aforementioned calcination in an atmosphere with an oxygen concentration exceeding 5% by volume and 21% by volume or less, a cooling time of more than 5 hours from a temperature T C The catalyst production method of the present invention is a catalyst production method for producing acrylic acid from acrolein, comprising the following steps: a step of obtaining a raw material mixed solution containing molybdenum, vanadium and copper; a step of drying the raw material mixed solution to obtain a dried product; a step of drying the dried product at a temperature T between 380°C and 460°C. C After the aforementioned calcination in an atmosphere with an oxygen concentration exceeding 5% by volume and 21% by volume or less, a cooling time of more than 5 hours from a temperature T C The step of cooling to 100°C; and the step of molding or supporting the calcined product obtained through the cooling step on an inactive carrier (hereinafter referred to as "the second production method"). The production method of the catalyst of the present invention is described in detail below.
[0051] In the step of obtaining a raw material mixed solution, a raw material mixed solution containing molybdenum, vanadium and copper is prepared as a raw material of the catalytically active component. As described above, when the catalytically active component contains other metal elements or semi-metal elements in addition to molybdenum, vanadium and copper, it is preferred that the raw material mixed solution also contains these metal elements or semi-metal elements.
[0052] The raw material mixed solution can be prepared by dissolving the molybdenum compound, vanadium compound and copper compound as raw material compounds in a solvent or dispersing them in a dispersion medium. The solvent or dispersion medium of the raw material mixed solution is not particularly limited, and water is conveniently used. Therefore, the raw material mixed solution is preferably obtained in the form of an aqueous solution in which a molybdenum compound, a vanadium compound and a copper compound are dissolved in water or a dispersion (slurry) in which a molybdenum compound, a vanadium compound and a copper compound are dispersed in water, and the aqueous solution or dispersion may also be dissolved or dispersed with compounds of other metal elements and compounds of semi-metal elements.
[0053] The forms of molybdenum compounds, vanadium compounds and copper compounds are not particularly limited, and oxides, hydroxides, halides such as chlorides, bromides and iodides, inorganic salts such as nitrates, carbonates and sulfates, organic acid salts such as formates, acetates, oxalates and citrates, and compounds in any form such as oxyacids or oxyacid salts (e.g., ammonium salts and alkali metal salts of oxyacids) can be used. Among them, as molybdenum compounds, oxyacids or oxyacid salts are preferred, and paramolybdic acid or ammonium paramolybdate is more preferred. As vanadium compounds, oxyacids or oxyacid salts are preferred, and metavanadic acid or ammonium metavanadate is more preferred. As copper compounds, inorganic salts are preferred, and copper nitrate is more preferred. When the catalytically active component contains other metal elements and semi-metal elements on the basis of molybdenum, vanadium and copper, compounds of these metal elements and semi-metal elements in any form can also be used. These compounds can be appropriately selected in consideration of solubility in solvents, etc. The solubility of the raw material mixture can be improved by appropriate stirring and / or heating.
[0054] The amount of the molybdenum compound, the vanadium compound and the copper compound can be appropriately set according to the desired composition of the catalytically active component. For example, in the raw material mixture, the molar ratio Mo / V of molybdenum (Mo) to vanadium (V) is preferably 0.8 or more, more preferably 1.2 or more, and further preferably 1.5 or more, and preferably 6.0 or less, and more preferably 4.0 or less. In addition, in the raw material mixture, the molar ratio Mo / Cu of molybdenum (Mo) to copper (Cu) is preferably 2.4 or more, more preferably 3.0 or more, and preferably 240 or less, more preferably 120 or less, and further preferably 60 or less.
[0055] When the catalytically active component contains other metal elements and semi-metallic elements on the basis of molybdenum, vanadium and copper, the amount of compounds of these metal elements and compounds of semi-metallic elements can also be appropriately set according to the desired composition of the catalytically active component. In the present invention, the catalytically active component preferably also contains tungsten and / or antimony. For example, when the catalytically active component also contains tungsten, the molar ratio Mo / W of molybdenum (Mo) to tungsten (W) is preferably 1.2 or more, more preferably 2.0 or more, further preferably 4.0 or more, further more preferably 6.0 or more, and preferably 240 or less, more preferably 120 or less, further preferably 40 or less, and further more preferably 24 or less. When the catalytically active component also contains antimony, the molar ratio Mo / Sb of molybdenum (Mo) to antimony (Sb) is preferably 2.4 or more, more preferably 3.0 or more, further preferably 4.0 or more, and preferably 240 or less, more preferably 120 or less, and further preferably 60 or less.
[0056] When the catalytically active component further contains tungsten and / or antimony, the form of the tungsten compound and antimony compound as the raw material compound is not particularly limited, and any form of the above compounds can be used. Among them, as the tungsten compound, an oxyacid or an oxyacid salt is preferred, and paratungstic acid or ammonium paratungstate is more preferred. As the antimony compound, antimony trioxide is preferred.
[0057] In the process of obtaining the raw material mixed solution, the molybdenum compound, the vanadium compound and the copper compound may be dissolved or dispersed at once to prepare the raw material mixed solution, or the compounds may be prepared into solutions or dispersions one by one, and then mixed to prepare the raw material mixed solution. In addition, a single solution or mixed solution or a single dispersion or a mixed dispersion of one or two of the molybdenum compound, the vanadium compound and the copper compound may be prepared, and then a single solution or mixed solution or a single dispersion or a mixed dispersion of the remaining one or two compounds may be prepared, and then mixed to prepare the raw material mixed solution. When the catalytically active component contains other metal elements or semi-metal elements on the basis of molybdenum, vanadium and copper, the dissolution and mixing methods of each compound are also not particularly limited, as long as a raw material mixed solution in which all or part of the raw material compounds are dissolved is finally obtained.
[0058] The raw material mixed solution obtained in the step of obtaining the raw material mixed solution may be subjected to the next step, i.e., the drying step, immediately after preparation, or may be subjected to the drying step after continuous stirring. The stirring of the raw material mixed solution may be accompanied by heating. The temperature when the raw material mixed solution is stirred is not particularly limited, and is preferably above 20°C, more preferably above 25°C, and further preferably above 30°C. In addition, it is preferably below 100°C, and more preferably below 90°C. The stirring time when the stirring of the raw material mixed solution is continuously performed is not particularly limited, and may be above 1 hour, above 5 hours, or above 10 hours. In addition, it may be below 360 hours, below 240 hours, or below 120 hours.
[0059] After the process of the raw material mixture, a drying process is performed to dry the raw material mixture. By drying the raw material mixture, a dried product can be obtained. As a drying method, known methods such as heating and decompression can be used. For example, a spray dryer, a drum dryer, etc. can be used to heat the raw material mixture to obtain a powdered dried product, or a box dryer, a tunnel dryer, etc. can be used to heat the raw material mixture under airflow conditions or without ventilation conditions to obtain a block or sheet-shaped dried product. As the gas circulated under airflow conditions or the atmospheric gas under no ventilation conditions, inert gases such as nitrogen, oxygen-containing gases such as air, etc. can be listed. In addition, the raw material mixture can also be concentrated and / or evaporated to dryness to obtain a cake-like solid, and the solid is further heated to obtain a dried product. When drying by heating, it is preferably dried at a temperature of 60°C to 180°C. The drying time is not particularly limited. From the perspective of the manufacturing efficiency of the catalyst, it is preferably more than 1 hour, more preferably more than 2 hours, and preferably less than 48 hours, more preferably less than 24 hours. When drying is performed under reduced pressure, the raw material mixed solution can be dried under reduced pressure using a vacuum dryer or the like to obtain a dried product in a block or powder form.
[0060] The obtained dried product can be pulverized and / or classified as needed to adjust to a suitable particle size. The particle size is not particularly limited, for example, preferably 90% by mass or more of the particles can pass through a sieve with an opening of 500 μm, and more preferably 90% by mass or more of the particles can pass through a sieve with an opening of 300 μm. It should be noted that the material obtained by pulverizing and / or classifying the dried product is also included in the dried product of the present invention.
[0061] In the first manufacturing method, the step of molding the dried product obtained in the drying step or loading it on an inactive carrier to obtain a molded body or a supported body is then performed (hereinafter sometimes referred to as the "first molding / loading step"). When the dried product is molded, the dried product can be molded into a predetermined shape by a known molding method such as an extrusion molding method and a tablet molding method. The shape of the molded body is not particularly limited, and spherical, cylindrical, annular, saddle-shaped, irregular shapes, etc. can be listed. When the dried product is loaded on an inactive carrier, the dried product can be loaded on any inactive carrier having a certain shape to obtain a supported body. The materials of the inactive carrier for loading the dried product are as described above. The shape of the inactive carrier is not particularly limited, and granular, spherical, cylindrical, annular, saddle-shaped, honeycomb, irregular shapes, etc. can be listed.
[0062] When the dried material is shaped or loaded, a molding auxiliary agent and a binder that can improve the moldability / loadability of the dried material, a pore forming agent for forming appropriate pores in the catalyst, etc., which are usually used in the manufacture of the catalyst to achieve these effects (hereinafter sometimes referred to as "auxiliary substances"), can be used, wherein a binder is preferably used. As a specific example of the binder, organic compounds such as ethylene glycol, glycerol, propionic acid, maleic acid, benzyl alcohol, propanol, butanol, phenols, celluloses (such as cellulose, ethyl cellulose) can be listed; water, nitric acid, ammonium nitrate, ammonium carbonate, etc. They can be used only one, or two or more can be used in combination. In addition, in addition to the auxiliary substance, a reinforcing agent can also be used to improve the mechanical strength of the catalyst. As a specific example of the reinforcing agent, various whiskers such as silicon dioxide, aluminum oxide, ceramic fiber, glass fiber, carbon fiber, mineral fiber, metal fiber, silicon carbide, silicon nitride, etc. can be listed, and its crystal structure can be polycrystalline, single crystal, amorphous, preferably polycrystalline or single crystal. In addition, a variety of reinforcing agents different in fiber diameter, fiber length, material, etc. can be used according to the shape of the catalyst and the desired mechanical strength. The reinforcing agent may be added to the raw material mixture or may be blended into the dry product during molding or loading.
[0063] There is no particular limitation on the device used when the dried product is loaded on the inactive carrier, and any known mixing device can be used. For example, the dried product is preferably loaded on the inactive carrier by the centrifugal flow coating method described in Japanese Patent Publication No. 63-200839 or the rocking mixer method described in Japanese Patent Publication No. 2004-136267.
[0064] In the first manufacturing method, the molded body or supported body obtained in the first molding / supporting step is then heated to a temperature T of 380° C. or higher and 460° C. or lower. C The calcination temperature T in the calcination step is CIt is preferably 390°C or higher and preferably 450°C or lower. In the calcination step, the heating rate for heating to the predetermined temperature is preferably 0.1°C / min or higher, more preferably 0.5°C / min or higher, and preferably 15°C / min or lower, more preferably 10°C / min or lower. At the calcination temperature T C The calcination time of calcination can be suitably adjusted between 0.5 hour and 12 hours, for example. The atmosphere during calcination is not particularly limited, and can be carried out under an inert gas atmosphere such as nitrogen, argon, a reducing gas atmosphere such as hydrogen, an oxygen-containing gas atmosphere such as air. Among them, it is preferably carried out under an oxygen-containing gas atmosphere. In addition, the oxygen concentration at this time is preferably more than 1 volume %, and in addition, it is preferably less than 21 volume %.
[0065] In the second production method, the following calcination step is performed: the dried product dried in the drying step or the dried product further pulverized and / or classified is calcined at a temperature T of 380° C. to 460° C. C For the description of the calcination step in the second manufacturing method, please refer to the description of the calcination step in the first manufacturing method.
[0066] The calcining furnace used in the calcining step of the first production method or the second production method is not particularly limited, and commonly used box-type calcining furnaces, tunnel-type calcining furnaces, etc. can be used. The method of measuring the calcining temperature will be described later.
[0067] In the first manufacturing method or the second manufacturing method, the cooling step is performed after the calcination in the calcination step. Specifically, after the dried product, the molded body or the supported body is calcined, in the cooling step, the dried product, the molded body or the supported body is cooled from the temperature T to the temperature T in an atmosphere with an oxygen concentration of more than 5 volume % and less than 21 volume %, for a cooling time of more than 5 hours. C Cool to 100°C. By cooling in this way, the catalyst of the present invention, that is, the catalyst having a diffraction peak at a specific diffraction angle and showing a predetermined peak intensity ratio in the X-ray diffraction analysis of the catalytically active component as described above, can be easily obtained. Therefore, the catalyst obtained by the method for producing the catalyst of the present invention shows a high acrylic acid selectivity and a high acrylic acid yield when acrylic acid is produced by catalytic gas phase oxidation of acrolein. It should be noted that the cooling step is preferably carried out after the calcining step, and preferably, after the dried product, the molded body or the supported body is calcined in a calcining furnace, cooling is then carried out in the furnace.
[0068] In the cooling process, the cooling time and the gas atmosphere in the furnace will significantly affect the crystal structure of the catalytically active component obtained. If this is described in detail, in the calcination process, crystal growth occurs with the solid phase reaction during calcination. Since the temperature does not immediately decrease in the cooling process after calcination, the solid phase reaction continues, thereby further crystal growth. At this time, by controlling the cooling time and oxygen concentration of the cooling process as described above, the crystal growth after calcination (in the cooling process) is slowed down, so that a catalyst having a diffraction peak at a specific diffraction angle and showing a specified peak intensity ratio as described above can be obtained. For example, in the cooling process, by cooling from a temperature T for more than 5 hours, C The catalyst was cooled to 100°C, and the catalytically active component of the obtained catalyst had a peak intensity ratio I(31.5°) / I(22.2°) of 0.03 or more in X-ray diffraction analysis, showing high acrylic acid selectivity and high acrylic acid yield. By setting the oxygen concentration in the atmosphere of the cooling process to more than 5% by volume, the catalytically active component of the obtained catalyst had a peak intensity ratio I(28.2°) / I(22.2°) of 0.50 or less, showing high acrylic acid selectivity and high acrylic acid yield. By setting the oxygen concentration in the atmosphere of the cooling process to 21% by volume or less, the peak intensity ratio I(32.6°) / I(22.2°) of the catalytically active component of the obtained catalyst was 0.40 or less. Since the catalyst is highly active and the reaction temperature can be set low, the result is that the acrylic acid selectivity can be improved. In addition, by setting the calcination temperature in the calcination step to 460°C or less, the catalytically active component of the obtained catalyst has a peak intensity ratio I(31.5°) / I(22.2°) of 0.20 or less and a peak intensity ratio I(32.6°) / I(22.2°) of 0.40 or less. Since the catalyst has high activity and the reaction temperature can be set low, the acrylic acid selectivity can be improved.
[0069] In the cooling process, the oxygen concentration in the atmosphere is preferably 6% by volume or more, more preferably 8% by volume or more, and further preferably 10% by volume or more. In addition, the upper limit of the oxygen concentration in the atmosphere is preferably 20% by volume or less, and more preferably 18% by volume or less.
[0070] In the cooling process, from the temperature T C The cooling time to 100° C. is preferably more than 5 hours, more preferably 5.2 hours or more, and even more preferably 6 hours or more. C The upper limit of the cooling time to 100° C. is not particularly limited, but is preferably 12 hours or less, and more preferably 10 hours or less, from the viewpoint of improving the production efficiency of the catalyst.
[0071] In the cooling step, it is also preferred to cool from the temperature T to the C The catalyst of the present invention can be easily obtained by cooling to 300°C, preferably for 3.5 hours or more. In addition, the obtained catalyst shows high acrylic acid selectivity and high acrylic acid yield. C The upper limit of the cooling time to 300° C. is not particularly limited, but is preferably 10 hours or less, more preferably 8 hours or less, and even more preferably 6 hours or less from the viewpoint of improving the production efficiency of the catalyst.
[0072] The cooling time in the cooling step can be easily adjusted by, for example, keeping the furnace in a windless state, blowing cold air into the furnace, adjusting the heating of the heater, circulating the atmosphere control gas in the furnace and controlling the flow rate, etc. C The average temperature drop rate when cooling to 100°C is preferably 0.38°C / min or more, more preferably 0.43°C / min or more, and preferably 1.2°C / min or less, more preferably 1.0°C / min or less. C The average temperature drop rate when cooling to 300°C is preferably 0.1°C / min or more, more preferably 0.2°C / min or more, and is preferably 1.0°C / min or less, more preferably 0.9°C / min or less.
[0073] The calcination temperature in the calcination step and the cooling temperature in the cooling step can be obtained as follows. For example, a dried object, a molded body or a support to be calcined can be piled up in a calcination furnace, a temperature measuring sensor can be set near the center of the dried object, molded body or support layer, and the calcination step and the cooling step can be carried out in this state, and the calcination temperature and the cooling temperature can be obtained by measuring the temperature in each step.
[0074] In the first production method, the calcined product obtained after the cooling step can be used directly as a catalyst. In the first production method, the dried product is molded or supported on an inactive carrier and heated to a temperature T C The calcination is carried out under the conditions of calcination, so the catalyst obtained after the calcination step and the cooling step is obtained in the form of a shaped catalyst or a supported catalyst.
[0075] In the second manufacturing method, after the cooling step, a step of molding or loading the calcined product obtained through the cooling step on an inactive carrier is performed (hereinafter sometimes referred to as the "second molding / loading step"). Thus, in the second manufacturing method, the catalyst can also be obtained in the form of a molded catalyst or a loaded catalyst. For the description of the molding method and the loading method in the second molding / loading step, please refer to the description of the molding method and the loading method in the first molding / loading step of the first manufacturing method.
[0076] In the second manufacturing method, the C Next, the molded body or the supported body obtained in the second molding / supporting step is subjected to heat treatment. The heating temperature (T h ) As long as the temperature T C The following are not particularly limited, preferably T C The temperature is preferably below -30°C, and preferably above 100°C, more preferably above 200°C. The heat treatment time can be appropriately adjusted between 0.5 hours and 12 hours, for example. The atmosphere during the heat treatment is not particularly limited, and the heat treatment can be carried out in an inert gas atmosphere such as nitrogen, argon, a reducing gas atmosphere such as hydrogen, or an oxygen-containing gas atmosphere such as air. Among them, the heat treatment is preferably carried out in an oxygen-containing gas atmosphere.
[0077] In the second manufacturing method, the heat treatment after the second molding / loading step is not performed for the purpose of controlling the growth of the crystal structure of the catalytically active component, but is performed for the purpose of, for example, volatilizing or decomposing the binder used in molding and loading as required. As described above, the heat treatment after the second molding / loading step is not performed for the purpose of controlling the growth of the crystal structure of the catalytically active component, so there is no particular restriction on the cooling time and cooling rate during cooling after the heat treatment. However, from the perspective of catalyst manufacturing efficiency, at a temperature T higher than 100°C, the cooling time and cooling rate are preferably 100°C. h When heat treatment is carried out at temperature T h The cooling time to 100°C is preferably 12 hours or less, more preferably 10 hours or less, and further preferably 8 hours or less. In addition, the cooling rate at this time is preferably 0.45°C / minute or more, more preferably 0.55°C / minute or more, and further preferably 0.68°C / minute or more. The atmosphere during cooling after the above-mentioned heat treatment is not particularly limited, and can be carried out under an inert gas atmosphere such as nitrogen, argon, a reducing gas atmosphere such as hydrogen, or an oxygen-containing gas atmosphere such as air.
[0078] The catalyst of the present invention and the catalyst obtained by the production method of the present invention are useful as a catalyst for producing acrylic acid from acrolein. The production method of acrylic acid of the present invention comprises the following steps: in the presence of the catalyst of the present invention or the catalyst obtained by the production method of the catalyst of the present invention, acrolein is subjected to catalytic gas phase oxidation to obtain acrylic acid. The production method of acrylic acid of the present invention may comprise the following steps: a step of obtaining the catalyst by the production method of the present invention; and a step of obtaining acrylic acid by catalytic gas phase oxidation of acrolein in the presence of the catalyst obtained by the above step. According to the production method of acrylic acid of the present invention, acrylic acid can be efficiently produced from acrolein.
[0079] The reaction conditions of the manufacturing method of acrylic acid of the present invention are not particularly limited, as long as they are the conditions commonly used in such reactions, they can all be implemented. As the raw material gas, for example, a mixed gas consisting of 1 to 15 volume %, preferably 4 to 12 volume % of acrolein, 0.5 to 25 volume %, preferably 2 to 20 volume % of molecular oxygen, 0 to 30 volume %, preferably 0 to 25 volume % of water vapor, and the balance being inert gases such as nitrogen can be used. In addition, acrolein-containing gas obtained by dehydration reaction of glycerol, catalytic gas phase oxidation reaction of propylene, or a mixed gas obtained by adding air or oxygen to the acrolein-containing gas as required can also be used as the raw material gas. As the reaction temperature, it can be appropriately set within the temperature range of 200°C to 400°C. As the heating means, known heating means such as molten salt and electric heater can be used.
[0080] The reactor may be a fixed bed reactor (a (multi) tubular reactor), a fluidized bed reactor, a moving bed reactor or other known reactors, and a catalyst may be arranged or filled in these reactors for use. When a fixed bed reactor is used as the reactor, the space velocity of the raw gas introduced into the fixed bed reactor is preferably 300 hr -1 More than 500 hr -1 More than 1000 hr -1 More than, preferably 10000hr -1 Below, more preferably 8000hr -1 Below, more preferably 5000hr -1 Herein, the space velocity refers to the amount of the raw material gas passing through the catalyst layer per unit time (the converted value under the standard temperature and pressure (STP) of 0°C and 1 bar).
[0081] Through the above reaction, an acrylic acid-containing gas is obtained as a reaction product. By condensing the acrylic acid-containing gas and trapping the solvent, a crude acrylic acid-containing liquid can be obtained. The crude acrylic acid-containing liquid can be purified by known purification means (e.g., distillation, crystallization, stripping, extraction) as needed to obtain high-purity acrylic acid.
[0082] This application claims the benefit of priority of Japanese Patent Application No. 2020-148124 filed on September 3, 2020. The entire contents of the specification of Japanese Patent Application No. 2020-148124 filed on September 3, 2020 are incorporated herein by reference.
[0083] Example
[0084] The present invention is described in more detail below by enumerating examples, but the present invention is certainly not limited by the following examples, and can be implemented by changing within the scope of the subject matter described above / below, and they are all included in the technical scope of the present invention. It should be noted that, in the following description, "parts" means "parts by mass" unless otherwise stated.
[0085] (1) Preparation of catalyst
[0086] (1-1) Preparation Example 1 (Preparation Example of Catalyst 1 Used in Example 1)
[0087] While stirring 1000 parts of pure water, heat it and dissolve 100 parts of ammonium paramolybdate, 22.1 parts of ammonium metavanadate and 12.8 parts of ammonium paratungstate. Separately, stir 100 parts of pure water and heat it and dissolve 11.4 parts of copper nitrate therein. Mix the two solutions obtained, add 4.1 parts of antimony trioxide thereto, and obtain a raw material mixture. The raw material mixture is spray dried, and the obtained dry matter is sieved to a size of less than 250 μm to obtain a dry powder. 300 parts of a spherical carrier formed of α-alumina with an average particle size of 4 mm are added to a centrifugal flow coating device, and then pure water as a binder is added to impregnate the carrier, and then the dry powder is loaded on the carrier, and then dried with hot air at about 90°C to obtain a catalyst precursor. The obtained catalyst precursor is placed in a crucible and placed in a box-type calcining furnace. The oxygen concentration in the furnace is adjusted to 10% by volume, and the temperature is raised at 2°C / min from room temperature, and then calcined at 380°C for 6.0 hours. After that, the oxygen concentration in the furnace was adjusted to 18% by volume, and the furnace was cooled from 380°C to 300°C in 3.0 hours and from 380°C to 100°C in 5.3 hours to obtain Catalyst 1. The loading rate of Catalyst 1 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 4.0 W 1.0 Cu 1.0 Sb 0.6 It should be noted that the loading rate is calculated by the following formula: loading rate (mass %)=(mass of the supported catalyst powder (g)) / (mass of the carrier used (g))×100.
[0088] (1-2) Preparation Example 2 (Preparation Example of Catalyst 2 Used in Example 2)
[0089] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 24.9 parts of ammonium metavanadate, 17.9 parts of ammonium paratungstate, 17.1 parts of copper nitrate, and 3.4 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 14% by volume, and the mixture was cooled from 400°C to 300°C in 3.5 hours, and then cooled from 400°C to 100°C in 6.0 hours, to obtain Catalyst 2. The loading rate of Catalyst 2 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 4.5 Cu 1.5 W 1.4 Sb 0.5 .
[0090] (1-3) Preparation Example 3 (Preparation Example of Catalyst 3 Used in Example 3)
[0091] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 22.1 parts of ammonium metavanadate, 15.3 parts of ammonium paratungstate, 6.8 parts of copper nitrate, and 4.8 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 410°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was cooled from 410°C to 300°C in 4.0 hours, and then cooled from 410°C to 100°C in 6.5 hours, to obtain Catalyst 3. The loading rate of Catalyst 3 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 4.0 Cu 0.6 W 1.2 Sb 0.7 .
[0092] (1-4) Preparation Example 4 (Preparation Example of Catalyst 4 Used in Example 4)
[0093] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 22.1 parts of ammonium metavanadate, 12.8 parts of ammonium paratungstate, 14.8 parts of copper nitrate, and 3.4 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the mixture was cooled from 400°C to 300°C in 3.5 hours, and then cooled from 400°C to 100°C in 6.0 hours, to obtain Catalyst 4. The loading rate of Catalyst 4 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 4.0 Cu 1.3 W 1.0 Sb 0.5 .
[0094] (1-5) Preparation Example 5 (Preparation Example of Catalyst 5 Used in Example 5)
[0095] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 24.9 parts of ammonium metavanadate, 15.3 parts of ammonium paratungstate, 18.3 parts of copper nitrate, and 4.1 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 420°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 12% by volume, and the mixture was cooled from 420°C to 300°C in 4.5 hours, and then cooled from 420°C to 100°C in 7.0 hours, to obtain Catalyst 5. The loading rate of Catalyst 5 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 4.5 Cu 1.6 W 1.2 Sb 0.6 .
[0096] (1-6) Preparation Example 6 (Preparation Example of Catalyst 6 Used in Example 6)
[0097] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 22.1 parts of ammonium metavanadate, 12.8 parts of ammonium paratungstate, 20.5 parts of copper nitrate, and 3.4 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 430°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 12% by volume, and the temperature was cooled from 430°C to 300°C in 5.0 hours, and then cooled from 430°C to 100°C in 7.5 hours, to obtain Catalyst 6. The loading rate of Catalyst 6 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 4.0 Cu 1.8 W 1.0 Sb 0.5 .
[0098] (1-7) Preparation Example 7 (Preparation Example of Catalyst 7 Used in Example 7)
[0099] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 19.3 parts of ammonium metavanadate, 12.8 parts of ammonium paratungstate, 34.2 parts of copper nitrate, and 3.4 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 420°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 21% by volume, and the mixture was cooled from 420°C to 300°C in 4.5 hours, and then cooled from 420°C to 100°C in 7.0 hours, to obtain Catalyst 7. The loading rate of Catalyst 7 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 3.5 Cu 3.0 W 1.0 Sb 0.5 .
[0100] (1-8) Preparation Example 8 (Preparation Example of Catalyst 8 Used in Example 8)
[0101] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 33.1 parts of ammonium metavanadate, 12.8 parts of ammonium paratungstate, 22.8 parts of copper nitrate, and 2.8 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the mixture was cooled from 400°C to 300°C in 3.5 hours, and then cooled from 400°C to 100°C in 6.0 hours, to obtain Catalyst 8. The loading rate of Catalyst 8 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 6.0 Cu 2.0 W 1.0 Sb 0.4 .
[0102] (1-9) Preparation Example 9 (Preparation Example of Catalyst 9 Used in Example 9)
[0103] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 16.6 parts of ammonium metavanadate, 10.2 parts of ammonium paratungstate, 3.4 parts of copper nitrate, and 2.1 parts of antimony trioxide were used, and a catalyst precursor was obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 440°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 20% by volume, and the temperature was cooled from 440°C to 300°C in 6.0 hours, and then cooled from 440°C to 100°C in 8.5 hours, to obtain Catalyst 9. The loading rate of Catalyst 9 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 3.0 Cu 0.3 W 0.8 Sb 0.3 .
[0104] (1-10) Preparation Example 10 (Preparation Example of Catalyst 10 Used in Example 10)
[0105] A catalyst precursor was obtained in the same manner as in Preparation Example 3. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 1 volume %, and the temperature was raised from room temperature at 2°C / min, and then calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10 volume %, and the mixture was cooled from 400°C to 300°C in 3.5 hours, and then from 400°C to 100°C in 6.0 hours, to obtain Catalyst 10. The loading rate of Catalyst 10 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 4.0 Cu0.6 W 1.2 Sb 0.7 .
[0106] (1-11) Preparation Example 11 (Preparation Example of Catalyst 11 Used in Example 11)
[0107] A catalyst precursor was obtained in the same manner as in Preparation Example 8. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 21% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the mixture was cooled from 400°C to 300°C in 3.5 hours, and then from 400°C to 100°C in 6.0 hours, to obtain Catalyst 11. The loading rate of Catalyst 11 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 6.0 Cu 2.0 W 1.0 Sb 0.4 .
[0108] (1-12) Preparation Example 12 (Preparation Example of Catalyst 12 Used in Example 12)
[0109] The catalyst precursor was obtained in the same manner as in Preparation Example 6. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 420°C for 1.0 hour. Thereafter, the oxygen concentration in the furnace was adjusted to 6% by volume, and the catalyst was cooled from 420°C to 300°C in 4.5 hours and from 420°C to 100°C in 7.0 hours to obtain Catalyst 12. The loading rate of Catalyst 12 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 4.0 Cu 1.8 W 1.0 Sb 0.5 .
[0110] (1-13) Preparation Example 13 (Preparation Example of Catalyst 13 Used in Example 13)
[0111] While stirring 1000 parts of pure water, heat it and dissolve 100 parts of ammonium paramolybdate, 33.1 parts of ammonium metavanadate and 12.8 parts of ammonium paratungstate. Separately, while stirring 100 parts of pure water, heat it and dissolve 22.8 parts of copper nitrate therein. The two solutions obtained are mixed, and 8.2 parts of cobalt nitrate and 2.8 parts of antimony trioxide are added thereto to obtain a raw material mixed solution. Otherwise, a catalyst precursor is obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor is placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace is adjusted to 10% by volume. After heating at 2°C / min from room temperature, the mixture is calcined at 390°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace is adjusted to 10% by volume, and the mixture is cooled from 390°C to 300°C in 3.5 hours, and then cooled from 390°C to 100°C in 6.0 hours to obtain Catalyst 13. The loading rate of Catalyst 13 is 30% by mass, and the metal element composition other than oxygen is Mo: 12 V 6.0 Cu 2.0 W 1.0 Sb 0.4 Co 0.6 .
[0112] (1-14) Preparation Example 14 (Preparation Example of Catalyst 14 Used in Example 14)
[0113] In Preparation Example 13, 0.4 parts of magnesium oxide was used instead of 8.2 parts of cobalt nitrate, and a catalyst precursor was obtained in the same manner as in Preparation Example 13. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the mixture was cooled from 400°C to 300°C in 3.5 hours, and then cooled from 400°C to 100°C in 6.0 hours, to obtain Catalyst 14. The loading rate of Catalyst 14 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 6.0 Cu 2.0 W 1.0 Sb 0.4 Mg 0.2 .
[0114] (1-15) Preparation Example 15 (Preparation Example of Catalyst 15 Used in Example 15)
[0115] While stirring 1000 parts of pure water, heat it and dissolve 100 parts of ammonium paramolybdate, 22.1 parts of ammonium metavanadate and 12.8 parts of ammonium paratungstate. Separately, while stirring 100 parts of pure water, heat it and dissolve 20.5 parts of copper nitrate therein. The two solutions obtained are mixed, and 6.3 parts of aluminum oxide and 3.4 parts of antimony trioxide are added thereto to obtain a raw material mixed solution. Otherwise, a catalyst precursor is obtained in the same manner as in Preparation Example 1. The obtained catalyst precursor is placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace is adjusted to 10% by volume. After heating at 2°C / min from room temperature, the mixture is calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace is adjusted to 10% by volume, and the mixture is cooled from 400°C to 300°C in 3.5 hours and then cooled from 400°C to 100°C in 6.0 hours to obtain Catalyst 15. The loading rate of Catalyst 15 is 30% by mass, and the metal element composition other than oxygen is Mo. 12 V 4.0 Cu 1.8 W 1.0 Sb 0.5 Al 1.3 .
[0116] (1-16) Preparation Example 16 (Preparation Example of Catalyst 16 Used in Example 16)
[0117] In Preparation Example 1, as raw materials, 100 parts of ammonium paramolybdate, 33.1 parts of ammonium metavanadate, 12.8 parts of ammonium paratungstate, 22.8 parts of copper nitrate, and 2.8 parts of antimony trioxide were used, and a dry powder was obtained in the same manner as in Preparation Example 1. The obtained dry powder was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 400°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the mixture was cooled from 400°C to 300°C in 3.5 hours, and then cooled from 400°C to 100°C in 6.0 hours to obtain a calcined product. The obtained calcined product was pulverized with a ball mill to obtain a calcined powder. 300 parts of a spherical carrier made of α-alumina with an average particle size of 4 mm were added to a centrifugal flow coating device, and then a 1% by mass hydroxyethyl cellulose solution as a binder was added to impregnate the carrier. After the calcined powder was attached to the carrier, it was dried with hot air at about 90°C to obtain a supported product. The supported product was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised at 2°C / min from room temperature, and then calcined at 300°C for 2.0 hours, and cooled from 300°C to 100°C in 2.5 hours to obtain a catalyst 16. The supported rate of the catalyst 16 was 30% by mass, and the metal element composition other than oxygen was Mo: 12 V 6.0 Cu 2.0 W 1.0 Sb0.4 .
[0118] (1-17) Preparation Example 17 (Preparation Example of Catalyst 17 Used in Comparative Example 1)
[0119] A catalyst precursor was obtained in the same manner as in Preparation Example 9. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 440°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 21% by volume, and the mixture was cooled from 440°C to 300°C in 2.0 hours, and then from 440°C to 100°C in 4.0 hours, to obtain Catalyst 17. The loading rate of Catalyst 17 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 3.0 Cu 0.3 W 0.8 Sb 0.3 .
[0120] (1-18) Preparation Example 18 (Preparation Example of Catalyst 18 Used in Comparative Example 2)
[0121] A catalyst precursor was obtained in the same manner as in Preparation Example 9. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 440°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 25% by volume, and the mixture was cooled from 440°C to 300°C in 6.0 hours, and then from 440°C to 100°C in 8.5 hours, to obtain Catalyst 18. The loading rate of Catalyst 18 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 3.0 Cu 0.3 W 0.8 Sb 0.3 .
[0122] (1-19) Preparation Example 19 (Preparation Example of Catalyst 19 Used in Comparative Example 3)
[0123] A catalyst precursor was obtained in the same manner as in Preparation Example 9. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 440°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 30% by volume, and the mixture was cooled from 440°C to 300°C in 6.0 hours, and then from 440°C to 100°C in 8.5 hours, to obtain Catalyst 19. The loading rate of Catalyst 19 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 3.0 Cu 0.3 W 0.8 Sb0.3 .
[0124] (1-20) Preparation Example 20 (Preparation Example of Catalyst 20 Used in Comparative Example 4)
[0125] The catalyst precursor was obtained in the same manner as in Preparation Example 8. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 420°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 5% by volume, and the mixture was cooled from 420°C to 300°C in 4.5 hours, and then from 420°C to 100°C in 7.0 hours, to obtain Catalyst 20. The loading rate of Catalyst 20 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 6.0 Cu 2.0 W 1.0 Sb 0.4 .
[0126] (1-21) Preparation Example 21 (Preparation Example of Catalyst 21 Used in Comparative Example 5)
[0127] The catalyst precursor was obtained in the same manner as in Preparation Example 8. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 480°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the mixture was cooled from 480°C to 300°C in 7.0 hours and from 480°C to 100°C in 9.5 hours to obtain Catalyst 21. The loading rate of Catalyst 21 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 6.0 Cu 2.0 W 1.0 Sb 0.4 .
[0128] (1-22) Preparation Example 22 (Preparation Example of Catalyst 22 Used in Comparative Example 6)
[0129] A catalyst precursor was obtained in the same manner as in Preparation Example 8. The obtained catalyst precursor was placed in a crucible, and in a box-type calcining furnace, the oxygen concentration in the furnace was adjusted to 10% by volume, and the temperature was raised from room temperature at 2°C / min, and then calcined at 370°C for 6.0 hours. Thereafter, the oxygen concentration in the furnace was adjusted to 10% by volume, and the mixture was cooled from 370°C to 300°C in 3.0 hours, and then from 370°C to 100°C in 5.0 hours, to obtain Catalyst 22. The loading rate of Catalyst 22 was 30% by mass, and the metal element composition other than oxygen was Mo. 12 V 6.0 Cu 2.0 W 1.0 Sb0.4 .
[0130] Tables 1 and 2 show the preparation conditions and catalyst compositions of the catalysts in the above-mentioned preparation examples.
[0131] (2) X-ray diffraction analysis of catalytically active components
[0132] The catalyst obtained in each preparation example was shaken in a sealed container to peel off the catalytic active components supported on the surface of the carrier, and then sieved to obtain a powder with a size of 150 μm or less. The obtained powder was subjected to X-ray diffraction using a Cu-Kα ray (X-ray output: 40 mA-45 kV, Kα1 ray wavelength: ) were subjected to X-ray diffraction analysis. The results of X-ray diffraction analysis of the catalytically active components of each catalyst are shown in Tables 3 and 4.
[0133] (3) Production of acrylic acid from acrolein
[0134] The catalyst was filled into a SUS U-shaped reaction tube with a total length of 300 mm and an inner diameter of 18 mm in such a way that the layer length was 100 mm. -1 A mixed gas consisting of 2% by volume of acrolein, 3% by volume of oxygen, 10% by volume of water vapor, and 85% by volume of nitrogen was introduced at a space velocity of (STP) to carry out an acrolein oxidation reaction. The reaction temperature was adjusted so that the conversion rate of acrolein was about 93.5%. The performance evaluation results of each catalyst are shown in Tables 3 and 4.
[0135] [Table 1]
[0136]
[0137] [Table 2]
[0138]
[0139] [Table 3]
[0140]
[0141] [Table 4]
[0142]
[0143] In the X-ray diffraction analysis using Cu-Kα rays of catalysts 1 to 16 used in the examples, the catalytically active components have diffraction peaks at 2θ=22.2°±0.3°, 28.2°±0.3°, 31.5°±0.3°, and 32.6°±0.3°, and the peak intensity ratio I(28.2°) / I(22.2°) is greater than 0.20 and less than 0.50, the peak intensity ratio I(31.5°) / I(22.2°) is greater than 0.03 and less than 0.20, and the peak intensity ratio I(32.6°) / I(22.2°) is greater than 0.03 and less than 0.40. On the other hand, in the X-ray diffraction analysis using Cu-Kα rays of catalysts 17 to 22 used in the comparative examples, although the catalytic active components have diffraction peaks at 2θ=22.2°±0.3°, 28.2°±0.3°, 31.5°±0.3°, and 32.6°±0.3°, the peak intensity ratio I(31.5°) / I(22.2°) of catalyst 17 is less than 0.03, and the peak intensity ratios of catalysts 18 and 19 are less than 0.03. I(32.6°) / I(22.2°) exceeded 0.40, the peak intensity ratio I(28.2°) / I(22.2°) of catalyst 20 exceeded 0.50, the peak intensity ratio I(31.5°) / I(22.2°) of catalyst 21 exceeded 0.20, the peak intensity ratio I(32.6°) / I(22.2°) exceeded 0.40, and the peak intensity ratio I(28.2°) / I(22.2°) of catalyst 22 was less than 0.20. As a result, when acrylic acid was produced by catalytic gas phase oxidation reaction of acrolein using each catalyst, Examples 1 to 16 showed higher acrylic acid selectivity and higher acrylic acid yield than Comparative Examples 1 to 6.
[0144] Catalysts 1 to 16 used in Examples were prepared by drying a raw material mixture of catalytically active components at a temperature T of 380° C. to 460° C. C The mixture is calcined at 400 °C and then cooled from the temperature T to 500 °C in an atmosphere with an oxygen concentration of more than 5% by volume and less than 21% by volume. C Cool to 100°C. In addition, it takes more than 3 hours to cool from temperature T C The catalyst 17 used in the comparative example was cooled to 300°C. As a result, a catalyst showing high acrylic acid selectivity and high acrylic acid yield was obtained as described above. On the other hand, in the cooling step after calcination during catalyst preparation, the catalyst 17 was cooled from the temperature T to the temperature T in less than 5 hours. C Cooling to 100°C, from temperature T in less than 3 hours C Cool to 300°C. Catalysts 18 to 20 were subjected to the cooling process after calcination at an oxygen concentration of less than 5% by volume or more than 21% by volume during catalyst preparation. Catalyst 21 was subjected to the calcination process at a temperature TC The temperature of the catalyst 22 is set to be higher than 460°C. C The temperature was set to be lower than 380° C. As a result, as described above, the obtained catalyst showed acrylic acid selectivity and acrylic acid yield lower than those of the Examples.
[0145] Industrial Applicability
[0146] The catalyst of the present invention can produce acrylic acid from acrolein. The obtained acrylic acid can be used as a raw material for various acrylic acid derivative products such as acrylic acid ester, sodium polyacrylate, acrylic resin, etc.
Claims
1. A method for producing a catalyst for producing acrylic acid, which is a method for producing a catalyst for producing acrylic acid from acrolein, characterized in that: The process has the following steps: A step of obtaining a raw material mixed solution containing molybdenum, vanadium and copper; The step of drying the raw material mixed liquid to obtain a dried product; The step of molding or supporting the dried product on an inactive carrier to obtain a molded body or a supported body; The molded body or the support is heated to a temperature T between 380°C and 460°C. C The next calcination process; and After the calcination, the mixture is cooled from the temperature T to the temperature T in an atmosphere with an oxygen concentration of more than 5% by volume and less than 21% by volume for 5 hours or more. C Cooling process to 100°C.
2. The method for producing a catalyst for producing acrylic acid according to claim 1, wherein: In the cooling process, the temperature T is cooled from the above temperature T by more than 3 hours. C Cool to 300°C.
3. A method for producing a catalyst for producing acrylic acid, which is a method for producing a catalyst for producing acrylic acid from acrolein, characterized in that: The process has the following steps: A step of obtaining a raw material mixed solution containing molybdenum, vanadium and copper; The step of drying the raw material mixed liquid to obtain a dried product; The dried product is heated at a temperature T between 380°C and 460°C. C The next calcination process; After the calcination, the mixture is cooled from the temperature T to the temperature T in an atmosphere with an oxygen concentration of more than 5% by volume and less than 21% by volume for 5 hours or more. C A step of cooling to 100°C; and A step of molding or supporting the calcined product obtained through the cooling step on an inactive carrier.
4. The method for producing a catalyst for producing acrylic acid according to claim 3, wherein: In the cooling process, the temperature T is cooled from the above temperature T by more than 3 hours. C Cool to 300°C.
5. A method for producing acrylic acid, characterized in that: The method comprises the step of obtaining acrylic acid by catalytically oxidizing acrolein in the presence of the catalyst obtained by the production method according to any one of claims 1 to 4.