Silver-palladium alloy powder suitable for making MLCC slurry and preparation process thereof

By rationally proportioning silver powder and palladium powder, and using ball milling technology and high-temperature treatment, the problems of low alloying degree and uneven particle size distribution of silver-palladium alloy powder were solved, and silver-palladium alloy powder with good alloying degree and morphology was prepared. Meet the technical requirements of MLCC slurry.

CN116037932BActive Publication Date: 2024-10-25DALIAN OVERSEAS HUASHENG ELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211627741.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-10-25
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

In the existing technology, silver-palladium alloy powder has low alloy degree and uneven particle size distribution, making it difficult to meet the technical requirements of MLCC slurry.

Method used

By properly proportioning silver powder and palladium powder, using ball milling technology and high-temperature treatment, combined with grinding aids and surfactants, the particle size distribution and dispersion of silver-palladium alloy powder are adjusted to prepare silver with good alloying degree and morphology. Palladium alloy powder.

Benefits of technology

The particle size distribution uniformity and dispersion of the silver-palladium alloy powder is achieved, meeting the technical requirements of MLCC slurry, and improving the purity and applicability of the alloy powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116037932B_ABST
    Figure CN116037932B_ABST
Patent Text Reader

Abstract

The present invention provides a silver-palladium alloy powder suitable for MLCC slurry production and a preparation process thereof. The raw materials of the silver-palladium alloy powder are composed of the following raw materials in mass percentage: 5-30% silver powder, the silver powder is a nano-spherical powder, and the particle size is 1 / 4-1 / 2 of the target silver-palladium alloy powder particle size; 2-10% palladium powder, the palladium powder is a nano-spherical powder, and the particle size is 1 / 4-1 / 2 of the target silver-palladium alloy powder particle size; 30-80% grinding aid; 2-5% dispersant; 0.5-2% surfactant; 20-60% pure water. At the same time, the present invention also provides a process for preparing the silver-palladium alloy powder. The silver-palladium alloy powder and the preparation process thereof provided by the present invention have good alloying degree, uniform particle size distribution and dispersibility, and the powder morphology is approximately spherical. The silver-palladium alloying degree can be appropriately adjusted according to the slurry requirements, which is suitable for the technical requirements of MLCC slurry production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of conductive pastes, and in particular to a silver-palladium alloy powder suitable for making MLCC pastes and a preparation process thereof. Background Art

[0002] Ceramic capacitors occupy more than 60% of the capacitor market due to their small size, high capacity and low cost, while the shipment volume of chip multilayer ceramic capacitors (MLCC; Multi-layer Ceramic Capacitors) accounts for more than 90% of the entire ceramic capacitors, and the annual production capacity has maintained a growth rate of 20-30% since 2018. With the rapid development of passive components, some products of precious metal passive components have been replaced by base metal conductive paste products, but some products still use precious metal conductive paste as their key raw materials, such as aerospace-grade, military-grade multilayer ceramic capacitors, medium- and high-voltage multilayer ceramic capacitors, etc., for which conductive pastes matching these MLCCs are required.

[0003] Silver-palladium paste is widely used in hybrid integrated circuits as interconnected conductive strips and welding areas of circuits due to its excellent sintering resistance, weldability, anti-migration ability and moderate price. It is also widely used as electrodes in external components such as chip resistors, MLCC capacitors, and chip inductors. As the key raw material of silver-palladium paste, silver-palladium alloy powder not only has the advantages of silver and palladium, but also overcomes the disadvantages of silver's inability to burn and silver migration at high temperatures. Therefore, the performance of silver-palladium alloy powder directly determines the characteristics of silver-palladium paste. There are many public data on the production of nano silver and palladium powder, but there are few public data on the relevant silver-palladium alloy powder process and application patents. Chinese patent CN110714133 mentions a method for synthesizing silver-palladium alloy using silver powder and palladium powder under high temperature and high pressure, but the silver-palladium alloy obtained by this process has a low alloying degree and is similar in quality to the silver-palladium co-precipitation powder obtained by chemical method. In addition, the particle size distribution of silver-palladium powder cannot be accurately controlled, and the alloy powder produced is difficult to use directly.

[0004] Therefore, there is an urgent need in the art to provide a silver-palladium alloy powder having good alloying degree, narrow particle size distribution and excellent dispersion and a preparation process thereof. Summary of the invention

[0005] In view of the above-mentioned technical problems of poor alloy degree and uneven particle size distribution of existing silver-palladium powder, the present invention provides a silver-palladium alloy powder with good alloy degree, particle size distribution and dispersibility and its preparation process. The present invention mainly improves the preparation process of silver-palladium alloy powder by reasonable raw material ratio, so that its alloy degree, dispersibility and morphology are all suitable for the technical requirements of MLCC slurry production.

[0006] The technical means adopted by the present invention are as follows:

[0007] A silver-palladium alloy powder suitable for making MLCC slurry, the raw materials are composed of the following raw materials in percentage by mass:

[0008] 5-30% silver powder, wherein the silver powder is nano-spherical powder, and the particle size is 1 / 4-1 / 2 of the target silver-palladium alloy powder particle size;

[0009] 2-10% palladium powder, wherein the palladium powder is a nano-spherical powder, and the particle size is 1 / 4-1 / 2 of the target silver-palladium alloy powder particle size; preferably, the ratio of silver powder to palladium powder can be adjusted within a certain range to obtain silver-palladium alloys of different ratios, and the ratio of silver to palladium can be adjusted between 9:1 and 7:3;

[0010] Grinding aid 30-80%;

[0011] Dispersant 2-5%;

[0012] Surfactant 0.5-2%;

[0013] Pure water 20-60%.

[0014] Furthermore, the grinding aid is one or a mixture of lithium tantalate, artificial diamond powder, aluminum oxide, silicon oxide, cerium oxide, chromium oxide, tungsten carbide or colloidal silicon dioxide.

[0015] Furthermore, the dispersant is one or a mixture of maleic acid-acrylic acid copolymer, sodium polyacrylate, polyoxyethylene alcohol, polycarboxylic acid sodium salt dispersant, polyurethane block copolymer or acrylic acid-styrene copolymer.

[0016] Furthermore, the surfactant is a cationic surfactant, an anionic surfactant or a nonionic surfactant, the cationic surfactant is one or a mixture of cetyltrimethylammonium bromide, dodecyltrimethylammonium chloride or dodecyltrimethylbenzylammonium chloride; the anionic surfactant is one or a mixture of sodium dodecylbenzene sulfonate, sodium lauryl sarcosinate, sodium lauryl sarcosinate; the nonionic surfactant is one or a mixture of nonylphenol polyoxyethylene ether, polyethylene glycol, and fatty alcohol polyoxyethylene ether.

[0017] The present invention also discloses a preparation process of the silver-palladium alloy powder suitable for making MLCC slurry, comprising the following steps:

[0018] Step 1: Weigh the materials according to the preset ratio and introduce them into the alumina tank;

[0019] Step 2: Add an appropriate amount of zirconium dioxide ceramic beads with a particle size of 5 mm into the alumina can;

[0020] Step 3: Fix the alumina can on the ball mill, set the speed to 300-500 RPM / min, and ball-mill for 1-2 hours;

[0021] Step 4: After ball milling, use a 10-mesh filter to filter out the zirconium dioxide ceramic beads;

[0022] Step 5: Spread the filtered material onto a surface dish and dry at 50-100°C for 2-5 hours;

[0023] Step 6: Place the dried material mixture into a sintering furnace, raise the temperature to 600-800°C at a heating rate of 5-20°C / min, maintain for 20-60min, and then cool it down to room temperature at a cooling rate of 5-20°C / min;

[0024] Step 7: After the material cools down to room temperature, re-introduce the mixed material and 50g pure water into the ball mill without adding zirconium oxide ceramic beads, set the ball mill speed to 100-300RPM, the ball milling time to 1-2h, and use a 100-mesh filter to filter out the grinding aid;

[0025] Step 8: Prepare 0.1 mol / L nitric acid solution, dissolve the filtered material in sufficient dilute nitric acid solution to remove excess impurities;

[0026] Step nine: Separate the mixed materials by filtration and obtain pure silver-palladium alloy powder after drying.

[0027] The present invention first adopts a grinding aid and a silver powder and a palladium powder ball milling process, which can not only effectively remove impurities such as oxides on the surface of the metal powder, but also better promote the uniform dispersion of the silver and palladium metal powders, reduce agglomeration and uneven mixing, and make the metal ratio of the alloy closer to the expected value.

[0028] High-temperature treatment is then used to remove impurities such as hydrogen and oxygen adsorbed on the surface of the powder. Different heating curves and holding times determine the growth rate of the silver-palladium alloy phase. The presence of grinding aids limits the growth of the silver and palladium alloy phases to occur only between powders in adjacent positions. The combination of chromium oxide of different sizes can not only obtain silver-palladium alloy powders of different particle sizes, but also avoid the formation of oversized particles, thereby making the resulting alloy phase purer, more alloyed, and more uniform in silver-palladium ratio.

[0029] The secondary ball milling process of the present invention can not only restore the alloy powder agglomerated due to high-temperature calcination to a well-dispersed state, but also modify the irregular alloy powder so that the overall alloy powder presents a good spherical morphology.

[0030] Compared with the conventional liquid phase method for preparing silver-palladium alloy, the present invention has the following advantages:

[0031] 1. The silver-palladium alloy degree obtained by the silver-palladium alloy preparation process adopted in the present invention can be appropriately adjusted according to the slurry requirements;

[0032] 2. The silver-palladium alloy preparation process adopted in the present invention can adjust the ratio of silver powder to palladium powder within a certain range to obtain silver-palladium alloys with different ratios;

[0033] 3. The alloy particle size distribution obtained by the silver-palladium alloy preparation process adopted in the present invention is more uniform, and the particle size is controllable. The silver-palladium alloy in the range of 500 to 2000 nm can be obtained according to the particle size of the silver powder or palladium powder.

[0034] 4. After separation, the alloy powder obtained by the silver-palladium alloy preparation process adopted in the present invention was characterized by SEM, XRD and laser particle size analyzer respectively. It was found that the alloy state of the obtained silver-palladium alloy powder was good, the morphology was closer to spherical, and the particle size distribution was uniform, which well met the technical requirements of silver-palladium slurry.

[0035] Based on the above reasons, the present invention can be widely used in the field of roller printing paste manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0037] Figure 1 This is a SEM picture of the silver-palladium alloy obtained in Example 3 of the present invention.

[0038] Figure 2 The figure is the XRD test result of the silver-palladium alloy obtained by the present invention.

[0039] Figure 3 Schematic diagram of particle size distribution of the silver-palladium alloy obtained by the present invention. DETAILED DESCRIPTION

[0040] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0041] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0043] The present invention provides a silver-palladium alloy powder suitable for making MLCC slurry, wherein the raw materials are composed of the following raw materials in percentage by mass:

[0044] 5-30% silver powder, wherein the silver powder is nano-spherical powder, and the particle size is 1 / 4-1 / 2 of the target silver-palladium alloy powder particle size;

[0045] 2-10% palladium powder, wherein the palladium powder is a nano-spherical powder with a particle size of 1 / 4-1 / 2 of the target silver-palladium alloy powder;

[0046] 30-80% of grinding aid; the grinding aid is one or a mixture of lithium tantalate, artificial diamond powder, aluminum oxide, silicon oxide, cerium oxide, chromium oxide, tungsten carbide or colloidal silicon dioxide; preferably, the present invention uses chromium oxide with a particle size of 100-500 μm.

[0047] Dispersant 2-5%; the dispersant is one or a mixture of maleic acid-acrylic acid copolymer, sodium polyacrylate, polyoxyethylene alcohol, polycarboxylic acid sodium salt dispersant, polyurethane block copolymer or acrylic acid-styrene copolymer; preferably, the present invention uses maleic acid-acrylic acid copolymer.

[0048] Surfactant 0.5-2%; the surfactant is a cationic surfactant, an anionic surfactant and a nonionic surfactant, the cationic surfactant is one or a mixture of cetyltrimethylammonium bromide, dodecyltrimethylammonium chloride or dodecyltrimethylbenzylammonium chloride; the anionic surfactant is one or a mixture of sodium dodecylbenzene sulfonate, sodium lauryl sarcosinate, sodium lauryl sarcosinate; the nonionic surfactant is one or a mixture of nonylphenol polyoxyethylene ether, polyethylene glycol, fatty alcohol polyoxyethylene ether; preferably, the present invention uses sodium lauryl sarcosinate among the anionic surfactants.

[0049] And 20-60% pure water.

[0050] The present invention also discloses a preparation process of the silver-palladium alloy powder suitable for making MLCC slurry, comprising the following steps:

[0051] Step 1: weigh 5-30% silver powder, 2-10% palladium powder, 30-80% grinding aid, 2-5% dispersant, 0.2-2% surfactant, and 20-60% pure water, and introduce the above materials into a 100ml alumina can;

[0052] Step 2: Add 100 g of zirconia ceramic beads with a particle size of 5 mm into the alumina can;

[0053] Step 3: Fix the alumina can on the ball mill, set the speed to 300-500RPM / min, and ball-mill for 1-2 hours;

[0054] Step 4: After ball milling, use a 10-mesh filter to filter out the zirconium dioxide ceramic beads;

[0055] Step 5: Spread the filtered material onto a surface dish and dry at 100°C for 2-5 hours;

[0056] Step 6: Place the dried material mixture into a sintering furnace, raise the temperature to 600-800°C at a heating rate of 5-20°C / min, maintain for 20-60min, and then cool it down to room temperature at a cooling rate of 5-20°C / min;

[0057] Step 7: After the material cools down to room temperature, the mixed material and 50g of pure water are re-introduced into the ball mill without adding zirconia ceramic beads. The ball mill speed is set to 100RPM, the ball milling time is 1h, and the grinding aid is filtered out using a 100-mesh filter;

[0058] Step 8: Prepare 0.1 mol / L nitric acid solution, dissolve the filtered material in sufficient dilute nitric acid solution to remove excess impurities;

[0059] Step 9: Separate the mixed materials by suction filtration and obtain pure silver-palladium alloy powder after drying;

[0060] After separation, the silver-palladium alloy powder was characterized using SEM, XRD and laser particle size analyzer respectively. It was found that the alloy state of the obtained silver-palladium alloy powder was good, and the morphology and particle size distribution met the technical requirements of silver-palladium slurry.

[0061] Examples 1-16

[0062] As shown in Table 1, the material ratios of the embodiments of the present invention are as follows:

[0063] Table 1

[0064]

[0065] The preparation process of Examples 1-5 is as follows:

[0066] Step 1, weigh the above-mentioned silver powder, palladium powder, chromium oxide, maleic acid acrylic acid copolymer, sodium lauryl sarcosinate, and pure water, and introduce the above-mentioned materials into a 100 ml alumina can;

[0067] Step 2: Add 100 g of zirconia ceramic beads with a particle size of 5 mm into the alumina can;

[0068] Step 3: Fix the alumina can on the ball mill, set the speed to 300RPM / min and ball-mill for 2h;

[0069] Step 4: After ball milling, use a 10-mesh filter to filter out the zirconium dioxide ceramic beads;

[0070] Step 5: Spread the filtered material onto a surface dish and dry at 100°C for 3 hours;

[0071] Step 6: Place the dried material mixture into a sintering furnace, raise the temperature to 600°C at a heating rate of 10°C / min, maintain for 40 minutes, and then cool it down to room temperature at a cooling rate of 10°C / min;

[0072] Step 7: After the material cools down to room temperature, the mixed material and 50g of pure water are re-introduced into the ball mill without adding zirconium dioxide ceramic beads, the ball mill speed is set to 100RPM, the ball milling time is 1h, and the grinding aid is filtered out using a 100-mesh filter;

[0073] Step 8: Prepare 0.1 mol / L nitric acid solution, dissolve the filtered material in sufficient dilute nitric acid solution to remove excess impurities;

[0074] Step nine: Separate the mixed materials by filtration to obtain pure silver-palladium alloy powder.

[0075] Preparation process of Example 6

[0076] Different from Examples 1-5, in step 6, the dried material mixture is placed in a sintering furnace, the temperature is raised to 600°C at a heating rate of 5°C / min, maintained for 40 minutes, and then cooled to room temperature at a cooling rate of 5°C / min.

[0077] Preparation process of Examples 7-8

[0078] Different from Examples 1-5, in step 6, the dried material mixture is placed in a sintering furnace, the temperature is raised to 800°C at a heating rate of 5°C / min, maintained for 40 minutes, and then cooled to room temperature at a cooling rate of 5°C / min.

[0079] Preparation process of Examples 9-16

[0080] Different from Examples 1-5, in step 6, the dried material mixture is placed in a sintering furnace, the temperature is raised to 800°C at a heating rate of 10°C / min, maintained for 40 minutes, and then cooled to room temperature at a cooling rate of 10°C / min.

[0081] like Figure 1 to Figure 3 As shown, XRD data show that the three strongest peak angles of the silver-palladium alloy are 38.56°, 45.23°, and 65.57°, respectively. The three strongest peaks of the known silver element are 38.12°, 44.28°, and 64.43°; the three strongest peak angles of the palladium element are 40.12°, 46.66°, and 68.12°; thus, it can be seen that silver and palladium have indeed formed an alloy phase; SEM and particle size distribution diagrams can prove that the obtained silver-palladium alloy has uniform particle size distribution and good sphericity, and the particle size distribution of the alloy powder is closer to the normal distribution, which is in line with the narrow distribution particle size distribution characteristics; the above data show that the process of this patent can obtain a silver-palladium alloy with excellent crystal form and uniform particle size distribution.

[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A preparation process of silver-palladium alloy powder suitable for making MLCC slurry, It is characterized in that The steps include: Step 1: Weigh the raw materials according to the preset ratio and introduce them into the alumina tank; The raw materials are composed of the following raw materials in percentage by weight: Silver powder 5-30%, wherein the silver powder is nano-spherical powder, and the particle size is 1 / 4-1 / 2 of the target silver-palladium alloy powder particle size; 2-10% palladium powder, wherein the palladium powder is a nano-spherical powder with a particle size of 1 / 4-1 / 2 of the target silver-palladium alloy powder; Grinding aid 30-80%; Dispersant 2-5%; Surfactant 0.5-2%; Pure water 20-60%; Step 2: Add an appropriate amount of zirconium dioxide ceramic beads with a particle size of 5 mm into the alumina can; Step 3: Fix the alumina can on the ball mill, set the speed to 300-500 RPM / min, and ball-mill for 1-2 hours; Step 4: After ball milling, use a 10-mesh filter to filter out the zirconium dioxide ceramic beads; Step 5: Spread the filtered material onto a surface dish and dry at 50-100°C for 2-5 hours; Step 6: Place the dried material mixture into a sintering furnace, raise the temperature to 600-800°C at a heating rate of 5-20°C / min, maintain for 20-60min, and then cool it down to room temperature at a cooling rate of 5-20°C / min; Step 7: After the material cools down to room temperature, re-introduce the mixed material and 50g pure water into the ball mill without adding zirconium oxide ceramic beads, set the ball mill speed to 100-300RPM, the ball milling time to 1-2h, and use a 100-mesh filter to filter out the grinding aid; Step 8: Prepare 0.1 mol / L nitric acid solution, dissolve the filtered material in sufficient dilute nitric acid solution to remove excess impurities; Step nine: Separate the mixed materials by filtration and obtain pure silver-palladium alloy powder after drying.

2. The preparation process according to claim 1, It is characterized in that The grinding aid is one or a mixture of lithium tantalate, artificial diamond powder, aluminum oxide, silicon oxide, cerium oxide, chromium oxide, tungsten carbide or colloidal silicon dioxide.

3. The preparation process according to claim 1, It is characterized in that The dispersant is one or a mixture of maleic acid-acrylic acid copolymer, sodium polyacrylate, polyoxyethylene alcohol, polycarboxylic acid sodium salt dispersant, polyurethane block copolymer or acrylic acid-styrene copolymer.

4. The preparation process according to claim 1, It is characterized in that The surfactant is a cationic surfactant, an anionic surfactant and a nonionic surfactant. The cationic surfactant is one or a mixture of cetyltrimethylammonium bromide, dodecyltrimethylammonium chloride or dodecyltrimethylbenzylammonium chloride; the anionic surfactant is one or a mixture of sodium dodecylbenzene sulfonate, sodium lauryl sarcosinate and sodium lauryl sarcosinate; the nonionic surfactant is one or a mixture of nonylphenol polyoxyethylene ether, polyethylene glycol and fatty alcohol polyoxyethylene ether.