A method for 3D printing of polymer composite material powder bed inkjet sintering and its products

By using the polymer composite powder bed inkjet sintering method in 3D printing technology, combined with microwave processing, the problems of slow part forming speed and large welds are solved, and high-strength and high-efficiency part manufacturing is achieved.

CN116039078BActive Publication Date: 2024-10-29SICHUAN UNIV
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202211436308.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-10-29
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

The molding speed of existing 3D printing technology parts is slow, and the printed parts have large welds and low mechanical properties.

Method used

The polymer composite powder bed inkjet sintering method is used to coat the carbon material on the surface of the polymer powder through liquid phase adsorption to form a composite powder. Combined with computer slicing technology and roller laying, the nozzle inkjet and solidify according to the pattern. agent, the print bed is lowered to print layer by layer, and finally further cured in a microwave processing device.

Benefits of technology

It significantly improves the forming speed and mechanical properties of the parts, reduces the weld width and material defects, and improves the overall manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116039078B_ABST
    Figure CN116039078B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for 3D printing of polymer composite powder bed inkjet sintering, including coating the powder to be printed with a coating material; computer slicing of the three-dimensional model to obtain the contour information of each cross section; loading the polymer powder into the paving trough, loading the ink into the ink cartridge connected to the nozzle, and preheating the printing bed; using a roller to roll the material, and the nozzle performs inkjet bonding molding according to the pattern of the sliced ​​cross section; the printing bed is lowered a certain distance, and the bonding molding steps are repeated until the printing is completed; after the preliminary surface cleaning treatment of the workpiece, it is placed in a microwave treatment device for further microwave curing and molding. The present invention adopts a method of first forming and then combining microwave treatment, which can avoid the process of light curing after each printing, improve the production rate, and the weld after microwave treatment is smaller than the weld cured layer by layer in the prior art, and its mechanical properties are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of 3D printed products, and specifically relates to a method for 3D printing of polymer composite material powder bed inkjet sintering and a product printed by using the printing method. Background Art

[0002] With the development of human society, 3D additive manufacturing technology has emerged. 3D printing technology is based on digital model files, using powdered metal or plastic and other bondable materials to construct objects by printing layer by layer. Through 3D printing technology, people can easily achieve one-piece molding of complex structures. Sand mold 3D printing is a technology that lays fine sand flat and then sprays adhesive from the machine nozzle according to the pattern of the sliced ​​model to bond it layer by layer. This technology greatly shortens the sand casting cycle and reduces the overall process difficulty.

[0003] CN105665632A discloses an adaptive sand mold 3D printing forming method and device, which mainly mixes the molding sand and curing agent through vacuum feeding, and cooperates with the molding sand without curing agent to lay the two types of molding sand according to the required structure; then the nozzle sprays the resin binder on demand according to the current layer cross-section information of the printed sand mold, and the curing agent in the raw sand reacts with the resin binder to solidify, and the sand is laid layer by layer, and the binder is sprayed layer by layer, and finally the sand mold printing is completed. However, the equipment is mainly used for the molding of inorganic materials (such as fine sand), and the application of this technology in polymers is still vacant. At the same time, there is no other treatment after curing, and the curing effect is unknown.

[0004] Composites Science and Technology, 2011, 72(1):85-90 discloses a method of using a continuously arranged carbon nanotube film as a heat source network, using microwave welding technology to melt polyethylene and wrap it around the carbon nanotubes to form a uniform and highly conductive CNT / PE nanocomposite material with good antistatic ability and very strong CNT / PE interface bonding. However, the document discloses that microwave technology is used to make composite materials with good performance, but does not apply it to sand mold printing, nor does it apply microwave technology to improve the overall manufacturing rate of parts.

[0005] Based on the above analysis, a 3D printing method that can effectively improve the molding rate of polymer 3D printing technology parts and obtain high-strength parts is urgently needed in the industry. Summary of the invention

[0006] In view of the technical problems of slow molding speed and large weld seams of printed parts in the prior art 3D printing technology, the present invention combines polymer materials with sand mold 3D printing for the first time, and then quickly produces high-strength 3D printed parts through further microwave post-treatment. The present invention is achieved through the following technical means:

[0007] A method for 3D printing of polymer composite powder bed inkjet sintering, comprising:

[0008] (1) coating the surface of the polymer powder with carbon material by a liquid phase adsorption deposition method to form a polymer composite powder;

[0009] (2) Slice the three-dimensional model to be printed by computer to obtain the contour information of each cross section;

[0010] (3) The polymer composite powder is loaded into the paving tank, the ink is loaded into the ink cartridge connected to the nozzle, the curing agent is loaded into another container connected to the nozzle, and the printing bed is preheated;

[0011] (4) The material is spread by a roller, and the nozzle sprays ink according to the pattern of the slice cross section;

[0012] (5) the nozzle further sprays a curing agent according to the pattern of the slice cross section to cure and bond the slices;

[0013] (6) The printing bed is lowered a certain distance, and steps (4) and (5) are repeated until printing is completed;

[0014] (7) After preliminary surface cleaning of the workpiece, it is placed in a microwave treatment device for further microwave curing and molding.

[0015] Furthermore, the polymer powder in step (1) is any polymer powder that can be 3D printed.

[0016] Furthermore, the particle size of the polymer powder is 5-500 μm.

[0017] Furthermore, the polymer powder includes, but is not limited to, polyurethane powder, polylactic acid powder, polypropylene powder, nylon powder, polyetheretherketone powder, ABS powder, polycarbonate powder, polystyrene powder, polycaprolactone powder, and polyphenylsulfone powder.

[0018] Furthermore, the carbon material in step (1) is one or more of carbon nanotubes, graphene, and conductive carbon black.

[0019] Furthermore, the polymer composite powder in step (1) includes but is not limited to: carbon material coated polyurethane composite powder, carbon material coated polylactic acid composite powder, carbon material coated polypropylene composite powder, carbon material coated nylon composite powder, carbon material coated polyetheretherketone composite powder, carbon material coated ABS composite powder, carbon material coated polycarbonate composite powder, carbon material coated polystyrene composite powder, carbon material coated polycaprolactone composite powder, and carbon material coated polyphenylsulfone composite powder.

[0020] Furthermore, the ink in step (3) is an ink having adhesive properties.

[0021] Furthermore, the ink includes: a furan resin binder and a phenolic resin binder.

[0022] Furthermore, the curing agent in step (3) is a commercial curing agent.

[0023] Furthermore, the certain distance in step (6) is 0.05-1 mm.

[0024] Furthermore, the microwave treatment in step (7) includes: radio frequency microwave treatment and electromagnetic microwave treatment; the microwave treatment power is 800-3000W, and the treatment time is 10-300s.

[0025] The present invention also discloses a product printed according to any of the above-mentioned polymer composite material powder bed inkjet sintering 3D printing methods.

[0026] The beneficial effects of the present invention are:

[0027] In the prior art, powder printing requires laying a layer of powder and then near-infrared light heating and curing once, which seriously reduces the printing efficiency. In addition, the welds between layers during the printing process are large, which reduces the mechanical properties of the product. The method of first forming and then combining microwave treatment can avoid the process of near-infrared light heating and curing after each printing. At the same time, the carbon material coated on the surface of the polymer powder helps to absorb microwaves and heat and cure, thereby increasing the production rate. After combined microwave treatment, the overall weld of the obtained product is smaller than the weld of layer-by-layer curing in the prior art, the defects of the material are reduced, and its mechanical properties are greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The figure is a flow chart of the printing method of the present invention.

[0029] Figure 2 The scanning electron microscope image of the weld width of the specimen prepared for comparative example 1.

[0030] Figure 3 This is a scanning electron microscope image of the weld width of the specimen obtained in Example 1. DETAILED DESCRIPTION

[0031] The present invention is further described below by means of specific embodiments. The description of the embodiments is only for the convenience of understanding and application of the present invention, but not for limiting the protection of the present invention.

[0032] Embodiment 1:

[0033] A method for 3D printing of polymer composite powder bed inkjet sintering, as follows:

[0034] (1) coating the surface of the polymer powder with carbon material by a liquid phase adsorption deposition method to form a polymer composite powder;

[0035] (2) Slice the three-dimensional model to be printed by computer to obtain the contour information of each cross section;

[0036] (3) The polymer composite powder is loaded into the paving tank, the ink is loaded into the ink cartridge connected to the nozzle, the curing agent is loaded into another container connected to the nozzle, and the printing bed is preheated;

[0037] (4) The material is spread by a roller, and the nozzle sprays ink according to the pattern of the slice cross section;

[0038] (5) the nozzle further sprays a curing agent according to the pattern of the slice cross section to cure and bond the slices;

[0039] (6) The printing bed is lowered a certain distance, and steps (4) and (5) are repeated until printing is completed;

[0040] (7) After preliminary surface cleaning of the workpiece, it is placed in a microwave treatment device for further microwave curing and molding.

[0041] Wherein: the polymer powder is polyurethane powder with a particle size of 100 μm; the carbon material is conductive carbon black; the polymer composite powder is conductive carbon black coated polyurethane composite powder; the ink is furan resin binder; the curing agent is a commercial curing agent; the falling distance is 0.1 mm; the microwave treatment is radio frequency microwave treatment, its power is 1000 W, and the treatment time is 30 s.

[0042] Embodiment 2:

[0043] A method for 3D printing of polymer composite powder bed inkjet sintering, as follows:

[0044] (1) coating the surface of the polymer powder with carbon material by a liquid phase adsorption deposition method to form a polymer composite powder;

[0045] (2) Slice the three-dimensional model to be printed by computer to obtain the contour information of each cross section;

[0046] (3) The polymer composite powder is loaded into the paving tank, the ink is loaded into the ink cartridge connected to the nozzle, the curing agent is loaded into another container connected to the nozzle, and the printing bed is preheated;

[0047] (4) The material is spread by a roller, and the nozzle sprays ink according to the pattern of the slice cross section;

[0048] (5) the nozzle further sprays a curing agent according to the pattern of the slice cross section to cure and bond the slices;

[0049] (6) The printing bed is lowered a certain distance, and steps (4) and (5) are repeated until printing is completed;

[0050] (7) After preliminary surface cleaning of the workpiece, it is placed in a microwave treatment device for further microwave curing and molding.

[0051] Among them: the polymer powder is nylon powder with a particle size of 150μm; the carbon material is carbon nanotubes; the polymer composite powder is carbon nanotube-coated nylon composite powder; the ink is a phenolic resin binder; the curing agent is a commercial curing agent; the falling distance is 0.2mm; the microwave treatment is radio frequency microwave treatment, its power is 1200W, and the treatment time is 120s.

[0052] Embodiment 3:

[0053] A method for 3D printing of polymer composite powder bed inkjet sintering, as follows:

[0054] (1) coating the surface of the polymer powder with carbon material by a liquid phase adsorption deposition method to form a polymer composite powder;

[0055] (2) Slice the three-dimensional model to be printed by computer to obtain the contour information of each cross section;

[0056] (3) The polymer composite powder is loaded into the paving tank, the ink is loaded into the ink cartridge connected to the nozzle, the curing agent is loaded into another container connected to the nozzle, and the printing bed is preheated;

[0057] (4) The material is spread by a roller, and the nozzle sprays ink according to the pattern of the slice cross section;

[0058] (5) the nozzle further sprays a curing agent according to the pattern of the slice cross section to cure and bond the slices;

[0059] (6) The printing bed is lowered a certain distance, and steps (4) and (5) are repeated until printing is completed;

[0060] (7) After preliminary surface cleaning of the workpiece, it is placed in a microwave treatment device for further microwave curing and molding.

[0061] Wherein: the polymer powder is polypropylene powder with a particle size of 200 μm; the carbon material is carbon nanotubes; the ink is a furan resin binder; the curing agent is a commercial curing agent; the falling distance is 0.2 mm; the microwave treatment is a radio frequency microwave treatment with a power of 1000 W and a treatment time of 150 s.

[0062] Embodiment 4:

[0063] A method for 3D printing of polymer composite powder bed inkjet sintering, as follows:

[0064] (1) coating the surface of the polymer powder with carbon material by a liquid phase adsorption deposition method to form a polymer composite powder;

[0065] (2) Slice the three-dimensional model to be printed by computer to obtain the contour information of each cross section;

[0066] (3) The polymer composite powder is loaded into the paving tank, the ink is loaded into the ink cartridge connected to the nozzle, the curing agent is loaded into another container connected to the nozzle, and the printing bed is preheated;

[0067] (4) The material is spread by a roller, and the nozzle sprays ink according to the pattern of the slice cross section;

[0068] (5) the nozzle further sprays a curing agent according to the pattern of the slice cross section to cure and bond the slices;

[0069] (6) The printing bed is lowered a certain distance, and steps (4) and (5) are repeated until printing is completed;

[0070] (7) After preliminary surface cleaning of the workpiece, it is placed in a microwave treatment device for further microwave curing and molding.

[0071] Wherein: the polymer powder is polystyrene powder with a particle size of 50 μm; the carbon material is graphene; the polymer composite powder is graphene-coated polystyrene composite powder; the ink is a furan resin binder; the curing agent is a commercial curing agent; the falling distance is 0.4 mm; the microwave treatment is a radio frequency microwave treatment with a power of 1300 W and a treatment time of 60 s.

[0072] Embodiment 5:

[0073] A method for 3D printing of polymer composite powder bed inkjet sintering, as follows:

[0074] (1) coating the surface of the polymer powder with carbon material by a liquid phase adsorption deposition method to form a polymer composite powder;

[0075] (2) Slice the three-dimensional model to be printed by computer to obtain the contour information of each cross section;

[0076] (3) The polymer composite powder is loaded into the paving tank, the ink is loaded into the ink cartridge connected to the nozzle, the curing agent is loaded into another container connected to the nozzle, and the printing bed is preheated;

[0077] (4) The material is spread by a roller, and the nozzle sprays ink according to the pattern of the slice cross section;

[0078] (5) the nozzle further sprays a curing agent according to the pattern of the slice cross section to cure and bond the slices;

[0079] (6) The printing bed is lowered a certain distance, and steps (4) and (5) are repeated until printing is completed;

[0080] (7) After preliminary surface cleaning of the workpiece, it is placed in a microwave treatment device for further microwave curing and molding.

[0081] Among them: the polymer powder is polyetheretherketone powder with a particle size of 100μm; the carbon material is graphene; the polymer composite powder is graphene-coated polyetheretherketone composite powder; the ink is a phenolic resin binder; the curing agent is a commercial curing agent; the descent distance is 1mm; the microwave treatment is radio frequency microwave treatment, its power is 2000W, and the treatment time is 30s.

[0082] Comparative Example 1:

[0083] A method for 3D printing of polymer composite powder bed inkjet sintering, as follows:

[0084] (1) Slice the 3D model to be printed by computer to obtain the contour information of each cross section;

[0085] (2) Loading polymer powder into the paving tank, loading ink into the ink cartridge connected to the nozzle, and preheating the printing bed;

[0086] (3) The material is spread by a roller, and the nozzle is inkjet bonded and formed according to the pattern of the slice section;

[0087] (4) using near-infrared light to heat and cure the product;

[0088] (5) The print bed is lowered a certain distance, and steps (3) and (4) are repeated until printing is completed;

[0089] Among them: the polymer powder is polyurethane powder with a particle size of 200 μm; the ink is conductive carbon black mixed with furan resin; the near-infrared irradiation time is 60 s; and the falling distance is 0.1 mm.

[0090] Test Example 1

[0091] Test: 1 mm thick specimens were printed using the conditions of Example 1 and Comparative Example 1 for mechanical property testing, and the time used in the processing was recorded for comparison. The results are shown in Table 1.

[0092] Table 1 Performance comparison table

[0093]

[0094] According to the results in Table 1, the method of overall bonding molding combined with radio frequency microwave post-treatment can improve the mechanical properties of the final polymer parts by about two times and greatly shorten the molding time of the overall parts. Figure 2 and Figure 3 The comparison of the scanning electron microscope results shows that the weld width after microwave sintering is significantly reduced. The weld width of the comparative example 1 without microwave sintering is 87.94 μm, and the widest weld width of the example 1 after microwave sintering is only 2.293 μm, and the weld width and internal defects of the sample strip are significantly reduced.

[0095] In summary, the present invention adopts a method of first one-step forming by powder bed inkjet printing and then microwave sintering treatment, which can avoid the process of near-infrared light heating and curing after each layer is printed, thereby improving production efficiency; at the same time, the internal welds of the parts obtained after microwave sintering treatment are significantly smaller than the welds cured layer by layer in the prior art, and the defects are reduced, so that the mechanical properties are significantly improved.

[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for 3D printing of polymer composite powder bed inkjet sintering, comprising: (1) coating the carbon material on the surface of polymer powder with a particle size of 5-500 μm by liquid phase adsorption deposition method to form a polymer composite powder; (2) Computer slicing of the three-dimensional model to be printed to obtain the contour information of each cross section; (3) The polymer composite powder is loaded into the paving tank, the ink is loaded into the ink cartridge connected to the nozzle, the curing agent is loaded into another container connected to the nozzle, and the printing bed is preheated; (4) The material is spread by a roller, and the nozzle sprays ink according to the pattern of the slice cross section; (5) the nozzle further sprays a curing agent according to the pattern of the slice cross section to cure and bond the slices; (6) The printing bed is lowered a certain distance, and steps (4) and (5) are repeated until printing is completed; (7) Cleaning the surface of the workpiece, followed by microwave curing and molding, wherein the microwave power is 800-3000 W and the time is 10-300 s; in: The polymer powder in step (1) is any polymer powder that can be 3D printed, including: Polyurethane powder, polylactic acid powder, polypropylene powder, nylon powder, polyetheretherketone powder, ABS powder, polycarbonate powder, polystyrene powder, polycaprolactone powder, polyphenylsulfone powder.

2. The method for 3D printing of polymer composite powder bed inkjet sintering according to claim 1, wherein: The carbon material in step (1) is one or more of carbon nanotubes, graphene, and conductive carbon black.

3. The method for 3D printing of polymer composite powder bed inkjet sintering according to claim 1, wherein: The polymer composite powder in step (1) comprises: Carbon material coated polyurethane composite powder, carbon material coated polylactic acid composite powder, carbon material coated polypropylene composite powder, carbon material coated nylon composite powder, carbon material coated polyetheretherketone composite powder, carbon material coated ABS composite powder, carbon material coated polycarbonate composite powder, carbon material coated polystyrene composite powder, carbon material coated polycaprolactone composite powder, carbon material coated polyphenylsulfone composite powder.

4. The method for 3D printing of polymer composite powder bed inkjet sintering according to claim 1, wherein: The ink in step (2) is an ink having bonding ability, comprising: One or more of furan resin binder and phenolic resin binder.

5. The method for 3D printing of polymer composite powder bed inkjet sintering according to claim 1, wherein: The curing agent in step (2) is a commercial curing agent.

6. The method for 3D printing of polymer composite powder bed inkjet sintering according to claim 1, wherein: The certain distance in step (4) is 0.05-1 mm.

7. A product printed by the polymer composite material powder bed inkjet sintering 3D printing method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Self-adaption sand mould 3D printing molding method and device

    CN105665632A

  • Casting mold three-dimensional printing formation method

    CN106799461A

  • 3D ink-jet printer

    CN110815822A

  • Near-infrared reflection composite material for ink-jet 3D printing and preparation method of near-infrared reflection composite material

    CN112322110A

  • Three-dimensional object forming method and device, storage medium and computer equipment

    CN113290852A