Preparation method and application of super-hydrophobic antifouling coating with antibacterial function
Through the reaction of n-octadecyltriethoxysilane with water and the use of dilution dispersant, a superhydrophobic coating with antibacterial effect is formed, which solves the limitations of the application of superhydrophobic coatings in the prior art and achieves no impact on the In the case of breathability and mechanical properties, the material is imparted with good hydrophobic and antibacterial properties and is suitable for large-scale production.
Patent Information
- Application Number
- CN202411406706.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-10
AI Technical Summary
The application of existing superhydrophobic coatings is limited by the single surface function, complicated preparation steps, dangerous chemical materials and inconvenient for large-scale manufacturing. The traditional methods have a great impact on breathable and mechanical properties, and lack simple operation, low cost and Environmentally friendly multifunctional superhydrophobic coating solution.
Using a mixture of n-octadecyltriethoxysilane, water and octadecyltrichlorosilane, superhydrophobic reaction product is formed by ultrasonic shock and standstill, and silver nitrate or organic is added to the diluted dispersant n-hexane. Silicon quaternary ammonium salts form superhydrophobic coating mixtures with antibacterial effects and are applied to the surface of solid materials by immersion or spraying.
It achieves the material with good hydrophobic and antibacterial properties without affecting the breathability and mechanical properties, and the preparation method is simple, fast, low-cost, and suitable for large-scale production.
Smart Images

Figure CN119081544A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of multifunctional composite antibacterial super-hydrophobic coating modification, and specifically relates to a method for preparing a super-hydrophobic antifouling coating with antibacterial function, and specific applications of the coating prepared by the method. Background Art
[0002] Super-hydrophobic coatings prepared by surface treatment technology can give the coating surface excellent anti-fouling and self-cleaning characteristics, and such coatings have a broad market demand. At present, super-hydrophobic coatings have been successfully prepared on solid substrates by various methods, but the application of super-hydrophobic coatings is still limited by the single surface function, complicated preparation steps, dangerous selected chemical materials, and inconvenience for large-scale manufacturing.
[0003] Fang et al. (J. Adv. Eng. Mater., 2021, 23 (12), 2102502) used polymethylhydrogensiloxane to prepare hydrophobic organosilicon nanowires through a base-catalyzed reaction, and thermally cured them at 120°C to prepare flexible fabrics with excellent superhydrophobicity. Ye et al. (J. Chem. Eng. J., 2021, 420, 127680) prepared double-nanocomposite coated fabrics by spraying, and successfully prepared a durable antibacterial and antifouling textile with high efficiency in preventing bacterial adhesion by using polydimethylsiloxane as an adhesive to adhere fluorinated mesoporous silica. However, at present, antifouling finishing usually uses an adhesive as an adhesive layer, and the low surface energy nanoparticles are modified to the surface of the substrate by simple scraping, dipping and other means. It has the fatal defects of easy damage to the surface structure and poor durability, and it also has a great impact on the air permeability of some object surfaces. Tasixiang et al. (Prog. Org. Coat., 2019, 135, 41-50) used a two-step coating method of polytetrafluoroethylene microparticles and fluorinated alkylsilane on aramid fabric to obtain a strong, super-amphiphobic self-cleaning fabric. However, the flexibility of the fabric decreased and the air permeability decreased from 313 mm / s to 10 mm / s. The self-assembly of organosiloxane on the fabric surface can give the substrate surface durable antifouling properties without affecting the air permeability. It is divided into two major categories. The organosiloxane with alkyl oxygen or hydroxyl as the functional group has a very slow reaction rate and usually needs to undergo a long-term heating reaction under strong acid catalysis, and the reaction process consumes a lot of water; the organosiloxane with halogen as the functional group is very sensitive to the humidity of the environment, the reaction rate is extremely fast (tens of seconds to several minutes), the reaction process is difficult to control and releases a large amount of strong acid gas, which has a great influence on the mechanical properties. Zhang et al. (Nat. Commun., 2021, 12(1), 982.) prepared a super-hydrophobic surface coating by reacting chlorosilane with water. The reaction is simple and rapid, but a large amount of hydrogen chloride gas is produced during the reaction. At present, it is of great practical significance to develop a multifunctional super-hydrophobic coating that is simple, fast, low-cost and environmentally friendly. Summary of the invention
[0004] Based on the above technical problems, the present invention proposes a preparation method and application of a super hydrophobic antifouling coating with antibacterial function.
[0005] The technical solution adopted by the present invention is:
[0006] A method for preparing a super hydrophobic antifouling coating with antibacterial function comprises the following steps:
[0007] S1, mixing n-octadecyltriethoxysilane, water and octadecyltrichlorosilane uniformly, and then standing to react to obtain a super hydrophobic reaction product;
[0008] S2. Dilute and disperse the super-hydrophobic reaction product obtained in step S1 with n-hexane to obtain a super-hydrophobic coating mixture.
[0009] Preferably, in step S1: the usage ratio of n-octadecyltriethoxysilane to water is 1 ml: 20-80 μL; the usage ratio of octadecyltrichlorosilane to n-octadecyltriethoxysilane is 1-6 μL: 1 ml.
[0010] Preferably, in step S1: after the n-octadecyltriethoxysilane, water and octadecyltrichlorosilane are mixed, they are first placed on a vortex mixer for mixing, and then placed in an ultrasonic cleaner for ultrasonic vibration treatment.
[0011] Preferably, in step S1: the static reaction time is 1-5h.
[0012] Preferably, in step S1: silver nitrate is also added when preparing the super-hydrophobic reaction product; silver nitrate is first added to water to prepare a silver nitrate solution; and then n-octadecyltriethoxysilane, octadecyltrichlorosilane and the silver nitrate solution are uniformly mixed.
[0013] Preferably, the concentration of the silver nitrate solution is 0.5-5wt%.
[0014] Preferably, in step S2: n-hexane is added to the super-hydrophobic reaction product; and the volume fraction of the super-hydrophobic reaction product in the obtained super-hydrophobic coating mixture is 1-10%.
[0015] Preferably, in step S2: a quaternary ammonium organosilicon salt is also added when preparing the super-hydrophobic coating mixture.
[0016] Preferably, the organosilicon quaternary ammonium salt is first added to n-hexane to obtain an organosilicon quaternary ammonium salt / n-hexane solution, and then the organosilicon quaternary ammonium salt / n-hexane solution is added to the superhydrophobic reaction product for mixing; the mass volume ratio of the added amount of the organosilicon quaternary ammonium salt to the amount of n-hexane used is 0.01-0.04g / ml.
[0017] The application of the super-hydrophobic coating mixture prepared as above in the surface modification of solid materials is as follows:
[0018] The solid material is immersed in the obtained super-hydrophobic coating mixture, taken out after 12-24 hours, washed with n-hexane, and then dried in the air; or the obtained super-hydrophobic coating mixture is transferred to a spray bottle and sprayed on the solid material to obtain a super-hydrophobic antifouling coating with antibacterial function.
[0019] The beneficial technical effects of the present invention are as follows:
[0020] a. Alkyloxysiloxane is used as a self-assembling prepolymer, and the reaction of the prepolymer is triggered by trace amounts of water and halogen siloxane to form an oil-in-water emulsion system. The emulsion system is then diluted with an organic solvent as a medium, and the disadvantages of the two types of organic alkyl oxygens are complemented as advantages of the entire reaction system.
[0021] b. Add water-soluble antibacterial agent silver nitrate to the reaction initiator water, and graft the antibacterial agent onto the material surface through the water initiator during the copolymerization self-assembly process, thereby giving the material good antibacterial properties during the anti-fouling finishing process.
[0022] c. Add the antibacterial agent silicone quaternary ammonium salt to the dilute dispersion solvent n-hexane, and attach it to the surface of the material without affecting the self-assembly of the super-hydrophobic coating copolymer, thereby giving the material good antibacterial properties during the anti-fouling finishing process.
[0023] d. The antibacterial super-hydrophobic coating prepared by the present invention exhibits good dynamic hydrophobic effect and has good antifouling and antibacterial properties.
[0024] The antibacterial super-hydrophobic coating prepared by the present invention exhibits good hydrophobic and antibacterial properties on the surface of textiles, while having little effect on the air permeability and mechanical properties of the fabrics.
[0025] f. The preparation method of the antibacterial super-hydrophobic antifouling coating of the present invention also has the advantages of simple and rapid operation, low cost, environmental friendliness, and large-scale production.
[0026] In summary, the present invention first uses alkyloxysiloxane as self-assembly prepolymer, triggers the reaction of prepolymer by trace water (initiator) and halogen siloxane (catalyst), forms oil-water emulsion system, then uses organic solvent as medium dilution emulsion system, and textile is carried out antifouling finishing.This method improves alkyloxy or hydroxyl as the organosiloxane reaction rate of functional group on the basis of, avoids the influence of halogen as organosiloxane modification of functional group on material surface.By in above-mentioned reaction initiator water, add water-soluble antibacterial agent silver nitrate or add organosilicon quaternary ammonium salt in normal hexane, obtain the super hydrophobic coating mixture with antibacterial effect, synchronously give textile good antibacterial property. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The change curve of the contact angle of the coating obtained before and after adding the catalyst in Example 1 of the present invention and Comparative Example 1 as the reaction time of the super-hydrophobic reaction product changes;
[0028] Figure 2The present invention adopts the super-hydrophobic coating mixture obtained in Example 1 and Comparative Example 1 to form a coating by immersion on the surface of a polyester fabric SEM images, wherein (a) is a SEM image of the super-hydrophobic antifouling coating formed in Example 1, and (b) is a SEM image of the super-hydrophobic antifouling coating formed in Comparative Example 1;
[0029] Figure 3 The effect of the antibacterial superhydrophobic antifouling coating prepared by the present invention on the contact angle of the coating under different conditions; wherein, (a) shows the effect of different reaction times on the contact angle of the coating, (b) shows the effect of different water and reaction reagent usage ratios on the contact angle of the coating, (c) shows the effect of different catalyst usage amounts on the contact angle of the coating, and (d) shows the effect of different reaction reagents on the contact angle of the coating;
[0030] Figure 4 The application of the coating prepared in Example 3 of the present invention on the surfaces of different materials, wherein (a) shows the application on the surface of a fabric, (b) shows the application on the surface of a filter paper, (c) shows the application on the surface of a wooden board, and (d) shows the application on a sponge; (b), (c), and (d) all use water droplets;
[0031] Figure 5 The antibacterial effect of the coating prepared in Example 3 of the present invention on the surface of cotton fabric; wherein (a 1 ) shows the antibacterial properties of raw cotton fabric against Escherichia coli, (a 2 ) shows the antibacterial performance of the coated cotton fabric against Escherichia coli, (b 1 ) shows the antibacterial properties of raw cotton fabric against Staphylococcus aureus, (b 2 ) shows the antibacterial properties of coated cotton fabric against Staphylococcus aureus;
[0032] Figure 6 The effects of the coating prepared by changing the amount of OTS in Example 3 of the present invention on the air permeability and mechanical properties of the fabric; wherein (a) shows the effect of adding different amounts of water to the coating reaction on the air permeability of the cotton fabric, (b) shows the effect of the amount of catalyst added in the coating reaction on the air permeability of the cotton fabric, (c) shows the effect of the coating on the mechanical properties of the polyester fabric, and (d) shows the effect of the coating on the mechanical properties of the cotton fabric;
[0033] Figure 7 The changes in contact angle and antibacterial effect of the coating prepared in Example 3 of the present invention after the experiment, wherein (a) shows the change in contact angle after the water drop experiment, and (b) shows the change in antibacterial effect after the washing experiment. DETAILED DESCRIPTION
[0034] The present invention discloses a preparation method and application of a super-hydrophobic antifouling coating with antibacterial function. The method comprises the following steps: (1) adding a trace amount of water and octadecyl trichlorosilane to n-octadecyl triethoxysilane, ultrasonic oscillation makes it evenly mixed and then stands to react, and obtains micron to nano-graded siloxane aggregates; (2) the aggregates are dispersed in normal hexane to obtain a coating mixture with super-hydrophobicity; (3) silver nitrate is added to initiator water or organosilicon quaternary ammonium salt is added to normal hexane to obtain a super-hydrophobic coating mixture with antibacterial effect; (4) by dipping or spraying the coating mixture, a super-hydrophobic coating with antibacterial effect can be formed on the surface of a solid material. The present invention utilizes octadecyl trichlorosilane and water to trigger the prepolymer reaction of octadecyl triethoxysilane, forms an oil-in-water emulsion system, and then disperses the emulsion system with an organic solvent as a medium, and the disadvantages of the current 2 types of organic alkyl oxygen are complemented as the advantages of the entire reaction system, and the reaction speed is fast, no gas is generated, and the reaction conditions are simple. Further, an antibacterial agent is added to the reaction system to obtain a super hydrophobic coating with an antibacterial effect. The method improves the reaction rate of the organosiloxane with alkyl oxygen or hydroxyl as the functional group, avoids the influence of the organosiloxane modification with halogen as the functional group on the material surface, is simple and fast to operate, low-cost, environmentally friendly and can be mass-produced. Moreover, the method does not involve the use of an adhesive, and has little effect on the air permeability and feel of fabric materials.
[0035] The present invention will be further described below in conjunction with specific embodiments:
[0036] Example 1
[0037] (1) 2 μL of octadecyltrichlorosilane and 20 μL of water were added to 1 ml of octadecyltriethoxysilane, which was immediately placed on a vortex mixer at 3000 rpm for 10 seconds, then sonicated in an ultrasonic cleaner for 10 seconds, and subjected to another round of vortex mixing for 10 seconds to obtain an emulsion.
[0038] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After standing for 2 hours, 10 mL of n-hexane was added to the vial to obtain a super hydrophobic coating mixture.
[0039] Example 2
[0040] (1) 2 μL of octadecyltrichlorosilane and 45 μL of 2 wt% silver nitrate solution were added to 1 ml of octadecyltriethoxysilane, and the mixture was immediately placed on a vortex mixer at 3000 rpm for 10 s, then sonicated in an ultrasonic cleaner for 10 s, and subjected to another round of vortex mixing for 10 s.
[0041] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After 2 hours, 10 mL of n-hexane was added to the vial to obtain a superhydrophobic coating mixture with antibacterial effect.
[0042] Example 3
[0043] (1) 2 μL of octadecyltrichlorosilane and 20 μL of water were added to 1 ml of octadecyltriethoxysilane, which was immediately placed on a vortex mixer at 3000 rpm for 10 seconds, then sonicated in an ultrasonic cleaner for 10 seconds, and subjected to another round of vortex mixing for 10 seconds.
[0044] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After 2 hours, 10 mL of n-hexane containing 0.3 g of organosilicon quaternary ammonium salt was added to the vial.
[0045] Example 4
[0046] (1) 4 μL of octadecyltrichlorosilane and 65 μL of 5 wt% silver nitrate solution were added to 1 ml of octadecyltriethoxysilane, and the mixture was immediately placed on a vortex mixer at 3000 rpm for 10 seconds, then sonicated in an ultrasonic cleaner for 10 seconds, and subjected to another round of vortex mixing for 10 seconds.
[0047] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After 1 hour, 15 mL of n-hexane was added to the vial.
[0048] Example 5
[0049] (1) 2 μL of octadecyltrichlorosilane and 80 μL of water were added to 1 ml of octadecyltriethoxysilane, which was immediately placed on a vortex mixer at 3000 rpm for 10 s, then sonicated in an ultrasonic cleaner for 10 s, and subjected to another round of vortex mixing for 10 s.
[0050] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After 4 hours, 10 mL of n-hexane containing 0.1 g of organosilicon quaternary ammonium salt was added to the vial.
[0051] Example 6
[0052] (1) 6 μL of octadecyltrichlorosilane and 30 μL of water were added to 1 ml of octadecyltriethoxysilane, which was immediately placed on a vortex mixer at 3000 rpm for 10 seconds and then sonicated in an ultrasonic cleaner for 10 seconds to obtain an emulsion.
[0053] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After standing for 5 hours, 10 mL of n-hexane containing 0.2 g of organosilicon quaternary ammonium salt was added to the vial.
[0054] Example 7
[0055] (1) 3 μL of octadecyltrichlorosilane and 15 μL of water were added to 1 ml of octadecyltriethoxysilane, which was immediately placed on a vortex mixer at 3000 rpm for 10 seconds and then sonicated in an ultrasonic cleaner for 10 seconds to obtain an emulsion.
[0056] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After standing for 3 hours, 20 mL of n-hexane containing 0.3 g of organosilicon quaternary ammonium salt was added to the vial.
[0057] The solid material is immersed in the super-hydrophobic coating mixture finally obtained by the above-mentioned embodiment, taken out from the solution after overnight, washed three times with n-hexane, and then dried in air. Or by spraying, the super-hydrophobic coating mixture obtained by the above-mentioned embodiment is transferred to a spray bottle, and sprayed to the sample to be processed at an angle of 30 ° above the solid material sample to obtain a super-hydrophobic antifouling coating with antibacterial function. The coating has good antibacterial effect and super-hydrophobic effect.
[0058] Comparative Example 1
[0059] (1) 20 μL of water was added to 1 ml of octadecyltriethoxysilane, which was immediately placed on a vortex mixer at 3000 rpm for 10 seconds, then sonicated in an ultrasonic cleaner for 10 seconds, and subjected to another round of vortex mixing for 10 seconds.
[0060] (2) 500 μL of the obtained emulsion was transferred to a 20 mL vial. After 2 hours, 10 mL of n-hexane was added to the vial.
[0061] The coating mixtures prepared in the embodiments and comparative examples were used to immerse polyester and cotton fabrics, and the treated polyester and cotton fabrics were subjected to morphological observation, elemental composition analysis, water contact angle test, antibacterial test, air permeability and mechanical property test, and the superhydrophobicity, antibacterial property, air permeability, durability, etc. of the coating were evaluated. The methods and results are as follows:
[0062] (1) Characterization of superhydrophobic properties:
[0063] In the test, polyester fabric was immersed in the super-hydrophobic coating mixture prepared in Example 1 and Comparative Example 1 overnight, taken out from the solution, washed three times with n-hexane, and then dried in air to test its hydrophobic property. Figure 1 The contact angle of the super hydrophobic coating mixture changes at different reaction times before and after the addition of octadecyltrichlorosilane as a catalyst (the control steps are the same as those in Example 1 and Comparative Example 1, except that the static reaction time is changed). Figure 1The test results in the analysis show that the reaction rate is significantly accelerated and the contact angle increases after octadecyltrichlorosilane catalysis. After 2 hours of reaction, the contact angle of the reaction coating catalyzed by octadecyltrichlorosilane is close to 160°, which is more than 15° higher than that of the uncatalyzed reaction coating. In addition, from Figure 2 It can be seen from the SEM image that in the uncatalyzed comparative example 1, the presence of micro-nano particles between the fibers increases the surface roughness, making the fabric hydrophobic, but the reaction is incomplete and the particle distribution is not dense and uniform. The micro-nano particles generated by the catalytic reaction of Example 1 self-assemble on the fibers to form a compact and highly oriented rough surface, giving the fabric a good hydrophobic effect.
[0064] To obtain the best hydrophobic effect of the hydrophobic coating, Figure 3 As shown, the changes in the contact angle of the coating after adding different amounts of water and catalysts and reacting for different time periods, as well as the hydrophobic effects of different reaction reagents, were tested. OTES is octadecyltriethoxysilane, OTS is octadecyltrichlorosilane, MTMS is methyltrimethoxysilane, and VTMS is vinyltrimethoxysilane.
[0065] In order to characterize the super hydrophobic antifouling property of the fabric, the antifouling properties of the modified fabric to liquids such as soy sauce, cola, and rose red b dye solution were tested. Figure 4 As shown. Figure 4 It can be seen that the modified cotton fabric has excellent antifouling properties to the above-mentioned various liquids.
[0066] (2) Characterization of antibacterial properties:
[0067] Silver ions have strong redox properties, can destroy the structure of bacterial cell membranes, cause the rupture and dissolution of cell membranes, thereby affecting the normal metabolism of cells. At the same time, silver ions can also bind to bacterial DNA, thereby inhibiting the replication and transcription of DNA, destroying the biological functions of bacteria, and finally achieving an antibacterial effect. Silver ion antibacterial agents have high efficiency and stability and are widely used. Embodiment 3 Silver nitrate is added to reaction initiator water, and silver ions are encapsulated in the coating with the reaction of octadecyl triethoxysilane and water, attached to the fabric surface, and have an antibacterial effect while the fabric is super-hydrophobic modified, and have excellent bactericidal effects on Escherichia coli and Staphylococcus aureus.
[0068] Organosilicon quaternary ammonium salt antimicrobial agent is a new type of antimicrobial agent, which is made by introducing siloxane into the chemical structure of quaternary ammonium salt antimicrobial agent. It has no obvious irritation to human skin and has extremely low toxicity. It acts on the surface of bacteria and can destroy the cell wall and cell membrane of bacteria. It also has an extremely obvious inhibitory or killing effect on pathogenic bacteria. It has a high-efficiency and broad-spectrum antimicrobial function, and is washable and heat-resistant, and has strong antimicrobial durability. In addition, fabrics treated with organosilicon quaternary ammonium salt antimicrobial agent can also achieve excellent softness and antistatic properties.
[0069] Example 3 Adding organosilicon quaternary ammonium salt to n-hexane makes the hydrophobically modified fabric have antibacterial properties. Figure 5 As shown, the modified cotton fabric has obvious bactericidal effect on Escherichia coli and Staphylococcus aureus. After 24 hours of cultivation, no colonies grow on the agar medium, and the bactericidal efficiency against Escherichia coli and Staphylococcus aureus reaches 99.99%.
[0070] (3) Characterization of air permeability and mechanical properties:
[0071] The tensile strength of polyester and cotton fabrics before and after antibacterial hydrophobic modification was tested using a universal material testing machine. The sample holding distance was 40 mm and the tensile speed was 20 mm / min. The stress-strain curves of the fabric (using the super-hydrophobic coating mixture obtained in Example 3) before and after antibacterial super-hydrophobic modification are shown in Figure 2. Figure 6 As shown in (c) and (d) in . Figure 6 As shown in (c) and (d), after antibacterial superhydrophobic modification, the tensile stress and strain of cotton fabric decreased by 2.1% and 1.2%, respectively, and the tensile stress and strain of polyester fabric decreased by 5.5% and 2.1%, respectively. This is because the addition of trace amounts of octadecyltrichlorosilane generates acidic gas during the catalytic reaction, which causes certain damage to the mechanical properties of the fabric.
[0072] The air permeability of cotton fabrics under different experimental parameters was evaluated using a fully automatic air permeability meter with a measuring pressure of 100 Pa and a measuring area of 20 cm. 2 , the results are as follows Figure 6 As shown in (a) and (b) in . Figure 6 It can be seen from (a) and (b) that the air permeability of the original cotton fabric is 270 mm / s, and the air permeability of the cotton fabric after antibacterial and hydrophobic treatment in Example 3 is 221.7 mm / s. Compared with the original cotton fabric, the air permeability of the fabric after modification with the antibacterial and hydrophobic coating decreases slightly, because the air permeability of the fabric is mainly determined by the porosity, and the antibacterial and hydrophobic coating self-assembled on the fabric surface reduces the porosity of the fabric, thereby causing the air permeability of the modified fabric to decrease.
[0073] (4) Characterization of coating durability:
[0074] In order to test the durability of the coating surface structure and performance, the fabric after antibacterial hydrophobic treatment was subjected to a water dripping test, a washing test and a post-washing antibacterial test. After the antibacterial hydrophobic treatment (using the super hydrophobic coating mixture obtained in Example 3), continuous water drops were provided by a disposable syringe and dripped on the cotton fabric placed at a 30° tilt to further characterize the hydrophobicity and durability of the coating. Figure 7 As shown in (a), before dripping water, the contact angle of the coated fabric was 156.3°. After 24 hours of dripping water, the contact angle of the fabric was still 146.4°.
[0075] The antibacterial and hydrophobic stability tests were conducted using the household double-drum washing machine washing method in the national standard GB / T 20944.3-2008 test standard. The cotton fabric that had been treated with antibacterial and hydrophobic treatment was treated for water resistance using a household drum washing machine. During the experiment, 20g of sample, 180g of wash fabric, 12g of detergent (AATCC1993 WOB phosphorus-free standard detergent) and 6L of water (40±3℃) were washed in a household drum washing machine for 25 minutes, then drained and then washed with 6L of tap water for 2 minutes, the fabric was taken out and centrifuged for 1 minute, then washed with 6L of tap water for 2 minutes, and the fabric was taken out and centrifuged for 1 minute. Repeat this procedure for multiple washing treatments, measure the change in the contact angle of the fabric, and test the antibacterial properties of the fabric by the oscillation method. Figure 7 As shown in (b), after 30 washes, the contact angle of the fabric is still 140.9°, and the bactericidal efficiency against Escherichia coli and Staphylococcus aureus reaches 99.98%.
[0076] The above description of the embodiments is to facilitate those skilled in the art to understand and use the present invention. Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by those skilled in the art within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing a super hydrophobic antifouling coating with antibacterial function, characterized in that The following steps are involved: S1, mixing n-octadecyltriethoxysilane, water and octadecyltrichlorosilane uniformly, and then standing to react to obtain a super hydrophobic reaction product; S2. Dilute and disperse the super-hydrophobic reaction product obtained in step S1 with n-hexane to obtain a super-hydrophobic coating mixture.
2. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 1, characterized in that: In step S1: the usage ratio of n-octadecyltriethoxysilane and water is 1 ml: 20-80 μL; the usage ratio of octadecyltrichlorosilane and n-octadecyltriethoxysilane is 1-6 μL: 1 ml.
3. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 1, characterized in that: In step S1: after the n-octadecyltriethoxysilane, water and octadecyltrichlorosilane are mixed, they are first placed on a vortex mixer for mixing, and then placed in an ultrasonic cleaner for ultrasonic vibration treatment.
4. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 1, characterized in that: In step S1: the standing reaction time is 1-5h.
5. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 1, characterized in that: In step S1: silver nitrate is also added when preparing the super-hydrophobic reaction product; silver nitrate is first added to water to prepare a silver nitrate solution; and then n-octadecyltriethoxysilane, octadecyltrichlorosilane and the silver nitrate solution are uniformly mixed.
6. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 5, characterized in that: The concentration of the silver nitrate solution is 0.5-5wt%.
7. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 1, characterized in that: In step S2: n-hexane is added to the super-hydrophobic reaction product; the volume fraction of the super-hydrophobic reaction product in the obtained super-hydrophobic coating mixture is 1-10%.
8. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 1, characterized in that: In step S2: a quaternary ammonium organosilicon salt is also added when preparing the super-hydrophobic coating mixture.
9. The method for preparing a super hydrophobic antifouling coating with antibacterial function according to claim 8, characterized in that: First, a quaternary ammonium salt of organic silicon is added to n-hexane to obtain a quaternary ammonium salt of organic silicon / n-hexane solution, and then the quaternary ammonium salt of organic silicon / n-hexane solution is added to a superhydrophobic reaction product for mixing; the mass volume ratio of the added amount of the quaternary ammonium salt of organic silicon to the amount of n-hexane used is 0.01-0.04 g / ml.
10. Application of the super-hydrophobic coating mixture prepared by any method of claims 1-9 in surface modification of solid materials, the specific steps being as follows: The solid material is immersed in the obtained super-hydrophobic coating mixture, taken out after 12-24 hours, washed with n-hexane, and then dried in the air; or the obtained super-hydrophobic coating mixture is transferred to a spray bottle and sprayed on the solid material to obtain a super-hydrophobic antifouling coating with antibacterial function.
Citation Information
Patent Citations
Super-hydrophobic anti-bacterial finishing agent as well as preparation method and application thereof
CN111118888A
Super-hydrophobic agent, super-hydrophobic agent preparation method and self-repairing super-hydrophobic structure
CN114106694A
Preparation method and application of super-hydrophobic silicon oxide nanowires and preparation method of super-hydrophobic coating
CN118419943A
Coating composition having antibiotic and ultrawater-repellent property, preparation method thereofand coating method using the coating composition
KR1020060107089A
Method for super-hydrophobic coating
KR102019315B1
Cited By
Antibacterial epoxy resin coating and preparation method thereof
CN119978942A