Catalyst component and preparation method thereof, catalyst system and application thereof
By forming a mixture of two liquid phases in the catalyst preparation and controlling the separation of the magnesium phase, the problems of catalyst particle morphology and particle size distribution are solved, efficient preparation and performance improvement of the catalyst are achieved, and the agglomeration of the catalyst and complex process are avoided. sex.
Patent Information
- Application Number
- CN202111265120.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-28
AI Technical Summary
It is difficult to prepare a supported Ziegler-Natta catalyst with good particle morphology and narrow particle size distribution in the prior art, and the agglomeration phenomenon and high viscosity problems of the catalyst are difficult to solve, affecting the operation of the industrial device.
The catalyst group is prepared by mixing the organophosphorus compound and the titanium-containing compound with an inert dispersion medium to form a mixture of at least two liquid phases and mixing it with a magnesium halide compound and a Lewis base, and heating is raised in the presence of a supplementary precipitant and a surfactant to obtain a catalyst group The crystallization process of the catalyst is controlled by avoiding the early separation of the magnesium phase and the solvent phase.
The prepared catalyst has good particle size, narrow particle size distribution, adjustable average particle size, excellent performance, high activity and strong stereotactic orientation ability, reducing the agglomeration phenomenon and process complexity of the catalyst.
Smart Images

Figure CN116041579B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of catalysts, and specifically relates to catalyst components and preparation methods thereof, catalyst systems and applications thereof. Background Art
[0002] Supported Ziegler-Natta catalysts have been widely developed because their morphology can be regulated by the support morphology, especially olefin polymerization catalysts supported by magnesium chloride supports. The preparation of catalysts with good particle morphology is beneficial to the operation of industrial devices and has always been one of the keys to catalyst development.
[0003] For example, well-known high-speed stirring technology, high-pressure extrusion technology, spray technology, ultra-gravity technology, etc. can be used to prepare magnesium compounds or complex solid carriers with good particle morphology, which are then contacted with titanium-containing compounds and loaded with internal electron donor compounds to form catalyst components. The morphology and particle size distribution of the catalyst in this type of technology are determined by the pre-prepared carrier, which can usually be spherical. However, these technologies usually have high energy consumption and complex processes, and cannot produce catalyst components in a continuous manner.
[0004] In addition, a titanium-containing magnesium-based solid can be prepared by crystallization, and an internal electron donor compound can be loaded to form a catalyst component. This technology can produce catalyst components in a continuous process. Early patents such as CN85100997A and CN1097597C precipitate granular catalysts with a wide particle size distribution. Later patents such as EP01115000, US13087210 and US14512130 use emulsion technology to control the crystallization process, and the precipitation form changes from granular to spherical, and the particle size distribution becomes narrower. It is well known that the premise for forming an emulsion is that the system must contain at least two liquid phases, a continuous phase and a dispersed phase. For example, EP01115000 uses perfluorinated hydrocarbons as a continuous phase, but the cost is very high. US13087210 and US14512130 use solvent selection to separate the solvent phase and the magnesium phase, but the viscosity of the magnesium phase is too high and it is very easy to become sticky, and the precipitate will inevitably agglomerate, which is not conducive to the operation of industrial equipment. Therefore, designing a system containing two liquid phases that can be used for the preparation of olefin catalysts is crucial for preparing catalysts with good particle morphology. Summary of the invention
[0005] The object of the present invention is to provide an olefin polymerization catalyst component, which has a good particle shape, a narrow particle size distribution, an adjustable average particle size, and excellent catalyst performance. Another object of the present invention is to provide a method for preparing the catalyst component of the present invention. The method of the present invention does not require the magnesium phase and the solvent phase in the magnesium-containing solution to be separated into two phases in advance, avoids the stickiness problem after the magnesium phase is separated in the solution, reduces the agglomeration phenomenon of the catalyst, and the catalyst crystallization process is easier to control, which is suitable for scale-up preparation. The present invention also aims to provide an application of the catalyst system of the present invention.
[0006] In a first aspect, the present invention provides a method for preparing a catalyst component, comprising the following steps:
[0007] (1) mixing an organic phosphorus compound and a titanium-containing compound with an inert dispersion medium, optionally an aromatic hydrocarbon solvent, to form a mixture M1 containing at least two liquid phases;
[0008] (2) mixing a magnesium halide compound, a Lewis base and an organic solvent to form a magnesium-containing solution;
[0009] (3) mixing the mixture M1, the magnesium-containing solution, optionally a Lewis acid, and optionally an inert dispersion medium to form a mixture M2;
[0010] (4) heating the mixture M2 in the presence of a precipitation aid, a surfactant and optionally an internal electron donor compound to obtain a solid; and
[0011] (5) optionally mixing the solid material and an internal electron donor compound to obtain the catalyst component;
[0012] Wherein, an internal electron donor compound is present in the operation in step (4) and / or step (5).
[0013] The inventors unexpectedly found that the catalyst spherical solid prepared by the method of the present invention has a good particle shape, a narrow particle size distribution, an adjustable average particle size, and excellent catalyst performance, with high activity and stereo-orientation ability. Without wishing to be bound by theory, this may be attributed to the fact that the method of the present invention prepares a two-phase system, and the method of the present invention does not require the magnesium phase and the solvent phase in the magnesium-containing solution to be separated into two phases in advance, avoiding the stickiness problem of the magnesium phase in the solution after separation, reducing the agglomeration phenomenon of the catalyst, and the catalyst crystallization process is easier to control, suitable for scale-up preparation.
[0014] The present invention uses an organic phosphorus compound and a titanium-containing compound to mix in an inert dispersion medium, optionally an aromatic hydrocarbon solvent, to form a mixture M1 containing at least two liquid phases, instead of adding an inert dispersion medium to a magnesium-containing solution in advance to prepare a two-phase system as described in many documents. Because, on the one hand, it is to avoid the stickiness problem caused by the high viscosity and high concentration of the magnesium phase after the magnesium phase and the solvent phase in the magnesium-containing solution are separated into two phases, so that the agglomeration phenomenon of the catalyst can be reduced. On the other hand, it can also be deeply recognized that the dispersed phase of the mixture M2, i.e., the emulsion system before the temperature is raised and precipitated, not only contains the magnesium phase, but also contains the dispersed phase of the mixture M1, which helps to control the crystallization process of the catalyst component.
[0015] Preferably, in the method for preparing the catalyst component of the present invention, the organophosphorus compound is selected from one or more of the compounds represented by formula (I) and formula (II):
[0016]
[0017] Wherein, R1, R2, R3, R4, R5 and R6 are each independently selected from a straight-chain alkyl group of 1-20 carbon atoms, a branched-chain alkyl group of 3-20 carbon atoms, a cycloalkane group of 3-20 carbon atoms, a halogenated hydrocarbon group of 1-20 carbon atoms or an aromatic hydrocarbon group of 6-20 carbon atoms and an aromatic hydrocarbon group with a substituent.
[0018] Preferably, in the method for preparing the catalyst component of the present invention, the organophosphorus compound is selected from one or more of trimethyl phosphate, triethyl phosphate, tributyl phosphate, tripentyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite and benzyl phosphite.
[0019] Preferably, in the method for preparing the catalyst component of the present invention, the general formula of the titanium-containing compound is as shown in formula (III):
[0020] TiX m (OR a ) 4-m Formula (III)
[0021] Where X is a halogen, R a It is a hydrocarbon group of 1 to 20 carbon atoms, and m is an integer of 1 to 4.
[0022] Preferably, in the method for preparing the catalyst component of the present invention, the titanium-containing compound is selected from one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, tetrabutoxytitanium, tetraethoxytitanium, triethoxytitanium monochloride, diethoxytitanium dichloride and monoethoxytitanium trichloride.
[0023] Preferably, in the method for preparing the catalyst component of the present invention, the inert dispersion medium is selected from one or more of silicone oil, kerosene, paraffin oil, white oil, vaseline oil, methyl silicone oil, aliphatic and cycloaliphatic hydrocarbons.
[0024] Preferably, in the method for preparing the catalyst component of the present invention, the inert dispersion medium is selected from one or more of white oil, hexane, heptane, octane, nonane, decane, dodecane and cyclohexane.
[0025] Preferably, in the method for preparing the catalyst component of the present invention, the aromatic hydrocarbon solvent is selected from one or more of toluene, ethylbenzene, benzene, xylene and chlorobenzene.
[0026] Preferably, in the method for preparing the catalyst component of the present invention, the magnesium halide compound has the general formula MgX2, wherein X is bromine, chlorine or iodine.
[0027] Preferably, in the method for preparing the catalyst component of the present invention, the Lewis base is selected from one or more of an organic epoxy compound, an organic phosphorus compound and a hydroxyl-containing compound.
[0028] Preferably, in the method for preparing the catalyst component of the present invention, the organic epoxy compound is selected from one or more of the oxidation products of C2-C8 aliphatic olefins and C2-C8 halogenated aliphatic olefins.
[0029] Preferably, in the method for preparing the catalyst component of the present invention, the organic epoxy compound is selected from one or more of ethylene oxide, propylene oxide, ethylene oxide, epichlorohydrin, butylene oxide, butadiene oxide, butadiene dioxide, methyl glycidyl ether and diglycidyl ether.
[0030] Preferably, in the method for preparing the catalyst component of the present invention, the general formula of the hydroxyl-containing compound is as shown in formula (IV):
[0031] HOR b Formula (IV)
[0032] Where R b It is a hydrocarbon group of 2 to 20 carbon atoms.
[0033] Preferably, in the method for preparing the catalyst component of the present invention, the hydrocarbon group is a saturated or unsaturated straight-chain or branched alkane group, cycloalkane group or aromatic hydrocarbon group.
[0034] Preferably, in the method for preparing the catalyst component of the present invention, the hydroxyl-containing compound is an alcohol compound.
[0035] Preferably, in the method for preparing the catalyst component of the present invention, the hydroxyl-containing compound is selected from one or more of ethanol, propanol, butanol, 2-ethylhexanol, benzyl alcohol and phenylethyl alcohol.
[0036] Preferably, in the method for preparing the catalyst component of the present invention, the organic solvent is an aromatic hydrocarbon or a halogenated hydrocarbon compound.
[0037] Preferably, in the method for preparing the catalyst component of the present invention, the organic solvent is selected from one or more of toluene, ethylbenzene, benzene, xylene and chlorobenzene.
[0038] Preferably, in the method for preparing the catalyst component of the present invention, the Lewis acid comprises one or more of a titanium-containing compound and a silicon-containing compound.
[0039] Preferably, in the method for preparing the catalyst component of the present invention, the general formula of the silicon-containing compound is as shown in formula (V):
[0040] SiX 1 n R c 4-n Formula (V)
[0041] Where X 1 is halogen, preferably chlorine, bromine or iodine; R c is a hydrocarbon group having 1 to 20 carbon atoms; and n is an integer of 1 to 4.
[0042] Preferably, in the method for preparing the catalyst component of the present invention, the silicon-containing compound is silicon tetrachloride.
[0043] Preferably, in the method for preparing the catalyst component of the present invention, the precipitation aid is selected from one or more of acetic anhydride, phthalic anhydride, succinic anhydride, maleic anhydride, pyromellitic anhydride, acetic acid, propionic acid, butyric acid, acrylic acid, methacrylic acid, acetone, methyl ethyl ketone, benzophenone, methyl ether, ethyl ether, propyl ether, butyl ether and pentyl ether.
[0044] Preferably, in the method for preparing the catalyst component of the present invention, the surfactant is selected from one or more of alcoholysis products of maleic anhydride polymers, alcoholysis products of maleic anhydride copolymers, (meth)acrylic acid alkyl ester polymers and (meth)acrylic acid alkyl ester copolymers.
[0045] Preferably, in the preparation method of the catalyst component described in the present invention, the surfactant is selected from one or more of the group consisting of polymaleic anhydride alcoholysis products, maleic anhydride-styrene copolymer alcoholysis products, maleic anhydride-styrene-(meth)acrylate terpolymer alcoholysis products, maleic anhydride-(meth)acrylate alkyl ester alcoholysis products, poly(meth)acrylate alkyl esters, (meth)acrylate alkyl ester-maleic anhydride copolymers, and (meth)acrylate alkyl ester-maleic anhydride-styrene copolymers.
[0046] Preferably, in the method for preparing the catalyst component of the present invention, the internal electron donor compound is selected from one or more of esters, ethers, ketones, amines and silanes.
[0047] Preferably, in the method for preparing the catalyst component of the present invention, the internal electron donor compound is selected from one or more of monovalent or polyvalent aliphatic carboxylic acid esters, aromatic carboxylic acid esters, diol ester compounds and diether compounds.
[0048] Preferably, in the method for preparing the catalyst component of the present invention, the internal electron donor compound is selected from one or more of phthalates, malonates, succinates, glutarates, glycol esters, 1,3-diethers, pivalates and carbonates.
[0049] Preferably, in the preparation method of the catalyst component described in the present invention, the internal electron donor compound is selected from one or more of di-n-butyl phthalate, diisobutyl phthalate, 2,4-pentanediol dibenzoate, 3,5-heptanediol dibenzoate, diethyl 2,3-diisopropylsuccinate, diisobutyl 2,3-diisopropylsuccinate, di-n-butyl 2,3-diisopropylsuccinate, dimethyl 2,3-diisopropylsuccinate, diisobutyl 2,2-dimethylsuccinate, diisobutyl 2-ethyl-2-methylsuccinate, diethyl 2-ethyl-2-methylsuccinate, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
[0050] Preferably, in the method for preparing the catalyst component of the present invention, the mixing in step (1) is carried out under the following conditions: the mixing temperature is -20°C-100°C, preferably 0°C-50°C; the mixing time is 0.01-10 hours, preferably 0.01-3 hours.
[0051] Preferably, in the method for preparing the catalyst component of the present invention, the mixing in step (2) is carried out under the following conditions: the mixing temperature is 10°C-150°C, preferably 30°C-130°C; the mixing time is 0.05-10 hours, preferably 0.1-6 hours.
[0052] Preferably, in the method for preparing the catalyst component of the present invention, the mixing in step (3) is carried out at -20°C to 60°C, preferably -10°C to 40°C.
[0053] Preferably, in the method for preparing the catalyst component of the present invention, the heating in step (4) is carried out under the following conditions: the mixture is heated to 20°C to 120°C, preferably 50°C to 100°C, and maintained for 0.1h to 24h after heating; the heating time is 1 minute to 36 hours, preferably 3 minutes to 24 hours.
[0054] Preferably, in the method for preparing the catalyst component of the present invention, per mole of magnesium halide,
[0055] The organic phosphorus compound is 0.1 to 10 moles, preferably 0.4 to 4 moles; and / or
[0056] The titanium-containing compound is 0.5 to 25 moles, preferably 1 to 20 moles; and / or
[0057] The inert dispersion medium is 0.1 g to 300 g, preferably 1 g to 150 g; and / or
[0058] The aromatic hydrocarbon solvent is 0.1 to 40 mol, preferably 0.1 to 30 mol; and / or
[0059] The organic epoxy compound is 0.1 to 10 moles, preferably 0.4 to 4 moles; and / or
[0060] The hydroxyl-containing compound is 0.1 to 10 moles, preferably 0.1 to 5 moles; and / or
[0061] The organic solvent is 0.1 to 40 mol, preferably 0.1 to 30 mol; and / or
[0062] The silicon-containing compound is 0.5 to 25 mol, preferably 0.5 to 20 mol; and / or
[0063] The precipitation aid is 0.01 to 1 mol, preferably 0.04 to 0.4 mol; and / or
[0064] The internal electron donor is 0.01-1 mol; and / or
[0065] The surfactant is present in an amount of 0.01 g to 5 g, preferably 0.05 g to 1 g, per gram of magnesium halide.
[0066] In a second aspect, the present invention provides a catalyst component, which is prepared by the method for preparing the catalyst component of the present invention.
[0067] In a third aspect, the present invention provides a catalyst system comprising the catalyst component of the present invention, an alkyl aluminum compound and optionally an external electron donor compound.
[0068] Preferably, in the catalyst system of the present invention, the general formula of the alkyl aluminum compound is AlR n X 3-n , wherein R is hydrogen, a hydrocarbon group having 1 to 20 carbon atoms, preferably an alkyl group, an aralkyl group, or an aryl group; X is a halogen, and n is an integer of 1 to 3.
[0069] Preferably, in the catalyst system described in the present invention, the alkyl aluminum compound is selected from one or more of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, trioctylaluminum, diethyl aluminum monohydrogenate, diisobutyl aluminum monohydrogenate, diethyl aluminum monochloride, diisobutyl aluminum monochloride, sesquiethyl aluminum chloride and ethyl aluminum dichloride.
[0070] Preferably, in the catalyst system of the present invention, the molar ratio of the aluminum in the alkyl aluminum compound to the titanium in the catalyst component is 5-5000:1, preferably 20-800:1.
[0071] Preferably, in the catalyst system of the present invention, the general formula of the external electron donor compound is R' n Si(OR y ) 4-n , wherein n is an integer of 0-3, and R' is selected from one or more of an alkyl group, a cycloalkyl group, an aryl group, a halogenated alkyl group, a halogen group and a hydrogen atom; R y One or more selected from alkyl, cycloalkyl, aryl and halogenated alkyl.
[0072] Preferably, the external electron donor compound is selected from one or more of trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyltert-butyldimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, dicyclohexyldimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, methylcyclohexyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane.
[0073] Preferably, in the catalyst system of the present invention, the molar ratio of the aluminum in the alkyl aluminum compound to the external electron donor compound is 0.1-500:1, preferably 1-300:1, more preferably 3-100:1.
[0074] In a fourth aspect, the present invention further provides use of the catalyst component or catalyst system of the present invention in the field of olefin polymerization.
[0075] Specific embodiments of the present invention are further described below.
[0076] In a specific embodiment of the present invention, the organophosphorus compound is tributyl phosphate.
[0077] In a specific embodiment of the present invention, the titanium-containing compound is titanium tetrachloride.
[0078] In a specific embodiment of the present invention, the inert dispersion medium is selected from one or more of white oil, hexane and decane.
[0079] In a specific embodiment of the present invention, the aromatic hydrocarbon solvent is toluene.
[0080] In a specific embodiment of the present invention, the mixing method for forming the mixture M1 containing at least two liquid phases is not particularly limited. The purpose of mixing is to form a mixture containing at least two liquid phases.
[0081] In a specific embodiment of the present invention, one of the two liquid phases contains at least an inert dispersion medium and the other liquid phase contains at least reactants of an organic phosphorus compound and a titanium-containing compound.
[0082] In a specific embodiment of the present invention, the magnesium halide compound is magnesium dichloride.
[0083] In a specific embodiment of the present invention, the organic epoxy compound is epichlorohydrin.
[0084] In a specific embodiment of the present invention, the organic solvent is toluene.
[0085] In a specific embodiment of the present invention, the mixing method for forming the magnesium-containing solution is not particularly limited, and the purpose of mixing is to form a uniform solution containing magnesium.
[0086] In a specific embodiment of the present invention, the silicon-containing compound is silicon tetrachloride.
[0087] In a specific embodiment of the present invention, the mixture M1, the magnesium-containing solution, the optional Lewis acid, and the optional inert dispersion medium may be mixed in any manner to form the mixture M2. Specifically, for example, the mixture M1 formed in step S1 may be mixed with the magnesium-containing solution to form the mixture M2; the magnesium-containing solution may be mixed with the Lewis acid and then mixed with the mixture M1 formed in step S1 to form the mixture M2; the magnesium-containing solution, the Lewis acid, and the inert dispersion medium may be mixed and then mixed with the mixture M1 formed in step S1 to form the mixture M2; the mixture M1 formed in step S1 may be mixed with the magnesium-containing solution and then mixed with the Lewis acid to form the mixture M2;
[0088] In a specific embodiment of the present invention, the mixture M2 includes colloids, two-phase solutions, emulsions and other forms. Preferably, the mixture is in the form of a mixture containing at least two liquid phases. In this way, in the presence of a surfactant, one or more methods such as vibration, stirring, atomization, shearing, etc. can be used to promote the mixture to form a uniform emulsion, thereby solidifying and precipitating spherical solids.
[0089] In a specific embodiment of the present invention, the precipitation aid is phthalic anhydride.
[0090] In a specific embodiment of the present invention, the surfactant is selected from one or more of the alcoholysis products of maleic anhydride polymers and the alcoholysis products of maleic anhydride copolymers, preferably one or more of the alcoholysis products of polymaleic anhydride, the alcoholysis products of maleic anhydride-styrene copolymers, the alcoholysis products of maleic anhydride-styrene-(meth)acrylate alkyl ester terpolymers, and the alcoholysis products of maleic anhydride-(meth)acrylate alkyl ester copolymers, wherein the alkyl ester side chain is a straight or branched alkyl, cycloalkyl or aromatic hydrocarbon group with 1 to 30 carbon atoms, preferably those with 1 to 20 carbon atoms; the alcoholysis product refers to a polymer product obtained by reacting the product with an organic alcohol compound, such as an organic alcohol compound having a structure of ROH, wherein R is a straight or branched alkyl, cycloalkyl or aromatic hydrocarbon group with 2 to 20 carbon atoms.
[0091] In a specific embodiment of the present invention, the surfactant described in the present invention also comprises at least one of a (meth)acrylic acid alkyl ester polymer and a (meth)acrylic acid alkyl ester copolymer, for example, it may be at least one of a poly (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester-maleic anhydride copolymer, and a (meth)acrylic acid alkyl ester-maleic anhydride-styrene copolymer; wherein the ester side chain is a straight or branched alkane group, a cycloalkane group or an aromatic hydrocarbon group having 1 to 30 carbon atoms, preferably those having 1 to 20 carbon atoms.
[0092] In a specific embodiment of the present invention, the poly (meth) acrylate polymer surfactant of the present invention can be a pour point depressant product purchased from an additive company with the trademark name T602.
[0093] In a specific embodiment of the present invention, the surfactant may be added at any position in the preparation method, and may be added as a whole or in a dispersed manner.
[0094] In a specific embodiment of the present invention, if a surfactant, especially the above-mentioned surfactant, is not used, the prepared magnesium-based carrier will be in powder form, and a magnesium-based carrier with a spherical or quasi-spherical structure cannot be prepared.
[0095] In a specific embodiment of the present invention, the internal electron donor compound can be added at any position in the preparation method, and can be added as a whole or in a dispersed manner. In a specific embodiment of the present invention, the internal electron donor compound can be added as a whole or in part to the uniform solution containing magnesium element; it can be added as a whole or in part after the mixture M2 is formed and during the solidification, temperature rise and precipitation process.
[0096] In a specific embodiment of the present invention, the mixture is heated to a target temperature so that the solid catalyst is precipitated from the mixture, wherein the target temperature is 20°C to 120°C, preferably 50°C to 100°C.
[0097] In some preferred embodiments of the present invention, in step S4, after the temperature is raised, the target temperature is maintained for 0.1 h to 24 h under stirring. In a specific embodiment of the present invention, after the solid is precipitated from the mixture, the suspension is stirred at a certain temperature for a certain time, such as 10 minutes to 24 hours, in order to make the crystal morphology more stable and improve the particle strength.
[0098] In a specific embodiment of the present invention, the temperature-raising process of the mixture is not specifically limited, and any known method can be used for heating, such as slow, step-by-step, fast or programmed heating. The specific heating method should be adjusted according to the specific formula, mixing temperature, etc.; and the inventors have found that in the preparation method of the present invention, when other conditions are the same, different heating processes will affect the particle morphology and particle size distribution of the final catalyst. Specifically, a slower heating process can obtain a better particle morphology, whereas a too fast heating rate will lead to a deterioration of the particle shape. Therefore, the mixture heating process can be 1 minute to 36 hours, preferably 3 minutes to 24 hours.
[0099] In a specific embodiment of the present invention, the solid is mixed with the internal electron donor after it is precipitated or after it is precipitated and filtered and washed.
[0100] In a specific embodiment of the present invention, the temperature at which the internal electron donor compound is added may be 10°C-150°C, preferably 10°C-100°C.
[0101] In a specific embodiment of the present invention, the mixing time of the solid material and the internal electron donor compound can be 0.05-8 hours, preferably 1-6 hours.
[0102] In a specific embodiment of the present invention, the catalyst component has a spherical or spheroidal structure.
[0103] In a specific embodiment of the present invention, the average particle size of the catalyst component is 1 μm to 150 μm.
[0104] In a specific embodiment of the present invention, the alkylaluminum compound is triethylaluminum and / or triisobutylaluminum.
[0105] In a specific embodiment of the present invention, the external electron donor compound is cyclohexylmethyldimethoxysilane.
[0106] In a particular embodiment of the invention, the olefin comprises propylene.
[0107] In a specific embodiment of the present invention, the olefin polymerization catalyst system of the present invention can be used for the homopolymerization of olefins, and can also be used for copolymerizing multiple olefins. At least one of the olefins is an olefin represented by the formula CH2=CHR, wherein R is hydrogen or a straight or branched alkyl group of C1-C6. Specific examples of the olefin represented by the formula CH2=CHR can include: ethylene, propylene, 1-n-butene, 1-n-pentene, 1-n-hexene, 1-n-octene and 4-methyl-1-pentene. Preferably, the olefin represented by the formula CH2=CHR is one or more of ethylene, propylene, 1-n-butene, 1-n-hexene and 4-methyl-1-pentene. More preferably, the olefin represented by the formula CH2=CHR is propylene, or copolymerization of propylene with other olefins.
[0108] In a specific embodiment of the present invention, the polymerization of olefins is carried out according to known methods, in the liquid phase of a liquid monomer or a solution of a monomer in an inert solvent, or in the gas phase, or by a combined polymerization process in the gas and liquid phase. The polymerization temperature is generally 0° C. to 150° C., preferably 60° C. to 100° C. The polymerization pressure is normal pressure or higher.
[0109] The present invention has the following beneficial effects:
[0110] The catalyst spherical solid prepared by the method of the present invention has a good particle shape, a narrow particle size distribution, an adjustable average particle size, and excellent catalyst performance, and has high activity and stereo-orientation ability. The method of the present invention does not require the magnesium phase and the solvent phase in the magnesium-containing solution to be separated into two phases in advance, avoids the stickiness problem after the magnesium phase is separated in the solution, reduces the agglomeration phenomenon of the catalyst, and the catalyst crystallization process is easier to control, which is suitable for scale-up preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0111] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention. In the accompanying drawings:
[0112] Figure 1 This is a diagram of the catalyst components prepared in Example 1.
[0113] Figure 2 This is a diagram of the catalyst components prepared in Comparative Example 1. DETAILED DESCRIPTION
[0114] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.
[0115] The present invention is described in detail below by way of examples, but the protection scope of the present invention is not limited to the following description.
[0116] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be obtained through commercial channels.
[0117] 1. Determination of titanium content in catalyst: Use UV-Vis spectrophotometer 722 for colorimetric determination.
[0118] 2. Magnesium content is measured by magnesium ion and EDTA complexometric titration.
[0119] 3. Catalyst particle size distribution: measured by Malvern 2000 n-hexane dispersant laser diffraction method.
[0120] 4. Determination of the content of internal electron donor compounds in the catalyst: The chromatographic method is used. The catalyst dry powder is decomposed with dilute acid, and the internal electron donor compounds are extracted with an extractant. The internal electron donor compounds are determined using an Agilent 6890N gas chromatograph.
[0121] 5. The bulk density (BD) of polymers is determined according to ASTM D1895-96.
[0122] 6. The isotacticity index (II) of propylene polymer is determined by the heptane extraction method: 2 g of dried polymer sample is placed in an extractor and extracted with boiling heptane for 6 hours. The residue is dried to constant weight. The ratio of the obtained polymer weight (g) to 2 (g) is the isotacticity.
[0123] 7. The melt flow index (MI) of the polymer is measured using the MI-4 melt flow index tester from GOTTFERT, Germany, in accordance with GB / T 3682.1-2018 standard.
[0124] Example 1
[0125] A. Preparation of two-phase mixture
[0126] In a reactor that has been repeatedly replaced with high-purity nitrogen, 210 g of food-grade No. 100 white oil and 29.3 g of tributyl phosphate are added, then the temperature is lowered to 20° C., 258.9 g of titanium tetrachloride is added, and the mixture is stirred at 400 RMP to obtain a two-phase mixture.
[0127] B. Preparation of magnesium-containing solution
[0128] In another reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 180g of toluene, 10.7g of epichlorohydrin, and 42.5g of tributyl phosphate are added in sequence, and stirred at 300RMP for 2 hours at a temperature of 60°C. Then, a mixture of 5.7g of T602 diluted with 2.7g of phthalic anhydride and 27.8g of toluene is added, and the temperature is maintained at 60°C for another hour. Then the temperature is lowered to 20°C to prepare a magnesium-containing solution.
[0129] C. Preparation of catalyst components
[0130] Add the magnesium-containing solution prepared in step B to the two-phase mixture prepared in step A, maintain stirring at 400RMP, and continue to maintain stirring for 1 hour after the addition is completed. Gradually heat to 80°C within 3 hours and maintain for 1 hour. Filter the mother liquor and wash it twice with 200ml of toluene. Remove the filtrate, add 200ml of toluene, 3ml of di-n-butyl phthalate, raise the temperature to 85 degrees, keep the temperature constant for 1 hour, and remove the filtrate. Add 120ml of toluene, 80ml of titanium tetrachloride, treat at 110°C for 1 hour, remove the filtrate, and repeat the treatment once. After washing repeatedly with 200ml of hexane 5 times, a solid olefin polymerization catalyst component is obtained. The average particle size D50 of the solid obtained in this embodiment is 46.5μm, and the SPAN value is 0.72. Catalyst component data is shown in Table 1. Catalyst component picture is shown in Figure 1 .
[0131] Propylene polymerization: In a 5-liter autoclave, after nitrogen is fully replaced, 5 ml of triethylaluminum hexane solution (the concentration of triethylaluminum is 0.5 mmol / ml), 1 ml of cyclohexylmethyldimethoxysilane (CHMMS) hexane solution (the concentration of CHMMS is 0.1 mmol / ml), 10 ml of anhydrous hexane and 10 mg of the catalyst component of Example 1 are added at room temperature. 1 liter of hydrogen under standard conditions and 1.15 kg of liquid propylene are introduced. The temperature is raised to 70°C and the polymerization reaction is carried out at 70°C for 1 hour. After the reaction is completed, the reactor is cooled and stirring is stopped to discharge the reaction product to obtain an olefin polymer. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0132] Example 2
[0133] A Preparation of two-phase mixture
[0134] In a reactor that has been repeatedly replaced with high-purity nitrogen, 178g of food-grade No. 26 white oil, 19.5g of toluene and 44g of tributyl phosphate are added. Then the temperature is lowered to -20°C, 258.9g of titanium tetrachloride is added, and the mixture is stirred at 400 RMP to obtain a two-phase mixture.
[0135] B Preparation of magnesium solution
[0136] In another reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 180g of toluene, 10.7g of epichlorohydrin, and 27.8g of tributyl phosphate are added in sequence, and stirred at 300RMP for 2 hours at a temperature of 60°C. Then, a mixture of 5.7g of T602 diluted with 2.7g of phthalic anhydride and 27.8g of toluene is added, and the temperature is maintained at 60°C for another hour. Then the temperature is lowered to 0°C to prepare a magnesium-containing solution.
[0137] C Solid Preparation
[0138] Add the magnesium-containing solution prepared in step B to the two-phase mixture prepared in step A, maintain stirring at 400 RMP, and continue to maintain stirring for 1 hour after the addition is completed. Gradually heat to 80°C within 5 hours. Add 3 ml of di-n-butyl phthalate, heat to 85 degrees, and keep constant temperature for 1 hour. Filter the mother liquor and wash it twice with 200 ml of toluene. Remove the filtrate, add 120 ml of toluene and 80 ml of titanium tetrachloride, treat at 110°C for 1 hour, remove the filtrate, and repeat the treatment once. After washing with 200 ml of hexane for 5 times, a solid olefin polymerization catalyst component is obtained. The average particle size D50 of the solid obtained in this embodiment is 21.5 μm, and the SPAN value is 0.86.
[0139] The propylene polymerization method is the same as in Example 1. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0140] Example 3
[0141] A Preparation of two-phase mixture
[0142] In a reactor that has been repeatedly replaced with high-purity nitrogen, 224 g of food-grade No. 100 white oil and 40.9 g of tributyl phosphate are added, then the temperature is lowered to 0°C, 234.3 g of titanium tetrachloride is added, and the mixture is stirred at 400 RMP to obtain a two-phase mixture.
[0143] B Preparation of magnesium solution
[0144] In another reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 160.5g of toluene, 9.5g of epichlorohydrin, 20.5g of tributyl phosphate, and 3g of 9,9-dimethoxymethylfluorene are added in sequence, and stirred at 400RMP for 2 hours at a temperature of 60°C. Then, a mixture of 5.7g of T602 diluted with 3.3g of phthalic anhydride and 27.8g of toluene is added, and the temperature is maintained at 60°C for another hour. Then the temperature is lowered to 0°C to prepare a magnesium-containing solution.
[0145] C Catalyst Component Preparation
[0146] Add the two-phase mixture prepared in step A to the magnesium-containing solution prepared in step B, maintain stirring at 400 RMP, and continue to maintain for 1 hour after the addition is completed. Gradually heat to 80°C within 4 hours and maintain for 1 hour. Filter the mother liquor. Hot wash with 200 ml of toluene twice, and remove the filtrate. Add 120 ml of toluene, 80 ml of titanium tetrachloride, treat at 110°C for 1 hour, remove the filtrate, and repeat the treatment once. After repeated washing with 200 ml of hexane for 5 times, a solid olefin polymerization catalyst component is obtained. The average particle size D50 of the solid obtained in this embodiment is 75.6 μm. Catalyst component data are shown in Table 1.
[0147] The propylene polymerization method is the same as in Example 1. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0148] Example 4
[0149] A Preparation of two-phase mixture
[0150] In a reactor that has been repeatedly replaced with high-purity nitrogen, 110.3 g of decane and 29.3 g of tributyl phosphate are added, then the temperature is lowered to 20° C., 258.9 g of titanium tetrachloride is added, and the mixture is stirred at 400 RMP to obtain a two-phase mixture.
[0151] B Preparation of magnesium solution
[0152] In another reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 73.6g of toluene, 10.7g of epichlorohydrin, and 20.5g of tributyl phosphate are added in sequence, and stirred at 300RMP for 2 hours at a temperature of 60°C. Then, a mixture of 5.7g of T602 diluted with 2.7g of phthalic anhydride and 17.3g of toluene is added, and the temperature is maintained at 60°C for another hour. Then the temperature is lowered to 20°C to prepare a magnesium-containing solution.
[0153] C Catalyst Component Preparation
[0154] Add the magnesium-containing solution prepared in step B to the two-phase mixture prepared in step A, maintain stirring at 400 RMP, and continue to maintain for 1 hour after the addition. Gradually heat to 80°C within 3 hours and maintain for 1 hour. Add 3 ml of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane during the heating process, heat to 80°C, and keep constant temperature for 1 hour. Filter the mother liquor. Hot wash with 200 ml of toluene twice, and remove the filtrate. Add 120 ml of toluene, 80 ml of titanium tetrachloride, treat at 110°C for 1 hour, remove the filtrate, and repeat the treatment once. After repeated washing with 200 ml of hexane 5 times, a solid olefin polymerization catalyst component is obtained. The average particle size D50 of the solid obtained in this embodiment is 6.6 μm. Catalyst component data is shown in Table 1.
[0155] The propylene polymerization method is the same as in Example 1. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0156] Example 5
[0157] A Preparation of two-phase mixture
[0158] The same preparation method as in Example 1;
[0159] B Preparation of magnesium solution
[0160] In another reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 180g of toluene, 6.3g of epichlorohydrin, 2.8g of ethanol, and 42.5g of tributyl phosphate are added in sequence, and stirred at 300RMP for 2 hours at a temperature of 60°C. Then, a mixture of 5.7g of T602 diluted with 2.7g of phthalic anhydride and 27.8g of toluene is added, and the temperature is maintained at 60°C for another hour. The temperature is lowered to 20°C to prepare a magnesium-containing solution.
[0161] C Catalyst Component Preparation
[0162] The preparation method is the same as that in Example 1; the average particle size D50 of the obtained olefin polymerization catalyst component solid is 51.6 μm.
[0163] The propylene polymerization method is the same as in Example 1. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0164] Comparative Example 1
[0165] The catalyst component was prepared by using the formulation of Example 1 and a preparation method similar to patents CN201280032149.7 and CN201580067255.2.
[0166] In a reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 180g of toluene, 10.7g of epichlorohydrin, and 71.8g of tributyl phosphate are added in sequence, and stirred at 300RMP for 2 hours at a temperature of 60°C. Then 2.7g of phthalic anhydride is added and maintained at 60°C for another hour. Cool down to 20°C, add a mixture of 210g of food-grade No. 100 white oil and 5.7g of T602 diluted with 27.8g of toluene, and stir at 400RMP for 1 hour. Drop 258.9g of titanium tetrachloride and continue to maintain for 1 hour after addition. Gradually heat to 80°C within 3 hours and maintain for 1 hour. Filter the mother liquor and wash it twice with 200ml of toluene. Remove the filtrate, add 200ml of toluene and 3ml of di-n-butyl phthalate, heat to 85 degrees, keep constant temperature for 1 hour, and remove the filtrate. Add 120 ml of toluene and 80 ml of titanium tetrachloride, treat at 110°C for 1 hour, remove the filtrate, and repeat the treatment once. After washing with 200 ml of hexane for 5 times, a solid olefin polymerization catalyst component is obtained. The average particle size D50 of the solid obtained in this comparative example is 67.3 μm, and the SPAN value is 0.93. The catalyst component data is shown in Table 1. The catalyst component picture is shown in Figure 2 .
[0167] The propylene polymerization method is the same as in Example 1. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0168] Table 1 Catalyst components and propylene polymerization performance
[0169]
[0170] In Table 1, BD represents polymer bulk density; II represents polymer isotacticity; MI represents polymer melt index; PP represents polypropylene; and Cat represents catalyst.
[0171] According to the above embodiments and comparative examples, in the preparation method described in the present invention, the precipitated catalyst spherical solid material has a more uniform particle shape, an adjustable average particle size, reduced catalyst agglomeration, and excellent catalyst performance, with high activity and stereospecific ability, and a high polymer bulk density.
[0172] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A method for preparing a catalyst component, wherein The following steps are involved: (1) mixing an organic phosphorus compound and a titanium-containing compound with an inert dispersion medium and optionally an aromatic hydrocarbon solvent to form a mixture M1 containing at least two liquid phases; (2) mixing a magnesium halide compound, a Lewis base and an organic solvent to form a magnesium-containing solution; (3) mixing the mixture M1, the magnesium-containing solution, optionally a Lewis acid, and optionally an inert dispersion medium to form a mixture M2; (4) heating the mixture M2 in the presence of a precipitation aid, a surfactant and optionally an internal electron donor compound to obtain a solid; and (5) optionally mixing the solid material and an internal electron donor compound to obtain the catalyst component; Wherein, an internal electron donor compound is present in the operation in step (4) and / or step (5).
2. The method for preparing the catalyst component according to claim 1, in, The organophosphorus compound is selected from one or more of the compounds represented by formula (I) and formula (II): Among them, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Each independently selected from a straight-chain alkyl group of 1 to 20 carbon atoms, a branched-chain alkyl group of 3 to 20 carbon atoms, a cycloalkane group of 3 to 20 carbon atoms, a halogenated hydrocarbon group of 1 to 20 carbon atoms, an aromatic hydrocarbon group of 6 to 20 carbon atoms, and an aromatic hydrocarbon group having a substituent; And / or, the general formula of the titanium-containing compound is as shown in formula (III): TiX m (OR a ) 4-m Formula (III) Where X is a halogen, R a is a hydrocarbon group of 1 to 20 carbon atoms, and m is an integer of 1 to 4; and / or, the inert dispersion medium is selected from one or more of silicone oil, kerosene, paraffin oil, white oil, vaseline oil, methyl silicone oil, aliphatic and cycloaliphatic hydrocarbons; And / or, the aromatic hydrocarbon solvent is selected from one or more of toluene, ethylbenzene, benzene, xylene and chlorobenzene; And / or, the magnesium halide compound has the general formula MgX 2 , wherein X is bromine, chlorine or iodine; and / or, the Lewis base is selected from one or more of an organic epoxy compound, an organic phosphorus compound and a hydroxyl-containing compound; Wherein, the organic epoxy compound is selected from one or more of the oxidation products of C2-C8 aliphatic olefins or C2-C8 halogenated aliphatic olefins; The general formula of the hydroxyl-containing compound is shown in formula (IV): HOR b Formula (IV) Where R b is a hydrocarbon group of 2 to 20 carbon atoms; Wherein, the hydrocarbon group is a saturated or unsaturated straight-chain or branched alkyl group, cycloalkyl group or aromatic hydrocarbon group; And / or, the organic solvent is an aromatic hydrocarbon or a halogenated hydrocarbon compound; And / or, the Lewis acid comprises one or more of a titanium-containing compound and a silicon-containing compound; Wherein, the general formula of the silicon-containing compound is as shown in formula (V): SiX 1 n R c 4-n Formula (V) Where X 1 is chlorine, bromine or iodine; R c is a hydrocarbon group having 1 to 20 carbon atoms; and n is an integer of 1 to 4.
3. The method for preparing the catalyst component according to claim 2, in, The organophosphorus compound is selected from one or more of trimethyl phosphate, triethyl phosphate, tributyl phosphate, tripentyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite and benzyl phosphite; And / or, the titanium-containing compound is one or more selected from titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxide, titanium tetraethoxide, titanium triethoxide monochloride, titanium diethoxide dichloride and titanium triethoxide monochloride; and / or, the inert dispersion medium is selected from one or more of white oil, hexane, heptane, octane, nonane, decane, dodecane and cyclohexane; And / or, the organic epoxy compound is one or more selected from ethylene oxide, propylene oxide, epichlorohydrin, epichlorohydrin, butylene oxide, butadiene oxide, butadiene dioxide, methyl glycidyl ether and diglycidyl ether; And / or, the hydroxyl-containing compound is selected from one or more of ethanol, propanol, butanol, 2-ethylhexanol, benzyl alcohol and phenylethyl alcohol; And / or, the organic solvent is selected from one or more of toluene, ethylbenzene, benzene, xylene and chlorobenzene; And / or, the silicon-containing compound is silicon tetrachloride.
4. The method for preparing the catalyst component according to claim 1, in, The precipitation aid is selected from one or more of acetic anhydride, phthalic anhydride, succinic anhydride, maleic anhydride, pyromellitic anhydride, acetic acid, propionic acid, butyric acid, acrylic acid, methacrylic acid, acetone, methyl ethyl ketone, benzophenone, methyl ether, ethyl ether, propyl ether, butyl ether and pentyl ether; And / or, the surfactant is selected from one or more of alcoholysis products of maleic anhydride polymers, alcoholysis products of maleic anhydride copolymers, (meth) alkyl acrylate polymers and (meth) alkyl acrylate copolymers; And / or, the internal electron donor compound is selected from one or more of esters, ethers, ketones, amines and silanes.
5. The method for preparing the catalyst component according to claim 4, in, The surfactant is selected from one or more of the group consisting of alcoholysis products of polymaleic anhydride, alcoholysis products of maleic anhydride-styrene copolymers, alcoholysis products of maleic anhydride-styrene-(meth)acrylate terpolymers, alcoholysis products of maleic anhydride-(meth)acrylate alkyl ester copolymers, poly(meth)acrylate alkyl esters, (meth)acrylate alkyl ester-maleic anhydride copolymers, and (meth)acrylate alkyl ester-maleic anhydride-styrene copolymers; And / or, the internal electron donor compound is selected from one or more of monovalent or polyvalent aliphatic carboxylic acid esters, aromatic carboxylic acid esters, diol ester compounds and diether compounds.
6. The method for preparing the catalyst component according to claim 5, in, The internal electron donor compound is selected from one or more of phthalates, malonates, succinates, glutarates, glycol esters, 1,3-diethers, pivalates and carbonates.
7. The method for preparing the catalyst component according to claim 6, in, The internal electron donor compound is selected from one or more of di-n-butyl phthalate, diisobutyl phthalate, 2,4-pentanediol dibenzoate, 3,5-heptanediol dibenzoate, diethyl 2,3-diisopropylsuccinate, diisobutyl 2,3-diisopropylsuccinate, di-n-butyl 2,3-diisopropylsuccinate, dimethyl 2,3-diisopropylsuccinate, diisobutyl 2,2-dimethylsuccinate, diisobutyl 2-ethyl-2-methylsuccinate, diethyl 2-ethyl-2-methylsuccinate, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
8. A method for preparing a catalyst component according to any one of claims 1 to 7, in, The mixing in step (1) is carried out under the following conditions: the mixing temperature is -20°C to 100°C; the mixing time is 0.01 to 10 hours; And / or, the mixing in step (2) is carried out under the following conditions: the mixing temperature is 10°C-150°C; the mixing time is 0.05-10 hours; And / or, the mixing in step (3) is carried out at -20°C to 60°C; And / or, the heating in step (4) is carried out under the following conditions: the mixture is heated to 20°C to 120°C and maintained for 0.1h to 24h after heating; the heating time is 1 minute to 36 hours.
9. A method for preparing a catalyst component according to any one of claims 1 to 7, in, Calculated per mole of magnesium halide, The organic phosphorus compound is 0.1 to 10 moles; and / or The titanium-containing compound is 0.5 to 25 moles; and / or The inert dispersion medium is 0.1 g to 300 g; and / or The aromatic hydrocarbon solvent is 0.1 to 40 moles; and / or The organic epoxy compound is 0.1 to 10 moles; and / or The hydroxyl-containing compound is 0.1 to 10 moles; and / or The organic solvent is 0.1 to 40 mol; and / or The silicon-containing compound is 0.5 to 25 moles; and / or The precipitation aid is 0.01 to 1 mol; and / or The internal electron donor is 0.01-1 mol; and / or The surfactant is present in an amount of 0.01 g to 5 g per gram of magnesium halide.
10. The method for preparing the catalyst component according to claim 9, in, Calculated per mole of magnesium halide, The organic phosphorus compound is 0.4 to 4 moles; and / or The titanium-containing compound is 1 to 20 moles; and / or The inert dispersion medium is 1 g to 150 g; and / or The aromatic hydrocarbon solvent is 0.1 to 30 moles; and / or The organic epoxy compound is 0.4 to 4 moles; and / or The hydroxyl-containing compound is 0.1 to 5 moles; and / or The organic solvent is 0.1 to 30 mol; and / or The silicon-containing compound is 0.5 to 20 moles; and / or The precipitation aid is 0.04 to 0.4 moles; and / or The surfactant is present in an amount of 0.05 g to 1 g per gram of magnesium halide.
11. A catalyst component obtained by the method for preparing a catalyst component according to any one of claims 1 to 10.
12. A catalyst system comprising the catalyst component according to claim 11, an alkyl aluminum compound and optionally an external electron donor compound.
13. The catalyst system according to claim 12, in, The general formula of the alkyl aluminum compound is AlR n X 3-n , wherein R is hydrogen or a hydrocarbon group having 1 to 20 carbon atoms; X is a halogen, and n is an integer of 1 to 3; And / or, the molar ratio of aluminum in the alkyl aluminum compound to titanium in the catalyst component is 5-5000:
1.
14. The catalyst system according to claim 13, in, The alkyl aluminum compound is one or more selected from trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, trioctylaluminum, diethyl aluminum monohydrogenate, diisobutyl aluminum monohydrogenate, diethyl aluminum monochloride, diisobutyl aluminum monochloride, sesquiethyl aluminum chloride and ethyl aluminum dichloride; And / or, the molar ratio of aluminum in the alkyl aluminum compound to titanium in the catalyst component is 20-800:
1.
15. The catalyst system according to any one of claims 12 to 14, in, The general formula of the external electron donor compound is R' n Si(OR y ) 4-n , wherein n is an integer of 0-3, and R' is selected from one or more of an alkyl group, a cycloalkyl group, an aryl group, a halogenated alkyl group, a halogen group and a hydrogen atom; R y One or more selected from alkyl, cycloalkyl, aryl and halogenated alkyl; And / or, the molar ratio of aluminum in the alkyl aluminum compound to the external electron donor compound is 0.1-500:
1.
16. The catalyst system according to claim 15, in, The external electron donor compound is selected from one or more of trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyltert-butyldimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, dicyclohexyldimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, methylcyclohexyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane; And / or, the molar ratio of aluminum in the alkyl aluminum compound to the external electron donor compound is 3-100:
1.
17. Use of the catalyst component according to claim 11 or the catalyst system according to any one of claims 12 to 16 in the field of olefin polymerization.