A method for synergistic oxidation leaching of low-grade tungsten-molybdenum ore
By using potassium permanganate oxidant to carry out collaborative oxidative leaching of tungsten ore and scheelite in an alkaline environment, the problem of difficulty in recovering low-grade tungsten and molybdenum ores is solved, and the leaching rate and recovery efficiency of tungsten and molybdenum are improved. It is suitable for For the processing of low-grade tungsten and molybdenum ores.
Patent Information
- Application Number
- CN202310093344.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-10
AI Technical Summary
Existing technology is difficult to effectively process low-grade tungsten and molybdenum ores that are difficult to float, resulting in a low recovery rate of tungsten and molybdenum resources, and the traditional smelting process has limited applicability to low-grade minerals.
Using the collaborative oxidation leaching method of low-grade tungsten-molybdenum ore, the tungsten-molybdenum ore and scheelite are reacted with alkali to form WO42- and MoO42- with good water solubility, and potassium permanganate is used as the oxidant, in sodium carbonate and carbonic acid. Mechanical stirring and leaching are carried out in the mixed alkali system of sodium hydrogen to improve the oxidation efficiency and leaching rate.
It realizes the one-step leaching of low-grade tungsten and molybdenum ores, simplifies the treatment process, improves the leaching rate and recovery efficiency of tungsten and molybdenum, and is suitable for the processing of low-grade tungsten and molybdenum ores.
Smart Images

Figure CN116043038B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore. Background Art
[0002] The mining and utilization of molybdenum is mainly based on primary ore, among which molybdenite is the main one. With the exploitation of resources, molybdenite resources are gradually reduced, and low-grade molybdenite has gradually become the object of mining. Molybdenite and scheelite often coexist to form tungsten-molybdenum ore. Some molybdenite ores in the shallow surface are easily oxidized and easily form isomorphous minerals (molybdenum-tungsten-calcium ore) with scheelite. Tungsten-molybdenum ores with high calcium, high magnesium, high iron, high fluorite, low tungsten and molybdenum are difficult to process. The concentrate grade and recovery rate obtained by flotation method are low, and it is still difficult to develop and utilize these tungsten-molybdenum ores.
[0003] For low-grade and difficult-to-process tungsten-molybdenum ores, the current technology is basically to select first and then smelt. In the process of ore dressing, there is also a method for recovering scheelite / molybdenum oxide ore from molybdenum sulfide flotation tailings through ore dressing (CN201110389747.7), which discloses that the treated pulp is re-selected and / or deslimed by flotation using molybdenum sulfide flotation tailings as raw materials; adding a regulator, auxiliary inhibitor, inhibitor and modified fatty acid collector to the floating sulfur tailings slurry, flotation recovery of scheelite / molybdenum oxide ore at room temperature, and after roughing, scavenging and concentrating, scheelite / molybdenum oxide concentrate is obtained. After fine grinding-desliming-scheelite / molybdenum oxide ore flotation, after one primary selection, two scavenging and two concentrating, a scheelite / molybdenum oxide concentrate with a grade of WO37.49% and Mo3.80% is obtained, WO3+Mo>10%, and the recovery rate of WO365.80% and Mo67.15%. It is difficult to separate and enrich low-grade and difficult-to-process tungsten-molybdenum ore using only physical beneficiation technology, and it is difficult to obtain an ideal tungsten-molybdenum grade and recovery rate.
[0004] In the process of smelting, there is smelting by wet method. A combined smelting process of molybdenum ore and tungsten ore (CN202011630584.2) discloses a combined smelting process of molybdenum concentrate and scheelite. The molybdenum concentrate is leached by oxygen pressure boiling with a molybdenum ore leaching agent, and the molybdenum ore filtrate is filtered to obtain the molybdenum ore raffinate; the molybdenum ore raffinate is used as a tungsten ore leaching agent for the atmospheric leaching of scheelite. The process contains only molybdenum concentrate, with a molybdenum content of 40% to 50%; the tungsten-containing mineral is only scheelite, with a tungsten trioxide content of 40%. The leaching of molybdenum concentrate adopts oxygen pressure boiling leaching with the addition of an auxiliary agent, and finally the extract of the molybdenum concentrate is used to leach scheelite. This method has relatively high requirements for the content of the original ore, and it is difficult to apply to lower-grade molybdenum concentrate, scheelite, molybdenum-tungsten-calcium ore, and mixed ores of the above-mentioned ores.
[0005] Therefore, in the current situation where molybdenum resources are relatively tight, how to recover tungsten and molybdenum from low-grade and difficult-to-float tungsten-molybdenum ores is particularly critical. Summary of the invention
[0006] The purpose of the present invention is to provide a method for the coordinated oxidation leaching of low-grade tungsten-molybdenum ore, which utilizes the fact that molybdenite in the ore is easily oxidized, and that molybdenite and scheelite have strong alkali reaction activity to form WO4 with good water solubility. 2- and MoO4 2- The characteristics of molybdenite are as follows: molybdenite is oxidized and then leached by mixed alkaline method with molybdenite and scheelite.
[0007] The low-grade refractory tungsten-molybdenum ore oxidation coordinated mixed alkaline leaching method of the present invention comprises the following steps:
[0008] (1) The tungsten-molybdenum ore is crushed, coarsely ground, screened and finely ground to a particle size of -200 mesh (-0.075 mm) ≥ 90% to obtain raw material fine-grained tungsten-molybdenum ore.
[0009] (2) Place fine-grained tungsten-molybdenum ore in a reaction kettle, add Na2CO3 solution, NaHCO3 solution, and KMnO4 oxidant in sequence, control the liquid-to-solid ratio to 2-8, and the solution pH value to 9-11; stir at a stirring rate of 200-400 rpm, a reaction time of 1-5 h, and a reaction temperature of 70-90°C.
[0010] (3) After stopping the reaction, filtering is performed directly, and the filter residue is washed with a mixed alkaline solution of Na2CO3 and NaHCO3 of the same concentration as in the above step (2) after being heated to the same temperature as in the above step (2), and then the filter residue is washed with distilled water at the same temperature as Na2CO3 and NaHCO3 to obtain leaching residue and leachate.
[0011] In the above step (1), the tungsten-containing minerals in the tungsten-molybdenum ore are molybdenite and scheelite, with contents of 0.05-0.30% and 0.05-0.30% respectively; the molybdenum-containing minerals are molybdenite and molybdenite, with contents of 0.05-0.30% and 0.05-0.30% respectively; after grinding treatment, the molybdenum grade in the tungsten-molybdenum ore is 0.10-0.50%, the tungsten grade is 0.05-0.50%, the calcium grade is 20-30%, the magnesium grade is 8-12%, the iron grade is 3-5%, and the fluorine grade is 3.5-5.5%.
[0012] In the above step (1), 50-70% of the molybdenite in the tungsten-molybdenum ore has a dissociation degree of more than 60%; and 70-90% of the molybdenite has a dissociation degree of more than 60%.
[0013] In the above step (1), 55-75% of the molybdenite in the tungsten-molybdenum ore is distributed between 10 and 23 μm, and more than 80% of the molybdenite is distributed below 10 μm.
[0014] The ore grinding in the above step (1) is performed by fine grinding using an oscillating sample preparation machine, and the sample preparation time is 1 to 5 minutes.
[0015] In the above step (2), the amount of Na2CO3 used is 40-100kg / t tungsten-molybdenum ore, the amount of NaHCO3 used is 6-15kg / t tungsten-molybdenum ore, and the amount of KMnO4 used is 2.5-12.5kg / t tungsten-molybdenum ore.
[0016] In the above step (2), the concentration of Na2CO3 is 40-100 g / L, and the concentration of NaHCO3 is 6-15 g / L.
[0017] In the above step (3), the solid-liquid separation method is vacuum filtration using a vacuum filter. The amount of the mixed alkaline solution used to wash the filter residue is 50-100 ml, and the amount of the distilled water used to wash the filter residue is 50-100 ml;
[0018] In the above step (3), the leached residue after filtering and washing is dried in a vacuum drying oven at a drying temperature of 60 to 80° C. until constant weight is achieved.
[0019] ICP-OES was used to analyze the contents of molybdenum and tungsten in fine-grained tungsten-molybdenum ore, leaching slag and leaching solution. The contents of molybdenum and tungsten in fine-grained tungsten-molybdenum ore and leaching slag were calculated as Mo and WO3, respectively, and the contents of molybdenum and tungsten in leaching solution were calculated as Mo and W, respectively. The leaching rate was calculated based on the contents of molybdenum and tungsten in the leaching solution.
[0020] Compared with the prior art, the low-grade tungsten-molybdenum ore collaborative oxidation leaching method of the present invention has the following beneficial effects:
[0021] The low-grade tungsten-molybdenum ore collaborative oxidation leaching method of the present invention can process low-grade tungsten-molybdenum ores that cannot be ore-selected, and solves the problem that such ores cannot be utilized. The method of the present invention changes the traditional technical route of first selecting and then smelting tungsten-molybdenum ores, oxidizes the unoxidized molybdenite in the ore and leaches it in a mixed alkali system with scheelite and molybdenum-tungsten calcium, so as to achieve one-step leaching of tungsten and molybdenum in low-grade tungsten-molybdenum ores, and simplifies the processing flow; adopts the use of strongly oxidized potassium permanganate as the oxidant of molybdenite to improve the oxidation efficiency, and uses sodium carbonate and sodium bicarbonate as mixed alkalis for leaching to improve the leaching rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a schematic diagram of a method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore in an embodiment of the present invention. DETAILED DESCRIPTION
[0023] In the present invention, the ore is crushed, roughly ground, screened and finely ground. The particle size of fine tungsten-molybdenum ore is -200 mesh ≥ 90%. The molybdenum grade is 0.10-0.50%; the tungsten grade is 0.05-0.50%.
[0024] The tungsten-containing minerals in tungsten-molybdenum ore are molybdenite and scheelite, with mass contents of 0.05-0.30% and 0.05-0.30% respectively; the molybdenum-containing minerals are molybdenite and molybdenite, with mass contents of 0.05-0.30% and 0.05-0.30% respectively.
[0025] In the examples of the present invention, leaching is carried out under normal pressure, and mechanical stirring is used for stirring.
[0026] In the examples of the present invention, the fine-grained tungsten-molybdenum ore is added as a solid sample, Na2CO3 and NaHCO3 are added as reagent liquids prepared to a concentration, and KMnO4 is added in batches multiple times, all at room temperature.
[0027] The order of adding materials is to add Na2CO3 solution first, then add NaHCO3 solution, and finally add KMnO4 solid in batches.
[0028] After the reaction is completed, hot filtration is performed in time. The leached residue is washed with a mixed leaching solution of Na2CO3 and NaHCO3 of the same concentration and temperature as mentioned above, and then washed with distilled water of the same temperature.
[0029] The leached residue after filtering and washing is dried in a vacuum drying oven at a drying temperature of 60-80°C until constant weight is achieved.
[0030] ICP-OES was used to analyze the contents of molybdenum and tungsten in the leaching solution and the leaching residue, and the leaching rates of tungsten and molybdenum were calculated based on the contents of molybdenum and tungsten in the leaching solution.
[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0032] Example 1
[0033] Process such as Figure 1 As shown; the tungsten-molybdenum ore is crushed-coarsely ground-screened-finely ground to a particle size of -200 mesh (-0.075mm) ≥ 90% to make fine-grained tungsten-molybdenum ore; the molybdenum grade is 0.10%, the tungsten grade is 0.42%, the calcium grade is 28.84%, the magnesium grade is 11.22%, the iron grade is 4.51%, and the fluorine grade is 3.65%.
[0034] 20g of fine tungsten-molybdenum ore was placed in a reactor, stirring was started, the stirring rate was adjusted to 250rpm, 20ml of Na2CO3 solution (concentration 100g / L) and 20ml of NaHCO3 (concentration 12g / L) were added in sequence, 0.25g of KMnO4 solid was slowly added in batches, and distilled water was added at the same time, the liquid-solid ratio was 2, 4, 6, and 8 respectively, and the temperature was raised to control the reaction temperature at 90℃ and the reaction time at 3h;
[0035] After stopping the reaction, vacuum filter while hot, wash the filter residue with 50 ml of mixed alkali solution of the same concentration and temperature as the reaction system, and then wash with 50 ml of distilled solution at the same temperature.
[0036] The leached residue after filtering and washing is dried in a vacuum drying oven at a drying temperature of 80°C until constant weight is achieved.
[0037] ICP-OES was used to analyze the contents of molybdenum and tungsten in the leachate and the leaching residue, and the leaching rates of tungsten and molybdenum were calculated based on the contents of molybdenum and tungsten in the leachate. This embodiment investigates the effect of liquid-solid ratio on the leaching rates of tungsten and molybdenum in tungsten-molybdenum ore. The test data are shown in Table 1. The optimal liquid-solid ratio is 6, at which the leaching rate of Mo is as high as 83.23%, and the leaching rate of W is 45.87%.
[0038] Example 2
[0039] The tungsten-molybdenum ore is crushed, coarsely ground, screened and finely ground to a particle size of -200 mesh (-0.075mm) ≥ 90% to make fine-grained tungsten-molybdenum ore; the molybdenum grade is 0.15%, the tungsten grade is 0.50%, the calcium grade is 24.34%, the magnesium grade is 11.63%, the iron grade is 4.09%, and the fluorine grade is 3.50%.
[0040] Place 20g fine-grained tungsten-molybdenum ore in a reactor, start stirring, adjust the stirring rate to 250rpm, add 20ml Na2CO3 solution (concentrations are 40g / L, 60g / L, 80g / L, 100g / L), 20ml NaHCO3 (concentration 12g / L) in sequence, slowly add 0.25g KMnO4 solid in batches, and add 80ml distilled water at the same time, with a liquid-to-solid ratio of 6, heat and raise the temperature, control the reaction temperature to 90℃, and the reaction time to 3h;
[0041] After stopping the reaction, vacuum filter while hot, wash the filter residue with 100 ml of mixed alkali solution of the same concentration and temperature as the reaction system, and then wash with 50 ml of distilled solution at the same temperature.
[0042] The leached residue after filtering and washing is dried in a vacuum drying oven at a drying temperature of 80°C until constant weight is achieved.
[0043] ICP-OES was used to analyze the content of molybdenum and tungsten in the leachate and the leaching residue, and the leaching rate of tungsten and molybdenum was calculated based on the content of molybdenum and tungsten in the leachate. This embodiment investigated the effect of the addition of Na2CO3 on the leaching rate of tungsten and molybdenum in tungsten-molybdenum ore. The test data are shown in Table 1. The best 20mlNa2CO3 (concentration 80g / L) is based on the original ore. The best Na2CO3 dosage is 80kg / t ore. At this time, the leaching rate of Mo is as high as 84.5%, and the leaching rate of W is 47.59%.
[0044] Example 3
[0045] The tungsten-molybdenum ore is crushed, coarsely ground, screened and finely ground to a particle size of -200 mesh (-0.075mm, accounting for ≥90%) to make fine-grained tungsten-molybdenum ore; the molybdenum grade is 0.22%, the tungsten grade is 0.38%, the calcium grade is 20.36%, the magnesium grade is 8.00%, the iron grade is 4.22%, and the fluorine grade is 4.37%.
[0046] Place 20g of fine-grained tungsten-molybdenum ore in a reactor, start stirring, adjust the stirring rate to 250rpm, add 20ml of Na2CO3 solution (concentration 80g / L), 20ml of NaHCO3 (concentration 6g / L, 9g / L, 12g / L, 15g / L) in sequence, slowly add 0.25g of KMnO4 solid in batches, and add 80ml of distilled water at the same time, with a liquid-to-solid ratio of 6, heat and raise the temperature, control the reaction temperature to 90℃, and the reaction time to 3h;
[0047] After stopping the reaction, vacuum filter while hot, wash the filter residue with 75 ml of mixed alkali solution of the same concentration and temperature as the reaction system, and then wash with 75 ml of distilled solution at the same temperature.
[0048] The leached residue after filtering and washing is dried in a vacuum drying oven at a drying temperature of 80°C until constant weight is achieved.
[0049] ICP-OES was used to analyze the contents of molybdenum and tungsten in the leachate and the leaching residue, and the leaching rates of tungsten and molybdenum were calculated based on the contents of molybdenum and tungsten in the leachate. The present embodiment investigated the influence of NaHCO3 addition on the leaching rates of tungsten and molybdenum in tungsten-molybdenum ore. The test data are shown in Table 1, with an optimum of 20 ml NaHCO3 (concentration 9 g / L), and an optimum NaHCO3 dosage of 9 kg / t ore based on the raw ore. At this time, the leaching rate of Mo was as high as 85.00%, and the leaching rate of W was 48.59%.
[0050] Example 4
[0051] The tungsten-molybdenum ore is crushed, coarsely ground, screened and finely ground to a particle size of -200 mesh (-0.075mm, accounting for ≥90%) to make fine-grained tungsten-molybdenum ore; the molybdenum grade is 0.30%, the tungsten grade is 0.35%, the calcium grade is 25.86%, the magnesium grade is 12.00%, the iron grade is 3.00%, and the fluorine grade is 4.91%.
[0052] 20g of fine-grained tungsten-molybdenum ore was placed in a reactor, stirring was started, the stirring rate was adjusted to 250rpm, 20ml of Na2CO3 solution (concentration 80g / L) and 20ml of NaHCO3 (concentration 9g / L) were added in sequence, 0.05g, 0.1g, 0.15g, 0.2g and 0.25g of KMnO4 solid were slowly added in batches, and 80ml of distilled water was added at the same time, with a liquid-to-solid ratio of 6, and the temperature was raised to 90℃ and the reaction time was 3h;
[0053] After stopping the reaction, vacuum filter while hot, wash the residue with 50 ml of mixed alkali solution of the same concentration and temperature as the reaction system, and then wash with 100 ml of distilled solution at the same temperature;
[0054] The leached residue after filtering and washing is dried in a vacuum drying oven at 80°C until constant weight;
[0055] ICP-OES was used to analyze the contents of molybdenum and tungsten in the leachate and the leaching residue, and the leaching rates of tungsten and molybdenum were calculated based on the contents of molybdenum and tungsten in the leachate. This embodiment investigates the effect of KMnO4 solid addition on the leaching rates of tungsten and molybdenum in tungsten-molybdenum ore. The test data are shown in Table 1. The optimal KMnO4 solid addition amount is 0.2g. The optimal KMnO4 dosage is 10kg / t ore based on the original ore. At this time, the highest leaching rate of Mo is 86.22%, and the leaching rate of W is 49.37%.
[0056] Example 5
[0057] The tungsten-molybdenum ore is crushed, coarsely ground, screened and finely ground to a particle size of -200 mesh (-0.075mm accounts for ≥90%) to make fine-grained tungsten-molybdenum ore; the molybdenum grade is 0.43%, the tungsten grade is 0.05%, the calcium grade is 27.44%, the magnesium grade is 8.89%, the iron grade is 5.0%, and the fluorine grade is 4.50%;
[0058] 20g of fine-grained tungsten-molybdenum ore was placed in a reactor, stirring was started, the stirring rate was adjusted to 250rpm, 20ml of Na2CO3 solution (concentration 80g / L) and 20ml of NaHCO3 (concentration 9g / L) were added in sequence, 0.2g of KMnO4 solid was slowly added in batches, and 80ml of distilled water was added at the same time, the liquid-solid ratio was 6, the temperature was raised, the reaction temperature was controlled at 90℃, and the reaction time was controlled at 1h, 2h, 3h, 4h, and 5h respectively;
[0059] After stopping the reaction, vacuum filter while hot, wash the residue with 100 ml of mixed alkali solution of the same concentration and temperature as the reaction system, and then wash with 50 ml of distilled solution at the same temperature;
[0060] The leached residue after filtering and washing is dried in a vacuum drying oven at 80°C until constant weight;
[0061] ICP-OES was used to analyze the contents of molybdenum and tungsten in the leachate and the leaching residue, and the leaching rates of tungsten and molybdenum were calculated based on the contents of molybdenum and tungsten in the leachate. This embodiment investigates the effect of reaction time on the leaching rates of tungsten and molybdenum in tungsten-molybdenum ore. The test data are shown in Table 1. The optimal reaction time is 4h, at which time the highest leaching rate of Mo is 87.11%, and the leaching rate of W is 50.05%.
[0062] Example 6
[0063] The tungsten-molybdenum ore is crushed, roughly ground, screened and finely ground to a particle size of -200 mesh (-0.075mm accounts for ≥90%) to make fine-grained tungsten-molybdenum ore; molybdenum grade 0.50%, tungsten grade 0.35%, calcium grade 21.52%, magnesium grade 9.93%, iron grade 4.2%, fluorine grade 5.5%;
[0064] 20g of fine-grained tungsten-molybdenum ore was placed in a reactor, stirring was started, the stirring rate was adjusted to 250rpm, 20ml of Na2CO3 solution (concentration 80g / L) and 20ml of NaHCO3 (concentration 9g / L) were added in sequence, 0.2g of KMnO4 solid was slowly added in batches, and 80ml of distilled water was added at the same time, the liquid-solid ratio was 6, and the temperature was heated to control the reaction temperature to 70℃, 75℃, 80℃, 85℃, and 90℃, respectively, and the reaction time was controlled to 4h;
[0065] After stopping the reaction, vacuum filter while hot, wash the residue with 100 ml of mixed alkali solution of the same concentration and temperature as the reaction system, and then wash with 100 ml of distilled solution at the same temperature;
[0066] The leached residue after filtering and washing is dried in a vacuum drying oven at 80°C until constant weight;
[0067] ICP-OES was used to analyze the contents of molybdenum and tungsten in the leachate and the leaching residue, and the leaching rates of tungsten and molybdenum were calculated based on the contents of molybdenum and tungsten in the leachate. This embodiment investigates the effect of reaction temperature on the leaching rates of tungsten and molybdenum in tungsten-molybdenum ore. The test data are shown in Table 1. The optimal reaction temperature is 85°C, the leaching rate of Mo is the highest at 87.15%, and the leaching rate of W is 51.59%.
[0068] Example 7
[0069] The tungsten-molybdenum ore is crushed, coarsely ground, screened and finely ground to a particle size of -200 mesh (-0.075mm accounts for ≥90%) to make fine-grained tungsten-molybdenum ore; molybdenum grade 0.30%, tungsten grade 0.35%, calcium grade 26%, magnesium grade 9%, iron grade 4.4%, fluorine grade 5.2%;
[0070] 20g of fine-grained tungsten-molybdenum ore was placed in a reactor, stirring was started, the stirring rate was adjusted to 250rpm, 20ml of Na2CO3 solution (concentration 80g / L), 20ml of NaHCO3 (concentration 9g / L) were added in sequence, 0.2g of KMnO4 solid was slowly added in batches, and 80ml of distilled water was added at the same time, the liquid-solid ratio was 6, the temperature was raised, the reaction temperature was controlled to 85℃, and the reaction time was controlled to 4h;
[0071] After stopping the reaction, vacuum filter while hot, wash the residue with 100 ml of mixed alkali solution of the same concentration and temperature as the reaction system, and then wash with 100 ml of distilled solution at the same temperature;
[0072] The leached residue after filtering and washing is dried in a vacuum drying oven at 80°C until constant weight;
[0073] ICP-OES was used to analyze the contents of molybdenum and tungsten in the leaching solution and the leaching residue. The leaching rates of tungsten and molybdenum were calculated based on the contents of molybdenum and tungsten in the leaching solution. The leaching rates of tungsten and molybdenum were investigated under the optimal conditions of the influencing factors. Under the optimal reaction conditions, the leaching rate of Mo was as high as 87.79%, and the leaching rate of W was 51.87%.
[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention.
[0075] Table 1
[0076]
Claims
1. A method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore, characterized in that: The following steps are involved: (1) crushing, coarse grinding, screening and fine grinding of tungsten and molybdenum ore to a particle size of -200 mesh (-0.075 mm) ≥ 90% to obtain raw material fine-grained tungsten and molybdenum ore; (2) Place fine-grained tungsten-molybdenum ore in a reaction kettle, add Na2CO3 solution, NaHCO3 solution, and KMnO4 oxidant in sequence, heat and stir; (3) After stopping the reaction, filtering is performed directly, and the filter residue is first washed with a mixed alkaline solution of Na2CO3 and NaHCO3 at the same concentration and temperature as the reaction system in step (2), and then the filter residue is washed with distilled water at the same temperature as the reaction system in step (2) to obtain leaching residue and leachate; The low-grade tungsten-molybdenum ore is a high-calcium, high-magnesium, high-iron, high-fluorite, low-tungsten-molybdenum refractory tungsten-molybdenum ore. The molybdenite in the ore is partially oxidized to form an isomorphous mineral molybdenum-tungsten-calcium ore with scheelite, and the fluorite grade is 8% to 12%; the non-metallic minerals are mainly pyroxene, olivine, dolomite, and calcite; the tungsten-containing minerals in the tungsten-molybdenum ore are molybdenum-tungsten-calcium ore and scheelite, with mass contents of 0.05 to 0.30% and 0.05 to 0.30% respectively; the molybdenum-containing minerals are molybdenum-tungsten-calcium ore and molybdenite, with mass contents of 0.05 to 0.30% and 0.05 to 0.30% respectively; In the step (2), the amount of Na2CO3 used is 40-100 kg / t of tungsten-molybdenum ore, the amount of NaHCO3 used is 6-15 kg / t of tungsten-molybdenum ore, and the amount of KMnO4 used is 2.5-12.5 kg / t of tungsten-molybdenum ore; In the step (2), the concentration of Na2CO3 is 40-100 g / L, and the concentration of NaHCO3 is 6-15 g / L; the liquid-to-solid ratio is controlled at 2-8, and the pH value is controlled at 9-11.
2. A method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore according to claim 1, characterized in that: In the step (1), after the grinding treatment, the molybdenum grade of the tungsten-molybdenum ore is 0.10-0.50%, the tungsten grade is 0.05-0.50%, the calcium grade is 20-30%, the magnesium grade is 8-12%, the iron grade is 3-5%, and the fluorine grade is 3.5-5.5%.
3. A method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore according to claim 1, characterized in that: In the step (1), 50-70% of the molybdenite in the tungsten-molybdenum ore has a dissociation degree of more than 60%; and 70-90% of the molybdenite has a dissociation degree of more than 60%.
4. A method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore according to claim 1, characterized in that: In the step (1), 55-75% of the molybdenite in the tungsten-molybdenum ore is distributed between 10 and 23 μm, and more than 80% of the molybdenite is distributed below 10 μm.
5. The method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore according to claim 1, characterized in that: In the step (1), the ore is ground by fine grinding using an oscillating sample preparation machine, and the sample preparation time is 1 to 5 minutes.
6. A method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore according to claim 1, characterized in that: The stirring in step (2) is specifically performed at a stirring rate of 200-400 rpm, a reaction time of 1-5 h, and a reaction temperature of 70-90°C.
7. The method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore according to claim 1, characterized in that: The filtration in step (3) is specifically carried out by using a vacuum filter; the amount of the mixed alkaline solution used to wash the filter residue is 50-100 mL, and the amount of distilled water used to wash the filter residue is 50-100 mL; the leached residue after filtration and washing is dried in a vacuum drying oven at a drying temperature of 60-80°C until constant weight.
8. The method for collaborative oxidation leaching of low-grade tungsten-molybdenum ore according to claim 1, characterized in that: ICP-OES was used to analyze the contents of molybdenum and tungsten in fine-grained tungsten-molybdenum ore, leaching slag and leaching solution. The molybdenum and tungsten in fine-grained tungsten-molybdenum ore and leaching slag were measured as Mo and WO3, respectively. The molybdenum and tungsten in the leaching solution were measured as Mo and W, respectively. The leaching rate was calculated based on the molybdenum and tungsten contents in the leaching solution.
Citation Information
Patent Citations
Mineral processing method for recycling scheelite / molybdenum oxide ores from molybdenum sulfide flotation tailings
CN102489407A
Combined smelting process of molybdenum ore and tungsten ore
CN114686704A
Methods for processing tungsten-molybdenum symbiotic mixed ores to produce tungsten-molybdenum products
CN102296179A