Catalyst for preparing phthalic anhydride by oxidation of o-xylene, and method for preparing phthalic anhydride by oxidation of o-xylene

By optimizing the catalyst bed structure, the catalytic efficiency in the oxidation process is improved, the problem of low efficiency of the catalyst bed is solved, and the production of phthalic anhydride with high conversion and high yield is achieved.

CN116060064BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111284068.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-01
Publication Date
2024-12-06
Estimated Expiration
2041-11-01

AI Technical Summary

Technical Problem

In the prior art, the catalytic efficiency of the oxidized phthalic anhydride catalyst bed is low, resulting in insufficient yield of phthalic anhydride and limited feeding amount of raw materials, making it impossible to effectively optimize the catalyst action of each bed.

Method used

Design a catalyst, including 3 catalyst beds arranged in sequence, the weight ratio of each bed is 8-20:100, and the Sn decreases in sequence and Pn increases in sequence, by optimizing the catalyst bed. The layer structure avoids deep oxidation of the product and improves the reaction load and selectivity of the catalytic medium.

Benefits of technology

The conversion rate of orthoxylene and the yield of phthalic anhydride were significantly improved, with a conversion rate of 99.95%, a yield of 115.2%, and the generation of impurities or overoxidation was reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0003332330040000041
    Figure BDA0003332330040000041
  • Figure BDA0003332330040000111
    Figure BDA0003332330040000111
Patent Text Reader

Abstract

The present invention relates to the technical field of preparing phthalic anhydride from o-xylene, and in particular, to a catalyst for preparing phthalic anhydride from o-xylene by oxidation, and a method for preparing phthalic anhydride from o-xylene by oxidation. The catalyst comprises at least three catalyst beds arranged in sequence, and the weight ratio of the active component to the carrier in the catalytic medium filled in each catalyst bed is 8-20:100; wherein, in the catalyst, along the logistics direction, the S n The P of each catalyst bed decreases in sequence. n Increasing in sequence, S n is the total surface area of ​​the carrier per unit volume of the nth catalyst bed along the direction of the flow, P n is the surface area of ​​a single carrier of the nth catalyst bed along the direction of the flow, and n is a positive integer. The catalyst provided by the present invention is used in the method for oxidizing o-xylene to prepare phthalic anhydride, which can effectively improve the conversion rate of o-xylene and the yield of phthalic anhydride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparing phthalic anhydride from o-xylene, and in particular to a catalyst for preparing phthalic anhydride from o-xylene by oxidation, and a method for preparing phthalic anhydride from o-xylene by oxidation. Background Art

[0002] Phthalic anhydride (PA) is an important organic chemical raw material, and is considered one of the top ten organic chemical raw materials. As an intermediate, PA is mainly used in the production of plasticizers, alkyd resins and unsaturated polyester resins (UPR). There are two methods for producing phthalic anhydride: oxidation method and o-xylene oxidation method. One is to use naphthalene or o-naphthalene mixture as raw materials, and then oxidize it through air catalysis, which is referred to as naphthalene method phthalic anhydride; the other is to use o-xylene as raw material, and then oxidize it through air under the action of vanadium catalyst to phthalic anhydride, which is referred to as o-phthalic anhydride.

[0003] At present, the patents for the production of phthalic anhydride by oxidation mainly focus on the selection of additives and the optimization of formulations. BASF has disclosed a gas phase oxidation method, in which a gas stream including at least one hydrocarbon and molecular oxygen is passed through a catalyst produced by using antimony trioxide containing a significant proportion of antimony fluoride. However, this method fails to specifically optimize the role played by each bed layer, and the catalytic efficiency needs to be improved.

[0004] Southern Chemical Co., Ltd. has developed a multi-layer catalyst for preparing phthalic anhydride, which uses a catalyst arrangement having a first catalyst layer on the gas inlet side and at least one second catalyst layer with different catalytic activity downstream of the first catalyst layer in the gas flow direction. However, this method has the problem that the catalytic efficiency of the catalyst has reached a bottleneck and is not enough to improve the weight yield of the phthalic anhydride product.

[0005] The imported phthalic anhydride catalysts used in China mainly come from BASF and Southern Chemical Company. The catalysts are divided into 3-6 stages, and the feed rate of raw materials is 90-100g / Nm 3 , the pure yield of phthalic anhydride is 113-114% in the first year. However, this method has the problem of failing to optimize the catalytic efficiency of each bed catalyst and limiting the amount of raw material feed. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of low catalytic efficiency of the catalyst in the catalyst bed and low phthalic anhydride yield in the prior art, and to provide a catalyst for preparing phthalic anhydride by oxidizing o-xylene and a method for preparing phthalic anhydride by oxidizing o-xylene. When the catalyst is used for preparing phthalic anhydride by oxidizing o-xylene, the selectivity of the catalytic medium in the catalyst bed is effectively improved, thereby improving the o-xylene conversion rate and the phthalic anhydride yield.

[0007] In order to achieve the above object, the first aspect of the present invention provides a catalyst for preparing phthalic anhydride by oxidation of o-xylene, the catalyst comprising up to 3 catalyst beds arranged in sequence, the weight ratio of active components to carriers in the catalytic medium filled in each catalyst bed being 8-20:100;

[0008] In the catalyst, along the flow direction, the S of each catalyst bed n The P of each catalyst bed decreases in sequence. n Increasing successively, among which, S n is the total surface area of ​​the carrier per unit volume of the nth catalyst bed along the direction of the flow, P n is the surface area of ​​a single carrier in the nth catalyst bed along the direction of the flow, where n is a positive integer;

[0009] The total surface area of ​​the carriers per unit volume is defined as the total number of carriers per 100 mL volume in a cylindrical container with a diameter of 29 mm × the surface area of ​​a single carrier;

[0010] The surface area of ​​a single carrier is defined as the surface area of ​​the carrier of the catalytic medium loaded in the nth catalyst bed.

[0011] The second aspect of the present invention provides a method for preparing phthalic anhydride by oxidation of o-xylene, which comprises: introducing o-xylene and an oxygen-containing gas into the catalyst provided in the first aspect, and sequentially contacting and reacting with the catalytic medium in each catalyst bed.

[0012] Compared with the prior art, the present invention has the following advantages:

[0013] (1) The catalyst provided by the present invention is characterized by limiting the S of each catalyst bed n and P n Change rule, that is, along the flow direction, the S of each catalyst bed n The P of each catalyst bed decreases in sequence. n Increasing successively, especially further limiting S n and P n Satisfying the relationship of formula (1), by optimizing the catalyst bed, deep oxidation of the product can be avoided, thereby improving the reaction load, selectivity and catalytic performance of the catalytic medium;

[0014] (2) The catalyst provided by the present invention is used in the method for oxidizing o-xylene to prepare phthalic anhydride, which can effectively improve the conversion rate of o-xylene and the yield of phthalic anhydride, that is, the conversion rate of o-xylene is as high as 99.95%, and the yield of phthalic anhydride is as high as 115.2%. DETAILED DESCRIPTION

[0015] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0016] The first aspect of the present invention provides a catalyst for preparing phthalic anhydride by oxidation of o-xylene, the catalyst comprising at least three catalyst beds arranged in sequence, the weight ratio of active components to carriers in the catalytic medium filled in each catalyst bed being 8-20:100;

[0017] In the catalyst, along the flow direction, the S of each catalyst bed n The P of each catalyst bed decreases in sequence. n Increasing successively, among which, S n is the total surface area of ​​the carrier per unit volume of the nth catalyst bed along the direction of the flow, P n is the surface area of ​​a single carrier in the nth catalyst bed along the direction of the flow, where n is a positive integer;

[0018] The total surface area of ​​the carriers per unit volume is defined as the total number of carriers per 100 mL volume in a cylindrical container with a diameter of 29 mm × the surface area of ​​a single carrier;

[0019] The surface area of ​​a single carrier is defined as the surface area of ​​the carrier of the catalytic medium loaded in the nth catalyst bed.

[0020] In the present invention, unless otherwise specified, the catalytic medium is a catalyst for preparing phthalic anhydride by oxidation of o-xylene.

[0021] In the present invention, unless otherwise specified, in the catalyst, along the flow direction, the S of each catalyst bed n The decreasing order refers to the S of the n+1th catalyst bed. n+1 The S of the nth catalyst bed n Satisfaction: S n+1 <S n , where S n+1 is the total surface area of ​​the carrier per unit volume of the n+1th catalyst bed along the direction of the flow, S n It is the total surface area of ​​the carrier within the unit volume of the nth catalyst bed along the direction of logistics, where n is a positive integer.

[0022] In the present invention, unless otherwise specified, in the catalyst, along the flow direction, the P of each catalyst bed nThe increasing order refers to the P of the n+1th catalyst bed. n+1 The P of the nth catalyst bed n Satisfaction: P n+1 >P n , where P n+1 is the surface area of ​​a single carrier in the n+1th catalyst bed along the direction of the flow, P n is the surface area of ​​a single carrier in the nth catalyst bed along the direction of flow, where n is a positive integer.

[0023] In some embodiments of the present invention, preferably, in the catalyst, S of each catalyst bed n With P n The relationship satisfying formula (1) is:

[0024]

[0025] Among them, S n is the total surface area of ​​the carrier per unit volume of the nth catalyst bed along the direction of the flow, P n is the surface area of ​​a single carrier of the nth catalyst bed along the direction of the flow, n is a positive integer, and m is any value from 50 to 200.

[0026] In some embodiments of the present invention, preferably, the catalyst comprises: 3-8 catalyst beds, preferably 4 catalyst beds.

[0027] In some embodiments of the present invention, preferably, in the catalyst, along the flow direction, the S1 of the first catalyst bed is 500-650cm 2 , preferably 580-620cm 2 ; S2 of the second catalyst bed is 480-620cm 2 , preferably 500-600cm 2 ; S3 of the third catalyst bed is 380-550cm 2 , preferably 400-520cm 2 ; S4 of the fourth catalyst bed is 280-480cm 2 , preferably 350-420cm 2 .

[0028] In some embodiments of the present invention, preferably, in the catalyst, along the flow direction, the P1 of the first catalyst bed is 100-250 mm 2 , preferably 150-250mm 2 ; The second catalyst bed P2 is 100-350mm 2 , preferably 150-300mm 2; The third catalyst bed P3 is 200-400mm 2 , preferably 250-350mm 2 ; The P4 of the fourth catalyst bed is 300-500mm 2 , preferably 300-400mm 2 .

[0029] In the present invention, unless otherwise specified, the surface area parameter of a single catalyst is measured by calculating the average value three times.

[0030] According to a preferred embodiment of the present invention, in the catalyst, along the logistics direction, the catalysts in the first catalyst bed to the fourth catalyst bed are catalytic medium A, catalytic medium B, catalytic medium C and catalytic medium D, wherein the S1 of the first catalyst bed is 580-620cm 2 , S2 of the second catalyst bed is 500-600cm 2 , S3 of the third catalyst bed is 400-520cm 2 , S4 of the fourth catalyst bed is 350-420cm 2 ; P1 of the first catalyst bed is 150-250mm 2 , the second catalyst bed P2 is 150-300mm 2 , the third catalyst bed P3 is 250-350mm 2 , the P4 of the fourth catalyst bed is 300-400mm 2 .

[0031] In some embodiments of the present invention, preferably, in the catalyst, along the logistics direction, the height ratio of the first catalyst bed, the second catalyst bed, the third catalyst bed and the fourth catalyst bed is 10-50: 10-40: 10-40: 0-30, preferably 30-45: 20-30: 20-30: 0-20. The preferred conditions are more conducive to improving the o-xylene load, phthalic anhydride yield and o-xylene conversion rate, thereby reducing impurities or over-oxidation.

[0032] In some embodiments of the present invention, preferably, in the catalytic medium, the weight ratio of the active component to the carrier is 10-18: 100. In the present invention, when the loading amount of the active component in the catalytic medium is too low, the conversion rate of o-xylene is relatively low; when the loading amount of the active component in the catalytic medium is too high, the catalytic medium will be severely deeply oxidized, resulting in more by-products, so that the yield of phthalic anhydride is significantly reduced.

[0033] In a specific embodiment of the present invention, the catalytic media AD each independently include a carrier and an active component supported on the carrier, wherein the weight ratio of the active component to the carrier is 8-20:100, preferably 10-18:100.

[0034] In some embodiments of the present invention, preferably, the active components include: a main active component, TiO2 and an auxiliary agent; further preferably, the main active component includes: V2O5, a phosphorus compound, a potassium compound and optionally a cesium compound.

[0035] In some embodiments of the present invention, preferably, based on the total weight of the active components, the V2O5 content is 5-18wt%, the phosphorus compound content calculated as P is 0.01-0.3wt%, the potassium compound content calculated as K is 0.01-0.5wt%, the cesium compound content calculated as Cs is 0-1wt%, the additive content calculated as oxide is 0.1-10wt%, and the balance is TiO2.

[0036] According to the present invention, the preparation method of the catalytic medium is not particularly limited, and the catalytic medium can be prepared according to the commonly used methods in the art. Preferably, the preparation method of the catalytic medium loaded in each catalyst bed comprises: loading a slurry containing a vanadium source, a phosphorus source, a potassium source, an optional cesium source, a titanium source and an additive on a carrier, and obtaining the catalytic medium through drying and calcination.

[0037] In some embodiments of the present invention, preferably, in the slurry, the dosage ratio of the vanadium source, phosphorus source, potassium source, cesium source, titanium source and additive is 5-18: 0.01-0.3: 0.01-0.5: 0-1: 85.88-93.2: 0.1-10, wherein the vanadium source is calculated as V2O5, the phosphorus source is calculated as P, the potassium source is calculated as K, the cesium source is calculated as Cs, the titanium source is calculated as TiO2, and the additive is calculated as oxide.

[0038] According to the present invention, there is no particular limitation on the mixing method, and wet grinding can be used. Considering the convenience and timeliness of grinding, preferably, the mixing is completed in a ball mill. Further preferably, the grinding time in the ball mill is 1-5h, preferably 2-4h.

[0039] According to a preferred implementation of the present invention, preferably, the method for preparing the catalytic medium in each catalyst bed comprises:

[0040] (1) mixing a vanadium source, a phosphorus source, a potassium source, an optional cesium source, a portion of an additive and a solvent to obtain a solution A;

[0041] (2) mixing the solution A with the titanium source, the remaining additives, and the binder to obtain a slurry;

[0042] (3) The slurry is loaded on a carrier, and the catalytic medium is obtained after drying and calcining.

[0043] In the present invention, in step (1), there is a wide range of selection for the mixing method, as long as the vanadium source, phosphorus source, potassium source, optional cesium source, part of the additives and the solvent are mixed evenly.

[0044] In the present invention, in step (2), there is a wide range of options for the mixing method, as long as solution A, titanium source, the remaining auxiliary agent and binder are mixed evenly.

[0045] According to the present invention, in order to prevent the vanadium source in solution A from reacting with the additive to produce precipitation, preferably, the solution A also contains oxalic acid. Further preferably, the weight ratio of the oxalic acid to the vanadium source is 1:0.2-0.8.

[0046] In the present invention, the type of the carrier has a wide range of selection, that is, the carrier is a conventional type in the art. Preferably, the carrier is a non-porous inert carrier, preferably selected from at least one of alumina, talc, silicon carbide, aluminum silicate, quartz and ceramics.

[0047] In the present invention, there is no particular limitation on the shape of the carrier, for example, it can be cylindrical, spherical, annular or granular. Preferably, the shape of the carrier is an annular carrier.

[0048] In some embodiments of the present invention, preferably, the outer diameter of the carrier is 3-13mm, for example, 3mm, 5mm, 7mm, 9mm, 11mm, 13mm, and any value in the range of any two values, preferably 5-9mm; the height is 2-12mm, for example, 2mm, 3mm, 5mm, 7mm, 8mm, 10mm, 12mm, and any value in the range of any two values, preferably 3-8mm; the porosity is 0.5-10%, for example, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, and any value in the range of any two values, preferably 2-8%. In the present invention, unless otherwise specified, the outer diameter parameter is measured by the method of taking the average value of 3 times with a vernier caliper; the height parameter is measured by the method of taking the average value of 3 times with a vernier caliper; and the porosity parameter is measured by a porosity measuring instrument.

[0049] In some embodiments of the present invention, preferably, the surface area of ​​the carrier is 100-500 mm 2 , for example, 100mm 2 , 150mm 2 , 200mm 2 、300mm2 , 400mm 2 , 500mm 2 , and any value in the range of any two values, preferably 150-400mm 2 .

[0050] In the present invention, the type of the vanadium source has a wide selection range. Preferably, the vanadium source is selected from at least one of ammonium metavanadate, vanadium pentoxide and sodium vanadate, preferably ammonium metavanadate.

[0051] In the present invention, the type of the phosphorus source has a wide selection range. Preferably, the phosphorus source is selected from at least one of diammonium phosphate, triammonium phosphate and phosphorus pentoxide, preferably diammonium phosphate.

[0052] In the present invention, the type of the potassium source has a wide selection range. Preferably, the potassium source is selected from at least one of potassium nitrate, potassium sulfate, potassium chloride and potassium bicarbonate, preferably potassium sulfate.

[0053] In the present invention, the type of the cesium source has a wide selection range. Preferably, the cesium source is selected from at least one of cesium nitrate, cesium sulfate, cesium chloride and cesium carbonate, preferably cesium sulfate.

[0054] In the present invention, the type of the titanium source has a wide range of choices. Preferably, the titanium source is titanium dioxide; further, the titanium dioxide is anatase TiO2 with a specific surface area of ​​10-30 m 2 / g, for example, 10m 2 / g, 15m 2 / g, 17m 2 / g, 20m 2 / g, 26m 2 / g, 30m 2 / g, and any value in the range of any two values, preferably 17-26m 2 / g.

[0055] In the present invention, the type of the auxiliary agent has a wide range of selection, as long as it contains the corresponding auxiliary element, and the auxiliary agent is a substance that can obtain the corresponding auxiliary element oxide through subsequent treatment. Preferably, the auxiliary agent contains at least one selected from rubidium, cerium, niobium, chromium, tungsten, iron, silver, cobalt, gold, gallium, indium, antimony, bismuth, zirconium, erbium, tungsten and tin.

[0056] According to the present invention, the auxiliary agent may include metal oxides and / or metal water-soluble salts that can provide the above-mentioned metal elements; further preferably, the metal oxide is silver oxide and / or antimony oxide, and the metal water-soluble salt is at least one of the water-soluble salts of rubidium, cerium, niobium, chromium, tungsten, iron, cobalt, gold, gallium, indium, bismuth, zirconium, erbium, tungsten and tin elements.

[0057] In the present invention, unless otherwise specified, the water-soluble metal salt may be nitrate, carbonate, sulfate, oxalate, chloride, etc.

[0058] According to the present invention, preferably, the water-soluble salt of cesium is at least one of cesium nitrate, cesium sulfate and cesium chloride, more preferably cesium sulfate.

[0059] In some embodiments of the present invention, preferably, the solvent includes water and an optional water-soluble organic solvent; wherein the water-soluble organic solvent includes but is not limited to at least one of methanol, ethanol, ethylene glycol dimethyl ether, formamide and N,N-dimethylamide.

[0060] In some embodiments of the present invention, preferably, the weight ratio of water to water-soluble organic solvent in the solvent is 1:0-0.3, for example, 1:0.1, 1:0.15, 1:0.2: 1:0.25, 1:0.3, and any value in the range consisting of any two values, preferably 1:0.1-0.2.

[0061] According to the present invention, preferably, the slurry also contains a binder; further preferably, the binder is at least one of a vinyl acetate-acrylate copolymer emulsion, a vinyl acetate-ethylene copolymer emulsion, a vinyl acetate-maleic acid copolymer emulsion and an acrylic acid-maleic acid copolymer emulsion, preferably a vinyl acetate-ethylene copolymer emulsion.

[0062] The present invention has a wide range of selection for the amount of the binder, in order to make the active components more evenly loaded on the carrier. Preferably, the amount of binder added is such that the viscosity of the slurry is 10-40 mPa·s, for example, 10 mPa·s, 12 mPa·s, 15 mPa·s, 20 mPa·s, 25 mPa·s, 30 mPa·s, 35 mPa·s, 40 mPa·s, and any value in the range of any two values, preferably 12-25 mPa·s. As long as the viscosity of the slurry can be within the specified range, the binder can be used in any form, preferably the binder is used in the form of an emulsion, and further preferably, the solid content of the binder is 10-15 wt%.

[0063] In the present invention, there is no particular limitation on the loading method, as long as the slurry can be loaded onto the carrier. Preferably, the loading method is spraying.

[0064] According to the present invention, in order to accelerate the volatilization of water and organic solvent in the slurry, so as to quickly and effectively attach the active components to the carrier, preferably, hot air at 90-160°C is used for drying during the spraying process; more preferably, hot air at 100-130°C is used for drying.

[0065] In some embodiments of the present invention, preferably, the spraying rate is 30-60 mL / min, for example, 30 mL / min, 35 mL / min, 40 mL / min, 45 mL / min, 50 mL / min, 55 mL / min, 60 mL / min, and any value in the range of any two values, preferably 35-50 mL / min, relative to every 2000 grams of the carrier. Controlling the spraying rate within the above-defined range can prevent the waste of the slurry and the active component from falling off the carrier.

[0066] According to the present invention, in order to make the slurry adhere to the carrier more easily, preferably, the carrier is heated before spraying to maintain the temperature of the carrier at 80-130°C, for example, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, and any value in the range of any two values, preferably 110-130°C.

[0067] According to the present invention, the calcination conditions can be selected in a wide range. Preferably, the calcination conditions include: 400-450° C., and a time of 2-24 h.

[0068] Since high temperature will cause the binder to disappear and reduce the adhesion of the active components on the catalytic medium, thus causing the active components to fall off during the catalytic medium filling process, in order to avoid the active components from falling off during the catalytic medium filling process, the catalytic medium precursor is first loaded into the catalyst bed and then calcined to obtain the catalytic medium.

[0069] According to the present invention, the device used for the spraying is not particularly limited, as long as it can meet the needs of the spraying. Preferably, the device used for the spraying includes a hot air blower, a coating main unit, an exhaust fan, a slurry spraying system, a control system and a strong power supply cabinet. The coating main unit includes a coating drum and a power mechanism thereof, and the coating drum is enclosed in the coating main unit, and the rotation speed can be adjusted. The coating drum adopts a horizontal hollow cylindrical structure, which can increase the contact opportunity between the active component and the inert carrier material. A circular mesh with an aperture of 1-8mm, preferably a circular mesh of 3-4mm, is provided on the horizontal hollow cylindrical structure, the purpose of which is to ensure that hot air penetrates the coating drum, and after evaporating the solvent in the slurry on the carrier, it passes through the coating drum to take the solvent away, preferably, the coating drum rotation speed is 5-10rpm. The slurry spraying system consists of a nozzle and a feeding system, and the feeding system consists of a barrel, a stirring and feeding pump and a feed pipeline. The feed pump can adjust the spraying rate, and the nozzle can ensure that the slurry can be evenly sprayed on the surface of the inert carrier material after passing through the feed pump, forming a smooth and flat coating of catalytically active substances to prepare a catalyst.

[0070] According to the present invention, the spraying amount of the active components in the catalytic medium is controlled by the drum rotation speed, spraying rate, loss rate and spraying time, thereby controlling the content of the active components in the catalytic medium.

[0071] According to a particularly preferred embodiment of the present invention, the catalyst comprises at least three catalyst beds arranged in sequence, and the weight ratio of the active component to the carrier in the catalytic medium loaded in each catalyst bed is 8-20:100;

[0072] Among them, in the catalyst, along the logistics direction, the S of each catalyst bed n The P of each catalyst bed decreases in sequence. n Increasing successively, among which, S n is the total surface area of ​​the carrier per unit volume of the nth catalyst bed along the direction of the flow, P n is the surface area of ​​a single carrier in the nth catalyst bed along the direction of the flow, where n is a positive integer;

[0073] The total surface area of ​​the carriers per unit volume is defined as the total number of carriers per 100 mL volume in a cylindrical container with a diameter of 29 mm × the surface area of ​​a single carrier;

[0074] Wherein, the surface area of ​​a single carrier is defined as the surface area of ​​the carrier of the catalytic medium loaded in the nth catalyst bed;

[0075] Among them, in the catalyst, the S of each catalyst bed is n With P n The relationship satisfying formula (1) is:

[0076]

[0077] Wherein, m is any value between 50 and 200.

[0078] The second aspect of the present invention provides a method for preparing phthalic anhydride by oxidizing o-xylene, which comprises: introducing o-xylene and an oxygen-containing gas into the catalyst provided in the first aspect, and sequentially contacting and reacting with the catalytic medium in each catalyst bed.

[0079] According to the present invention, preferably, the reaction conditions include: molten salt temperature is 300-450°C, preferably 330-400°C; volume space velocity is 700-5000h -1 , preferably 2200-4000h -1 ; The concentration of o-xylene is 60-120g / m 3 , preferably 80-110g / m 3 Wherein, the volume space velocity is the volume space velocity of the oxygen-containing gas.

[0080] According to the present invention, the gas may be an oxygen-containing gas, preferably, the gas is air.

[0081] According to the present invention, the reaction of oxidizing o-xylene to produce phthalic anhydride can be carried out in a fixed bed or in a fluidized bed. Preferably, the reaction of oxidizing o-xylene to produce phthalic anhydride is carried out in a fixed bed single tube reactor. Further preferably, the tube length of the fixed bed single tube reactor is 3000-4800 mm and the inner diameter is 20-30 mm. The outside of the reaction tube of the fixed bed single tube reactor adopts a circulating molten salt to force the exchange of reaction heat. There is a thermocouple sleeve with an outer diameter of 5-10 mm in the reaction tube, and there are several thermocouples with the same spacing in the thermocouple sleeve for measuring the reaction bed temperature and the molten salt temperature. The outlet of the fixed bed single tube reactor is connected to a product capture device, and a sampling port is arranged at the outlet of the lower end of the reaction tube.

[0082] According to the present invention, preferably, the catalytic medium in the reaction tube of the fixed bed single tube reactor is loaded in sections, and the total loading height is 2400-3400 mm; according to the logistics direction, the loading height of the catalytic medium in the first section is 10-50% of the total loading height, the loading height of the catalytic medium in the second section is 10-40% of the total loading height, the loading height of the catalytic medium in the third section is 10-40% of the total loading height, and the loading height of the catalytic medium in the fourth section is 0-30% of the total loading height.

[0083] The present invention defines the total surface variation law of the carrier per unit volume in each catalyst bed, that is, uses multi-sized carriers to load active components to prepare the catalytic medium, optimizes the catalyst bed function, avoids deep oxidation of the product, and improves the selectivity of the catalytic medium, thereby improving the performance of the catalytic medium. Using the method provided by the present invention, the concentration of the reaction raw materials can be increased by 5-10g / Nm 3 The raw material conversion rate can reach 99.95%, and the actual mass yield of industrial production of phthalic anhydride can be increased by 1-3%.

[0084] The present invention will be described in detail below through examples.

[0085] The molecular formula of ammonium metavanadate is NH4VO3, and its relative molecular weight is 116.98;

[0086] The molecular formula of diammonium phosphate is NH4H2PO4, and its relative molecular weight is 115.03;

[0087] The molecular formula of cesium sulfate is Cs2SO4, and its relative molecular weight is 361.87;

[0088] The molecular formula of potassium sulfate is K2SO4, and its relative molecular weight is 174.24;

[0089] Titanium dioxide is anatase titanium dioxide with a specific surface area of ​​19m 2 / g;

[0090] The solid content of the vinyl acetate-ethylene copolymer emulsion was 50% by weight.

[0091] The catalytic products were analyzed by chromatography;

[0092] The calculation formula of the conversion rate (%) of o-xylene is:

[0093]

[0094] The calculation formula of the yield (%) of phthalic anhydride is:

[0095]

[0096] The content of each active component in the following catalytic medium is calculated by the feed amount, and the content of each active component in the catalytic medium is listed in Table 1.

[0097] Preparation Example 1

[0098] (1) 50 g of ammonium metavanadate, 115.4 g of oxalic acid, 4.62 g of cesium sulfate, 0.1 g of ammonium dihydrogen phosphate, 5 g of niobium oxalate, 0.2 g of potassium sulfate, 220 mL of formamide and 2200 mL of water were prepared into a solution.

[0099] (2) The solution, 625 g of titanium dioxide, and 12.22 g of antimony trioxide were poured into a ball mill, and an appropriate amount of vinyl acetate / ethylene copolymer emulsion was added. The mixture was ball milled for 4 h to form a uniform slurry, and the slurry concentration was controlled to be 15 mPa·s.

[0100] (3) 2000 g of a talc ring inert carrier (outer diameter 6 mm, height 5 mm, wall thickness 1.5 mm, surface area 183.7 mm 2 ) is placed in a rotating drum, and the drum speed is controlled to be 5rpm; the emulsion prepared above is added to the stirring tank of the liquid spraying system and stirred; the hot air blower is turned on, and the hot air at 100°C penetrates into the drum to preheat the above carrier. When the carrier temperature reaches 110°C, the feed nozzle is turned on, and the liquid spraying rate is controlled to be 30mL / min; the slurry is sprayed on the surface of the carrier through the nozzle and quickly dried by hot air; the content of the active component reaches 10wt% of the weight of the carrier, and the spraying is completed, and it is calcined at 400°C for 5h to obtain the catalytic medium A1.

[0101] Preparation Example 1

[0102] The method of Preparation Example 1 was followed, except that 2000 g of a talc ring inert carrier (outer diameter 6 mm, height 5 mm, wall thickness 1.5 mm, surface area 183.7 mm 2 ) was replaced with 2000 g of a steatite ring inert carrier (outer diameter 8 mm, height 6 mm, wall thickness 1.5 mm, surface area 306.2 mm 2 ), and other conditions remain the same to obtain catalytic medium A2.

[0103] Preparation Example 2

[0104] (1) 55.75 g of ammonium metavanadate, 128.67 g of oxalic acid, 3.21 g of cesium sulfate, 0.1 g of ammonium dihydrogen phosphate, 5.25 g of niobium oxalate, 0.1 g of potassium sulfate, 220 mL of formamide and 2200 mL of water were prepared into a solution.

[0105] (2) The solution, 625 g of titanium dioxide, and 12.22 g of antimony trioxide were poured into a ball mill, and an appropriate amount of vinyl acetate / ethylene copolymer emulsion was added. The mixture was ball milled for 4 h to form a uniform slurry, and the slurry concentration was controlled to be 13 mPa·s.

[0106] (3) 2000 g of talc ring inert carrier (outer diameter 6 mm, height 6 mm, wall thickness 1.5 mm, surface area 212 mm 2) is placed in a rotating drum, and the drum speed is controlled to be 5rpm; the emulsion prepared above is added to the stirring tank of the liquid spraying system and stirred; the hot air blower is turned on, and the hot air at 100°C penetrates into the drum to preheat the above carrier. When the carrier temperature reaches 90°C, the feed nozzle is turned on, and the liquid spraying rate is controlled to be 50mL / min; the slurry is sprayed on the surface of the carrier through the nozzle and quickly dried by hot air; the content of the active component reaches 13wt% of the weight of the carrier, and the spraying is completed, and it is calcined at 400°C for 5h to obtain the catalytic medium B1.

[0107] Preparation Example 2'

[0108] The method of Preparation Example 2 was followed, except that 2000 g of a talc ring inert carrier (outer diameter 6 mm, height 6 mm, wall thickness 1.5 mm, surface area 212 mm 2 ) was replaced with 2000 g of a steatite ring inert carrier (outer diameter 8 mm, height 6 mm, wall thickness 1.5 mm, surface area 306.2 mm 2 ), and other conditions remain the same to obtain catalytic medium B2.

[0109] Preparation Example 3

[0110] (1) 60.08 g of ammonium metavanadate, 138.66 g of oxalic acid, 2.14 g of cesium sulfate, 4.12 g of ammonium dihydrogen phosphate, 3.86 g of niobium oxalate, 0.05 g of potassium sulfate, 3.59 g of zirconium sulfate tetrahydrate, 220 mL of formamide and 2200 mL of water were prepared into a solution.

[0111] (2) The solution, 625 g of titanium dioxide, and 17.45 g of antimony trioxide were poured into a ball mill, and an appropriate amount of vinyl acetate / ethylene copolymer emulsion was added. The mixture was ball milled for 4 h to form a uniform slurry, and the slurry concentration was controlled to be 14 mPa·s.

[0112] (3) 2000 g of a talc ring inert carrier (outer diameter 7 mm, height 7 mm, wall thickness 1.5 mm, surface area 293.6 mm) was placed on a 2 ) is placed in a rotating drum, and the drum speed is controlled to be 5rpm; the emulsion prepared above is added to the stirring tank of the liquid spraying system and stirred; the hot air blower is turned on, and the hot air at 100°C penetrates into the drum to preheat the above carrier. When the carrier temperature reaches 130°C, the feed nozzle is turned on, and the liquid spraying rate is controlled to be 60mL / min; the slurry is sprayed on the surface of the carrier through the nozzle and quickly dried by hot air; the content of the active component reaches 14wt% of the weight of the carrier, and the spraying is completed, and it is calcined at 400°C for 5h to obtain the catalytic medium C1.

[0113] Preparation Example 3'

[0114] The method of Preparation Example 3 was followed, except that 2000 g of a talc ring inert carrier (outer diameter 7 mm, height 7 mm, wall thickness 1.5 mm, surface area 293.6 mm 2 ) was replaced with 2000 g of a steatite ring inert carrier (outer diameter 8 mm, height 6 mm, wall thickness 1.5 mm, surface area 306.2 mm 2 ), and other conditions remain the same to obtain catalytic medium C2.

[0115] Preparation Example 4

[0116] (1) 72.28 g of ammonium metavanadate, 166.82 g of oxalic acid, 0.4 g of cesium sulfate, 5.18 g of ammonium dihydrogen phosphate, 6.68 g of niobium oxalate, 4.39 g of zirconium sulfate tetrahydrate, 220 mL of formamide and 2200 mL of water were prepared into a solution.

[0117] (2) The solution, 625 g of titanium dioxide, and 2.57 g of antimony trioxide were poured into a ball mill, and an appropriate amount of vinyl acetate / ethylene copolymer emulsion was added. The mixture was ball milled for 4 h to form a uniform slurry, and the slurry concentration was controlled to be 12 mPa·s.

[0118] (3) 2000 g of a talc ring inert carrier (outer diameter 8 mm, height 6 mm, wall thickness 1.5 mm, surface area 306.2 mm) was placed in the 2 ) is placed in a rotating drum, and the drum speed is controlled to be 5rpm; the emulsion prepared above is added to the stirring tank of the liquid spraying system and stirred; the hot air blower is turned on, and the hot air at 100°C penetrates into the drum to preheat the above carrier. When the carrier temperature reaches 100°C, the feed nozzle is turned on, and the liquid spraying rate is controlled to be 30mL / min; the slurry is sprayed on the surface of the carrier through the nozzle and quickly dried by hot air; the content of the active component reaches 15wt% of the weight of the carrier, and the spraying is completed, and it is calcined at 400°C for 5h to obtain the catalytic medium D1.

[0119] Table 1

[0120]

[0121] Example 1

[0122] A fixed bed single tube reactor simulating industrial production conditions is used to load the catalytic medium. The fixed bed single tube reactor has an inner diameter of 29 mm, a tube length of 4400 mm, and a loading height of 3400 mm. In the direction of raw material flow, the reactor comprises: a first catalyst bed, a second catalyst bed, and a third catalyst bed, wherein the first catalyst bed, the second catalyst bed, and the third catalyst bed are loaded with catalytic medium A1, catalytic medium C1, and catalytic medium D1 in sequence, and the loading lengths of the first catalyst bed, the second catalyst bed, and the third catalyst bed are 1600 mm, 800 mm, and 1000 mm, respectively.

[0123] Among them, the S1 of the first catalyst bed is 618cm 2 ; S2 of the second catalyst bed is 500cm 2 ; S3 of the third catalyst bed is 400cm 2 That is, along the flow direction, the S of each catalyst bed n Satisfaction in descending order;

[0124] Among them, the P1 of the first catalyst bed is 183.7mm 2 ; P2 of the second catalyst bed is 293.6 mm 2 ; P3 of the third catalyst bed is 306.2mm 2 That is, along the flow direction, the P of each catalyst bed n Satisfaction increases in sequence;

[0125] Among them, S1 and P1 of the first catalyst bed satisfy the relationship of formula (1): Wherein, m=163.58; S2 and P2 of the second catalyst bed satisfy the relationship of formula (1): Wherein, m=163.03; S3 and P3 of the third catalyst bed satisfy the relationship of formula (1): Among them, m=119.37.

[0126] Example 2

[0127] A fixed bed single tube reactor simulating industrial production conditions is used to load the catalytic medium. The fixed bed single tube reactor has an inner diameter of 29 mm, a tube length of 4400 mm, and a loading height of 3400 mm. In the direction of raw material flow, the reactor comprises: a first catalyst bed, a second catalyst bed, and a third catalyst bed, wherein the first catalyst bed, the second catalyst bed, and the third catalyst bed are loaded with catalytic medium A1, catalytic medium B1, and catalytic medium D1 in sequence, and the loading lengths of the first catalyst bed, the second catalyst bed, and the third catalyst bed are 1400 mm, 1200 mm, and 800 mm, respectively.

[0128] Among them, the S1 of the first catalyst bed is 603cm 2 ; S2 of the second catalyst bed is 585cm 2 ; S3 of the third catalyst bed is 405cm 2 That is, along the flow direction, the S of each catalyst bed n Satisfaction in descending order;

[0129] Among them, the P1 of the first catalyst bed is 183.7mm 2; P2 of the second catalyst bed is 212mm 2 ; P3 of the third catalyst bed is 306.2mm 2 That is, along the flow direction, the P of each catalyst bed n Satisfaction increases in sequence;

[0130] Among them, S1 and P1 of the first catalyst bed satisfy the relationship of formula (1): Wherein, m=171.75; S2 and P2 of the second catalyst bed satisfy the relationship of formula (1): Wherein, m=57.39; S3 and P3 of the third catalyst bed satisfy the relationship of formula (1): Among them, m=117.73.

[0131] Example 3

[0132] A fixed bed single tube reactor simulating industrial production conditions is used to load the catalytic medium. The fixed bed single tube reactor has an inner diameter of 29 mm, a tube length of 4400 mm, and a loading height of 3400 mm. In the direction of raw material flow, the fixed bed single tube reactor comprises: a first catalyst bed, a second catalyst bed, a third catalyst bed, and a fourth catalyst bed, wherein the first catalyst bed, the second catalyst bed, the third catalyst bed, and the fourth catalyst bed are sequentially loaded with catalytic medium A1, catalytic medium B1, catalytic medium C1, and catalytic medium D1, and the loading lengths of the first catalyst bed, the second catalyst bed, the third catalyst bed, and the fourth catalyst bed are 1400 mm, 700 mm, 800 mm, and 500 mm, respectively.

[0133] Among them, the S1 of the first catalyst bed is 610cm 2 ; S2 of the second catalyst bed is 589cm 2 ; S3 of the third catalyst bed is 495cm 2 ; S4 of the fourth catalyst bed is 400cm 2 That is, along the flow direction, the S of each catalyst bed n Satisfaction in descending order;

[0134] Among them, the P1 of the first catalyst bed is 183.7mm 2 ; P2 of the second catalyst bed is 212mm 2 ; P3 of the third catalyst bed is 293.6mm 2 ; P4 of the fourth catalyst bed is 306.2mm 2 That is, along the flow direction, the P of each catalyst bed n Satisfaction increases in sequence;

[0135] Among them, S1 and P1 of the first catalyst bed satisfy the relationship of formula (1): Wherein, m=167.94; S2 and P2 of the second catalyst bed satisfy the relationship of formula (1): Wherein, m=55.5; S3 and P3 of the third catalyst bed satisfy the relationship of formula (1): Wherein, m=81.4; S4 and P4 of the fourth catalyst bed satisfy the relationship of formula (1): Among them, m=69.37.

[0136] Example 4

[0137] The method of Example 1 is the same except that the first catalyst bed, the second catalyst bed and the third catalyst bed are filled with catalytic medium A1, catalytic medium B1 and catalytic medium C1 in sequence, and the other conditions are the same;

[0138] Among them, the S1 of the first catalyst bed is 605cm 2 ; S2 of the second catalyst bed is 592cm 2 ; S3 of the third catalyst bed is 500cm 2 That is, along the flow direction, the S of each catalyst bed n Satisfaction in descending order;

[0139] Among them, the P1 of the first catalyst bed is 183.7mm 2 ; P2 of the second catalyst bed is 212mm 2 ; P3 of the third catalyst bed is 293.6mm 2 That is, along the flow direction, the P of each catalyst bed n Satisfaction increases in sequence;

[0140] Among them, S1 and P1 of the first catalyst bed satisfy the relationship of formula (1): Wherein, m=170.66; S2 and P2 of the second catalyst bed satisfy the relationship of formula (1): Wherein, m=54.08; S3 and P3 of the third catalyst bed satisfy the relationship of formula (1): Among them, m=79.7.

[0141] Comparative Example 1

[0142] The method of Example 1 is the same except that the first catalyst bed, the second catalyst bed and the third catalyst bed are sequentially filled with catalytic medium A2, catalytic medium C2 and catalytic medium D1, and the other conditions are the same;

[0143] Among them, the S1 of the first catalyst bed is 611cm 2 ; S2 of the second catalyst bed is 608cm 2 ; S3 of the third catalyst bed is 400cm 2 That is, along the flow direction, the S of each catalyst bed n Satisfaction in descending order;

[0144] Among them, the P1 of the first catalyst bed is 306.2mm 2 ; P2 of the second catalyst bed is 306.2 mm 2 ; P3 of the third catalyst bed is 306.2mm 2 That is, along the flow direction, the P of each catalyst bed n Not satisfying the increasing order;

[0145] Among them, S1 and P1 of the first catalyst bed do not satisfy the relationship of formula (1): Wherein, m=300.46; S2 and P2 of the second catalyst bed satisfy the relationship of formula (1): Wherein, m=134.77; S3 and P3 of the third catalyst bed satisfy the relationship of formula (1): Among them, m=119.37.

[0146] Comparative Example 2

[0147] The method of Example 2 is the same except that the first catalyst bed, the second catalyst bed and the third catalyst bed are sequentially filled with catalytic medium A2, catalytic medium B2 and catalytic medium D1, and the other conditions are the same;

[0148] Among them, the S1 of the first catalyst bed is 614cm 2 ; S2 of the second catalyst bed is 616cm 2 ; S3 of the third catalyst bed is 405cm 2 That is, along the flow direction, the S of each catalyst bed n Not satisfied with decreasing order;

[0149] Among them, the P1 of the first catalyst bed is 306.2mm 2 ; P2 of the second catalyst bed is 306.2 mm 2 ; P3 of the third catalyst bed is 306.2mm 2 That is, along the flow direction, the P of each catalyst bed n Not satisfying the increasing order;

[0150] Among them, S1 and P1 of the first catalyst bed do not satisfy the relationship of formula (1): Wherein, m=299.48; S2 and P2 of the second catalyst bed do not satisfy the relationship of formula (1): Wherein, m=298.82; S3 and P3 of the third catalyst bed satisfy the relationship of formula (1): Among them, m=117.73.

[0151] Comparative Example 3

[0152] The method of Example 3 is the same except that the first catalyst bed, the second catalyst bed, the third catalyst bed and the fourth catalyst bed are sequentially filled with catalytic medium A2, catalytic medium B2, catalytic medium C2 and catalytic medium D1, and the other conditions are the same;

[0153] Among them, the S1 of the first catalyst bed is 611cm 2 ; S2 of the second catalyst bed is 615cm 2 ; S3 of the third catalyst bed is 607cm 2 ; S4 of the fourth catalyst bed is 400cm 2 That is, along the flow direction, the S of each catalyst bed n Satisfaction in descending order;

[0154] Among them, the P1 of the first catalyst bed is 306.2mm 2 ; P2 of the second catalyst bed is 306.2 mm 2 ; P3 of the third catalyst bed is 306.2mm 2 ; P4 of the fourth catalyst bed is 306.2mm 2 That is, along the flow direction, the P of each catalyst bed n Not satisfying the increasing order;

[0155] Among them, S1 and P1 of the first catalyst bed do not satisfy the relationship of formula (1): Wherein, m=300.46; S2 and P2 of the second catalyst bed satisfy the relationship of formula (1): Wherein, m=132.48; S3 and P3 of the third catalyst bed satisfy the relationship of formula (1): Wherein, m=51.76; S4 and P4 of the fourth catalyst bed satisfy the relationship of formula (1): Among them, m=69.37.

[0156] Test Case

[0157] o-Xylene and air were introduced into the fixed bed single tube reactor filled with catalytic medium in the above examples and comparative examples for evaluation. The evaluation conditions included: a volume space velocity of 3000-4000 h -1 , the test results are listed in Table 2.

[0158] Table 2

[0159]

[0160] It can be seen from the data in Table 2 that when the catalyst provided by the present invention is used for the reaction of oxidizing o-xylene to produce phthalic anhydride, the conversion rate of o-xylene is as high as 99.95%, and the yield of phthalic anhydride is as high as 115.2%.

[0161] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A catalyst for preparing phthalic anhydride by oxidation of o-xylene, the catalyst comprising at least three catalyst beds arranged in sequence, wherein the weight ratio of active component to carrier in the catalytic medium filled in each catalyst bed is 8-20: 100; It is characterized in that Among them, in the catalyst, along the logistics direction, the S of each catalyst bed n The P of each catalyst bed decreases in sequence. n Increasing successively, among which, S n is the total surface area of ​​the carrier per unit volume of the nth catalyst bed along the direction of the flow, P n is the surface area of ​​a single carrier in the nth catalyst bed along the direction of the flow, where n is a positive integer; The total surface area of ​​the carriers per unit volume is defined as the total number of carriers per 100 mL volume in a cylindrical container with a diameter of 29 mm × the surface area of ​​a single carrier; Wherein, the surface area of ​​a single carrier is defined as the surface area of ​​the carrier of the catalytic medium loaded in the nth catalyst bed; Among them, in the catalyst, the S of each catalyst bed is n With P n The relationship satisfying formula (1) is: S n = 0.01 × P n × Formula (1); Wherein, m is any value between 50 and 200.

2. The catalyst according to claim 1, wherein The catalyst comprises: 3-8 catalyst beds.

3. The catalyst according to claim 2, wherein The catalyst comprises 4 catalyst beds.

4. The catalyst according to claim 3, wherein In the catalyst, along the flow direction, the S1 of the first catalyst bed is 500-650 cm 2 ; S2 of the second catalyst bed is 480-620 cm 2 ; S3 of the third catalyst bed is 380-550 cm 2 ; S4 of the fourth catalyst bed is 280-480 cm 2 .

5. The catalyst according to claim 4, wherein In the catalyst, along the flow direction, the S1 of the first catalyst bed is 580-620 cm 2 ; S2 of the second catalyst bed is 500-600 cm 2 ; S3 of the third catalyst bed is 400-520 cm 2 ; S4 of the fourth catalyst bed is 350-420 cm 2 .

6. The catalyst according to claim 3, wherein In the catalyst, along the flow direction, the P1 of the first catalyst bed is 100-250 mm 2 ; P2 of the second catalyst bed is 100-350 mm 2 ; P3 of the third catalyst bed is 200-400 mm 2 ; P4 of the fourth catalyst bed is 300-500 mm 2 .

7. The catalyst according to claim 6, wherein In the catalyst, along the flow direction, the P1 of the first catalyst bed is 150-250 mm 2 ; P2 of the second catalyst bed is 150-300 mm 2 ; P3 of the third catalyst bed is 250-350 mm 2 ; P4 of the fourth catalyst bed is 300-400 mm 2 .

8. The catalyst according to any one of claims 3 to 7, wherein In the catalyst, along the flow direction, the height ratio of the first catalyst bed layer, the second catalyst bed layer, the third catalyst bed layer and the fourth catalyst bed layer is 10-50:10-40:10-40:0-30.

9. The catalyst according to claim 8, wherein In the catalyst, along the flow direction, the height ratio of the first catalyst bed layer, the second catalyst bed layer, the third catalyst bed layer and the fourth catalyst bed layer is 30-45:20-30:20-30:0-20.

10. The catalyst according to claim 1, wherein In the catalytic medium, the weight ratio of the active component to the carrier is 10-18:100; And / or, the active components include a main active component, TiO2 and an auxiliary agent; the main active component includes: V2O5, a phosphorus compound, a potassium compound and a cesium compound.

11. The catalyst according to claim 10, wherein Based on the total weight of the active component, the content of V2O5 is 5-18wt%, the content of phosphorus compounds calculated as P is 0.01-0.3wt%, the content of potassium compounds calculated as K is 0.01-0.5wt%, the content of cesium compounds calculated as Cs is 0-1wt%, the content of additives calculated as oxides is 0.1-10wt%, and the balance is TiO2; And / or, the preparation method of the catalytic medium loaded in each catalyst bed layer independently comprises: loading a slurry containing a vanadium source, a phosphorus source, a potassium source, a cesium source, a titanium source and an additive on a carrier, and obtaining the catalytic medium through drying and calcining; Wherein, the viscosity of the slurry is 10-40 mPa·s.

12. The catalyst according to claim 11, wherein The viscosity of the slurry is 12-25 mPa·s.

13. The catalyst according to claim 11, wherein The vanadium source is selected from at least one of ammonium metavanadate, vanadium pentoxide and sodium vanadate; and / or, the phosphorus source is selected from at least one of diammonium phosphate, triammonium phosphate and phosphorus pentoxide; And / or, the potassium source is selected from at least one of potassium nitrate, potassium sulfate, potassium chloride and potassium bicarbonate; And / or, the cesium source is selected from at least one of cesium nitrate, cesium sulfate, cesium chloride and cesium carbonate; And / or, the titanium source is selected from titanium dioxide, and the titanium dioxide is anatase TiO2 with a specific surface area of ​​10-30m 2 / g; and / or, the auxiliary agent contains at least one selected from rubidium, cerium, niobium, chromium, tungsten, iron, silver, cobalt, gold, gallium, indium, antimony, bismuth, zirconium, erbium, tungsten and tin; and / or, the carrier is a non-porous inert carrier; And / or, the outer diameter of the carrier is 3-13 mm; the height is 2-12 mm; and the void ratio is 0.5-10%.

14. The catalyst according to claim 13, wherein The specific surface area of ​​the anatase TiO2 is 17-26 m 2 / g; and / or, the carrier is selected from at least one of alumina, talc, silicon carbide, aluminum silicate, quartz and ceramics; And / or, the outer diameter of the carrier is 5-9 mm; the height is 3-8 mm; and the porosity is 2-8%.

15. A method for preparing phthalic anhydride by oxidation of o-xylene, characterized in that: The method comprises: introducing o-xylene and oxygen-containing gas into the catalyst described in any one of claims 1 to 14 to sequentially contact with the catalytic medium in each catalyst bed layer and react.

16. The method according to claim 15, wherein: The reaction conditions are: molten salt temperature is 300-450°C; volume space velocity is 700-5000 h -1 ; The concentration of o-xylene is 60-120 g / m 3 .

17. The method according to claim 16, wherein: The reaction conditions are: molten salt temperature is 330-400°C; volume space velocity is 2200-4000 h -1 ; The concentration of o-xylene is 80-110 g / m 3 .