A method for improving diamond ultraviolet detection performance using localized surface plasmon resonance of indium nanoparticles
By plating indium nano-islands on the surface of diamond and using the localized surface plasmon resonance of indium nanoparticles, the problem of insufficient response rate of diamond ultraviolet detectors has been solved, achieving higher spectral response rate and signal-to-noise ratio, close to 5S' standard, and simplifies the preparation process and reduces costs.
Patent Information
- Application Number
- CN202310058297.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-01-16
AI Technical Summary
Existing diamond UV detectors have not yet reached the industry-recognized ‘5S’ standards in terms of responsivity and signal-to-noise ratio, especially the spectral responsivity in the deep ultraviolet range is insufficient.
Using the localized surface plasmon resonance of indium nanoparticles, by plating indium nanoislands on the diamond surface, the local electric field enhancement and semiconductor light absorption effects are used to enhance the ultraviolet light absorption capacity of diamond, thereby improving the ultraviolet detection performance.
It significantly improves the spectral responsivity of diamond UV detectors, especially in the deep ultraviolet region, which is close to the industry-recognized ‘5S’ standard. It also simplifies the device preparation process, avoids the mechanical processing of diamond materials, and reduces production costs.
Smart Images

Figure CN116072744B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for improving the diamond ultraviolet detection spectrum response rate by using indium nanoparticle localized surface plasmon resonance. Background Art
[0002] Ultraviolet detection has attracted much attention due to its important applications in fire detection, ozone monitoring and satellite communications. High-performance photon detectors usually need to meet the "5S" standard, namely high sensitivity, high signal-to-noise ratio, high spectral selectivity, high response speed and high stability. Diamond has excellent physical and chemical properties, such as wide bandgap (5.47eV), high carrier mobility (electron mobility is about 2000cm 2 V -1 s -1 , the hole mobility is about 1700 cm 2 V -1 s -1 ), high thermal conductivity (22W cm -1 K -1 ), high breakdown field strength (greater than 10MV cm -1 ) and high carrier saturation velocity (electrons are about 9.6×10 6 cm s -1 , the hole is about 1.4×10 7 cm s -1 ), known as the ultimate semiconductor, is considered to be the ideal material for photon detectors that is most likely to meet the "5S" standard. In recent years, researchers have been committed to improving the performance of diamond UV detectors by adopting different device structure design schemes and using diamond substrates with higher material quality, and have achieved remarkable results. In addition, since the localized surface plasmon resonance of metal nanoparticles can enhance the local electric field and semiconductor light absorption, using metal nanoparticles whose localized surface plasmon resonance band is in the deep ultraviolet range to enhance diamond UV absorption can be an effective solution to improve the performance of diamond UV detectors. Summary of the invention
[0003] The purpose of the present invention is to improve the response rate of the diamond ultraviolet detector spectrum and to provide a method for improving the ultraviolet detection performance of diamond by using the localized surface plasmon resonance of indium nanoparticles.
[0004] The method of improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles is implemented by the following steps:
[0005] 1. Acid-boiled samples:
[0006] The autoclave is filled with mixed acid, the intrinsic single crystal diamond is immersed in the mixed acid, and heated at a high temperature of 120°C to 160°C for 2 to 4 hours to obtain diamond with oxygen terminals;
[0007] 2. Sample cleaning:
[0008] Using acetone, anhydrous ethanol and deionized water in sequence to ultrasonically clean the diamond with oxygen terminals to obtain cleaned diamond;
[0009] 3. Preparation of Ohmic Contact Electrode:
[0010] Titanium and gold layers were sequentially sputtered on the cleaned diamond surface by magnetron sputtering to form interdigital electrodes, and then the diamond surface was deposited at a depth of less than 8×10 -4 Pa vacuum, annealing at 400-600°C to obtain ohmic contact diamond;
[0011] 4. Preparation of Indium Nanoparticles on Diamond Surface:
[0012] An anodized aluminum mask is set on the surface of the ohmic contact diamond, and a through hole is opened in the anodized aluminum mask. Indium nano-islands are plated on the ohmic contact diamond surface by thermal evaporation of indium, thereby improving the ultraviolet detection performance of diamond through localized surface plasmon resonance of indium nanoparticles.
[0013] The localized surface plasmon resonance band of indium overlaps with the corresponding band of the diamond ultraviolet response peak. Under ultraviolet light excitation, conduction electron oscillation occurs in the indium nanoparticles, capturing light around the surface of the nanoparticles, resulting in an enhancement of the local electric field, thereby enhancing the light absorption of diamond. Under this drive, the diamond excitons and plasmons interact with each other, resulting in an increase in the ultraviolet spectrum response rate. The enhancement effect of indium nanoparticles is more significant than that of other metal particles (such as aluminum nanoparticles and iridium nanoparticles). In addition, indium is relatively cheap, has a low melting point, is convenient for evaporation technology, and has good stability at room temperature. Therefore, the present invention uses indium nanoparticles to enhance the diamond ultraviolet detection spectrum response rate by localized surface plasmon resonance.
[0014] The method of improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles in the present invention has the following beneficial effects:
[0015] 1. There is no need to perform mechanical processing on the diamond material, which simplifies the device preparation process, ensures that the diamond material is not damaged to the greatest extent, and is more conducive to the advantages of diamond materials in device performance.
[0016] 2. Indium is relatively cheap, has a low melting point, and is convenient for evaporation process, and has good stability at room temperature.
[0017] 3. Expanded the ways to enhance the performance of diamond UV detection, making diamond UV detectors closer to the industry-recognized "5S" standard. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 are scanning electron microscope images of the surface of the diamond UV detector in the embodiment at different magnifications, wherein (a) represents a magnification of 70,000×, and (b) represents a magnification of 50,000×;
[0019] Figure 2 The spectral response rate test graph of the diamond ultraviolet detector obtained in the embodiment and the comparative embodiment, wherein the upper curve represents the embodiment and the lower curve represents the comparative embodiment;
[0020] Figure 3 The dark current and photocurrent curves of the diamond ultraviolet detectors obtained in the examples and comparative examples under 215nm illumination, wherein 1 represents the photocurrent of the example, 2 represents the photocurrent of the comparative example, 3 represents the dark current of the example, and 4 represents the dark current of the comparative example. DETAILED DESCRIPTION
[0021] Specific implementation method 1: This implementation method uses indium nanoparticle localized surface plasmon resonance to improve the ultraviolet detection performance of diamond according to the following steps:
[0022] 1. Acid-boiled samples:
[0023] The autoclave is filled with mixed acid, the intrinsic single crystal diamond is immersed in the mixed acid, and heated at a high temperature of 120°C to 160°C for 2 to 4 hours to obtain diamond with oxygen terminals;
[0024] 2. Sample cleaning:
[0025] Using acetone, anhydrous ethanol and deionized water in sequence to ultrasonically clean the diamond with oxygen terminals to obtain cleaned diamond;
[0026] 3. Preparation of Ohmic Contact Electrode:
[0027] Titanium and gold layers were sequentially sputtered on the cleaned diamond surface by magnetron sputtering to form interdigital electrodes, and then the diamond surface was deposited at a depth of less than 8×10 -4 Pa vacuum, annealing at 400-600°C to obtain ohmic contact diamond;
[0028] 4. Preparation of Indium Nanoparticles on Diamond Surface:
[0029] An anodized aluminum mask is set on the surface of the ohmic contact diamond, and a through hole is opened in the anodized aluminum mask. Indium nano-islands are plated on the ohmic contact diamond surface by thermal evaporation of indium, thereby improving the ultraviolet detection performance of diamond through localized surface plasmon resonance of indium nanoparticles.
[0030] In this embodiment, a plurality of indium nanoparticles are plated on the surface of the diamond photon detector, and the diamond ultraviolet light absorption is enhanced through the effect of the localized surface plasmon resonance of the indium nanoparticles, thereby enhancing the spectral response rate of the diamond ultraviolet detector.
[0031] Specific implementation method 2: The difference between this implementation method and specific implementation method 1 is that the mixed acid in step 1 is composed of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1.
[0032] In this embodiment, the mass concentration of concentrated sulfuric acid is 98%, and the mass concentration of concentrated nitric acid is 68%.
[0033] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that in step one, heating is performed at a high temperature of 150° C. for 2 hours.
[0034] Specific implementation method 4: The difference between this implementation method and specific implementation methods 1 to 3 is that the ultrasonic cleaning time in step 2 is 15 to 30 minutes each time.
[0035] Specific implementation mode 5: This implementation mode is different from any one of specific implementation modes 1 to 4 in that the thickness of the sputtered titanium layer in step 3 is 20 to 30 nm, and the thickness of the gold layer is 30 to 50 nm.
[0036] Specific implementation example 6: This implementation example is different from specific implementation example 5 in that the thickness of the sputtered titanium layer in step 3 is 20 nm, and the thickness of the gold layer is 30 nm.
[0037] Specific implementation example 7: This implementation example is different from specific implementation examples 1 to 5 in that the interdigitated electrode in step 3 has 6 to 10 electrodes, and the finger width is 100 to 150 μm.
[0038] Specific embodiment eight: This embodiment differs from any one of specific embodiments one to six in that in step three, an annealing treatment is performed at 500° C. for 30 minutes.
[0039] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 7 in that the process of thermal evaporation of indium in step 4 is to place the single substance indium into an electron beam evaporation device (EB) and control the heating current to 46-52A.
[0040] Specific embodiment ten: This embodiment differs from any one of specific embodiments one to seven in that the diameter of the indium nano-islands in step four is 20 to 30 nm.
[0041] Embodiment: The method of improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles in this embodiment is implemented according to the following steps:
[0042] 1. Acid-boiled samples:
[0043] The autoclave is filled with mixed acid, and the intrinsic single crystal diamond is immersed in the mixed acid, which is concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, and heated at 150°C for 2 hours to obtain diamond with oxygen termination;
[0044] 2. Sample cleaning:
[0045] The diamond with oxygen terminal is ultrasonically cleaned by acetone, anhydrous ethanol and deionized water in sequence, the power of ultrasonic cleaning is 100W, and the cleaning time is 15 minutes to obtain the cleaned diamond;
[0046] 3. Preparation of Ohmic Contact Electrode:
[0047] The magnetron sputtering method was used to sputter a titanium layer with a thickness of 20 nm and a gold layer with a thickness of 30 nm on the cleaned diamond surface to form an interdigitated electrode structure. The interdigitated electrode structure has a total of 10 electrodes (5 interdigitated electrodes on one side), the interval between the interdigitated electrodes is 80 μm, and the finger width is 120 μm. Then, the interdigitated electrode structure is formed in a smaller area than 8×10 -4 Pa vacuum, annealing treatment was performed at 500°C for 30 minutes to obtain ohmic contact diamond;
[0048] 4. Preparation of Indium Nanoparticles on Diamond Surface:
[0049] An anodized aluminum mask is set on the surface of the ohmic contact diamond. The anodized aluminum mask is provided with through holes (the through hole diameter is 20 to 30 nm). Indium nano-islands are plated on the ohmic contact diamond surface by thermal evaporation of indium. The diameter of the indium nano-islands is 20 to 30 nm, thereby improving the ultraviolet detection performance of diamond through the localized surface plasmon resonance of indium nanoparticles.
[0050] In this embodiment, the intrinsic single crystal diamond sample was purchased from Element Six, and is an optical grade CVD single crystal diamond with dimensions of 3 mm × 3 mm × 0.25 mm, roughness of double-sided polishing, Ra < 30 nm, boron impurity concentration < 0.05 ppm, and nitrogen impurity concentration < 1 ppm.
[0051] Comparative Example: This example is different from Example 1 in that step 4 of the diamond surface indium nanoparticle preparation process is not performed.
[0052] Characterization and testing: A scanning electron microscope was used to characterize the surface of the detector in the experimental group to confirm whether the indium nano-islands were successfully plated; and the ultraviolet detection spectral response rates of the diamond ultraviolet detectors of the embodiment and the comparative embodiment were characterized and compared.
[0053] like Figure 1 As shown in the figure, indium nano-islands with a diameter of 20 to 30 nm and almost uniform size can be clearly observed. Figure 2 As shown in the figure, under the measured wavelength, the spectral response rate of the detector of the embodiment is higher than that of the detector of the comparative experimental group as a whole, especially in the deep ultraviolet region, where the contrast is very obvious. Under 215nm illumination, the spectral response rate of the detector of the embodiment and the comparative embodiment is most obvious, achieving a leap of 2 orders of magnitude. Under 215nm illumination, the response rate of the detector of the embodiment is about 2.94×10 – 3 Under 500nm illumination, the spectral response rates of the detectors of the embodiment and the comparative embodiment are relatively close, from which it can be seen that the ultraviolet / visible light (215nm / 500nm) suppression ratio of the detector of the embodiment is significantly enhanced compared with that of the comparative embodiment. Figure 3 As shown in the figure, the dark currents of the two detectors are almost the same, while the photocurrent enhancement is very obvious. Under 215nm light, the detector current of the embodiment reaches 1.12×10 – 9 A.
Claims
1. A method for improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles, characterized in that The method for improving the ultraviolet detection performance of diamond is implemented according to the following steps:
1. Acid-boiled samples: The autoclave is filled with mixed acid, the intrinsic single crystal diamond is immersed in the mixed acid, and heated at 120°C to 160°C for 2 to 4 hours to obtain diamond with oxygen termination; 2. Sample cleaning: Using acetone, anhydrous ethanol and deionized water in sequence to ultrasonically clean the diamond with oxygen terminals to obtain cleaned diamond; 3. Preparation of Ohmic Contact Electrode: The titanium layer and the gold layer were sputtered on the cleaned diamond surface in sequence by magnetron sputtering to form interdigital electrodes. The thickness of the sputtered titanium layer was 20 nm and the thickness of the gold layer was 30 nm. −4 Pa vacuum, annealing at 400-600°C to obtain ohmic contact diamond; 4. Preparation of Indium Nanoparticles on Diamond Surface: An anodic aluminum mask is set on the surface of the ohmic contact diamond. A through hole is opened on the anodic aluminum mask. Indium nano-islands are plated on the ohmic contact diamond surface by thermal evaporation of indium. The diameter of the indium nano-islands is 20 to 30 nm, thereby improving the ultraviolet detection performance of diamond through the localized surface plasmon resonance of indium nanoparticles. In step three, the interdigitated electrode has 6 to 10 electrodes, and the finger width is 100 to 150 μm.
2. The method for improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles according to claim 1, characterized in that In step 1, the mixed acid is composed of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:
1.
3. The method of improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles according to claim 1, characterized in that In step 1, the mixture is heated at 150° C. for 2 hours.
4. The method of claim 1 for improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles, characterized in that The ultrasonic cleaning time in step 2 is 15 to 30 minutes each time.
5. The method for improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles according to claim 1, characterized in that In step 3, annealing is performed at 500° C. for 30 minutes.
6. The method of claim 1 for improving the ultraviolet detection performance of diamond by using localized surface plasmon resonance of indium nanoparticles, characterized in that The process of thermal evaporation of indium in step 4 is to place elemental indium into an electron beam evaporation device and control the heating current to 46~52A.