A kind of adsorbent for removing heavy metals from waste gas and preparation method thereof

By modifying and activating industrial waste to form porous adsorbents, the problem of easy loss of adsorbents in high-temperature exhaust gases and complex and high-cost preparation is achieved, and high-efficiency, low-cost adsorption of various heavy metals is achieved.

CN116078343BActive Publication Date: 2024-10-08SHANGHAI LANKE PETROCHEM ENG & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211566549.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-10-08
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

Existing adsorbents are easily lost in high-temperature exhaust gases, have low adsorption efficiency, complex preparation processes and high costs, making it difficult to effectively remove a variety of heavy metals.

Method used

Industrial waste containing silicon and aluminum oxides is used as raw material, and an adsorbent with a porous structure is formed at room temperature through modification and activation. It is combined with modifiers such as alkali metal hydroxide or phosphoric acid to form an adsorbent with a high specific surface area, which avoids This eliminates the easy loss of surface active ingredients and simplifies the preparation process.

Benefits of technology

It improves the adsorption efficiency and selectivity, reduces the preparation energy cost, ensures the stability and mechanical strength of the adsorbent under high temperature conditions, and is suitable for the coordinated removal of multiple heavy metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116078343B_ABST
    Figure CN116078343B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing an adsorbent for removing heavy metals from waste gas, comprising the following steps: grinding and screening industrial waste raw materials containing silicon aluminum oxides to micron-sized solid powder raw materials after pretreatment to remove impurities and moisture; mixing the solid powder raw materials with a modifier in proportion, stirring the reaction to form an amorphous polymer, and condensing and hardening the polymer into a mold; washing and drying the hardened product after molding, and then continuously curing it at a constant temperature to obtain an adsorbent module, and then performing crushing, grinding, and screening steps to prepare a micron-sized adsorbent. The present invention selects industrial waste containing target active components, performs modification and activation, and can convert industrial waste into a new type of adsorbent with a porous structure and a high specific surface area, and the industrial waste has high mechanical strength and high temperature resistance, so that the adsorbent is not easy to be lost under the condition of high-temperature waste gas. At the same time, the preparation method of the adsorbent is relatively simple and the energy consumption cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste gas adsorption treatment, and in particular to an adsorbent for removing heavy metals from waste gas and a preparation method thereof. Background Art

[0002] At present, other industrial industries such as petrochemicals and coal chemical industry will produce waste gas containing heavy metals such as mercury, lead, arsenic, chromium, etc. during the use of metal catalysts. Existing waste gas incineration treatment measures cannot remove such heavy metal substances. They can be released through waste gas emissions, but the waste gas will seriously threaten the surrounding environment and human health in the atmospheric environment. Existing pretreatment methods, such as water washing methods, will lead to the generation of a large amount of heavy metal wastewater, and its secondary treatment cost is high. Therefore, the use of adsorption method to capture heavy metals in waste gas has become one of the main methods for controlling heavy metal pollution. And efficient adsorption materials are the most critical core issue. Traditional adsorbents such as activated carbon, although they have strong adsorption capacity, are very limited in their application in removing heavy metals from waste gas due to their high price and weak selectivity. In recent years, non-activated carbon solid adsorbents have also received widespread attention, mainly molecular sieves, resin adsorbents, etc. However, the non-activated carbon solid adsorbents currently on the market have problems such as complex preparation and modification processes, high production costs, and unsatisfactory adsorption efficiency.

[0003] In view of the above problems and characteristics of the release of waste gas containing heavy metals, the selection of adsorption process and adsorbent needs to be determined in combination with the upstream production process and the characteristics of heavy metals in the waste gas, and the adsorption amount, adsorption rate, selectivity and material cost of the adsorbent need to be considered. Finding clean, efficient, cheap and environmentally friendly adsorbents is a hot topic in the research of heavy metal flue gas treatment at home and abroad.

[0004] Chinese patent document CN 106861633B provides a method for preparing a chromium adsorbent, using fly ash, microsilica, rice husk ash, diatomaceous earth and other industrial and agricultural waste as raw materials, and using cationic surfactants as templates to synthesize porous organic-inorganic composite materials at room temperature for adsorbing Cr(VI) in wastewater. Although the synthesis process of this patent can be completed at room temperature, the raw materials need to be calcined at high temperature (400-700°C) to obtain an activated silicon source, which is time-consuming and has high energy consumption costs.

[0005] Chinese patent document CN 112138637B provides an adsorbent for simultaneously removing heavy metals and VOCs from waste gas and a preparation method thereof, wherein zinc-modified carbon nanotubes are modified with γ-methacryloxypropyltrimethoxysilane to obtain modified carbon nanotubes; then the modified carbon nanotubes are reacted with trimethylolpropane tris(3-mercaptopropionate) to obtain thiolated carbon nanotubes; then the thiolated carbon nanotubes are mixed with polyethersulfone resin, melt-spun to obtain composite fibers, which are cut into short fibers of 1 to 2 mm; finally, the short fibers are mixed with acrylamide and N-(4-aminophenyl)acrylamide to undergo polymerization reaction to obtain an adsorbent. Although the adsorbent has a good removal effect on heavy metals and VOCs in waste gas (chromium ion removal rate is about 99%), the preparation steps are relatively complicated and the preparation cost is relatively high.

[0006] Chinese patent document CN 112156750 B provides a method for preparing a fly ash carrier heavy metal adsorbent, wherein kaolin powder, Fe powder, and Ca powder are mixed with the fly ash particles, stirred evenly, and calcined at high temperature, and then cooled to obtain an adsorbent. The adsorption capacities of cadmium and lead are tested to be 16 mg / g and 21 mg / g, respectively. This method uniformly solidifies kaolin, Fe, and Ca powders on the surface of fly ash particles by physical blending-high temperature calcination. Although the active components on the surface improve the adsorption efficiency, there is a problem that after the adsorbent is used, the surface active components are reduced, resulting in a decrease in adsorption efficiency.

[0007] Chinese patent document CN 101876087B provides a method for preparing calcium sulfate whiskers for adsorbing heavy metal ions in waste incineration flue gas. The unmodified calcium sulfate whiskers are obtained by uniformly mixing gypsum raw materials with water and filtering them. The unmodified calcium sulfate whiskers are then soaked in alkaline solution, dried, and activated at high temperature (600-900°C) to obtain modified calcium sulfate whisker adsorbent. After testing, the heavy metal removal rate is 95% (cadmium ions) and 94% (lead ions). The patent increases the pH value of the surface of calcium sulfate whiskers by soaking in alkaline solution, thereby enhancing the adsorption of heavy metal ions. However, there is a problem that the adsorption efficiency is reduced after the surface alkalinity is consumed, and the preparation process requires microwave reactor heating to increase the crystallization reaction rate. The modification process requires high temperature (600-900°C) under anaerobic conditions to activate the whisker surface. Although the cost of gypsum raw materials is low, the energy consumption cost of its whisker preparation process is high.

[0008] The adsorbent prepared in the above-mentioned prior art has a relatively high adsorption capacity for heavy metals in exhaust gas, and its characteristic is that the adsorption efficiency of the adsorbent is improved by modifying the surface of the adsorbent. However, the active components on the surface of the adsorbent prepared by this method are easily worn and consumed during the adsorption of heavy metals in high-temperature exhaust gas, which will indirectly lead to problems such as reduced adsorption efficiency and frequent replacement of adsorbents.

[0009] Moreover, the adsorbent provided by the above patent technology requires high-temperature roasting, long-term curing and multiple modification and functionalization operations during the preparation process, which has the disadvantages of long time consumption, numerous operation steps and high preparation cost. In addition, there are currently few patents related to the preparation and application of adsorbents for the adsorption of heavy metals in waste gas.

[0010] Based on this, it is necessary to provide a new adsorbent for removing heavy metals from waste gas and its preparation method to address the current application defects of the adsorbent surface modification that is easy to wear, resulting in reduced adsorption efficiency, as well as the complex preparation method and high preparation cost of the adsorbent. Summary of the invention

[0011] The purpose of the present invention is to provide an adsorbent for removing heavy metals from waste gas and a preparation method thereof, which effectively solves the technical defects of the current heavy metal waste gas adsorption treatment device, which has a relatively simple structure and function and a low heavy metal adsorption efficiency; at the same time, it solves the problem that the adsorbent is easily blocked. Specifically, by selecting industrial waste containing target active components, the required adsorbent raw material powder is obtained by screening, and the modifier corresponding to the heavy metal adsorption target is selected. The adsorbent raw material powder and the modifier are mixed and reacted, and activated and cured at room temperature to prepare the required new adsorbent. This modification and activation process can convert industrial waste into a new adsorbent with a porous structure and a high specific surface area, and its mechanical strength and high temperature resistance are high, so that the adsorbent has good stability under high temperature waste gas conditions. At the same time, the preparation method of the adsorbent is relatively simple and the energy consumption cost is low. In addition, the new adsorbent integrates multiple active components, which significantly improves the adsorption efficiency compared with traditional activated carbon adsorbents, and its multi-selective characteristics solve the technical problem of synergistic removal of multiple heavy metals.

[0012] The technical solution adopted by the present invention to solve its technical problem is:

[0013] A method for preparing an adsorbent for removing heavy metals from exhaust gas comprises the following steps:

[0014] The industrial waste raw materials containing silicon aluminum oxide are pre-treated to remove impurities and moisture, and then ground and sieved into micron-sized solid powder raw materials;

[0015] The solid powder raw material and the modifier are mixed in proportion, stirred to react to form an amorphous polymer, and then coagulated and hardened to form;

[0016] The hardened product after molding is cleaned and dried, and then continuously solidified at a constant temperature to obtain an adsorbent module, which is then crushed, ground, and sieved to produce a micron-sized adsorbent.

[0017] Preferably, for the pretreated raw material, by mass percentage, the solid powder raw material accounts for 69-75.2%, and the modifier accounts for 24.8-31%.

[0018] Preferably, the oxide component ratios of the industrial solid waste raw materials are SiO2: 30-60%, Al2O3: 15-30%, CaO: 1-15%, and Fe2O3: 0.5-10%.

[0019] Preferably, the industrial solid waste raw material includes waste molecular sieve and fly ash, wherein the mass ratio of waste molecular sieve to fly ash is 0.4 to 2.5, so as to maintain the Si / Al molar ratio in the raw material at 2 to 3.5.

[0020] Preferably, the modifier is selected from one or a mixture of any two or more of alkali metal hydroxides, silicates, carbonates, bicarbonates, phosphoric acid, sulfuric acid and hydrogen peroxide.

[0021] Preferably, the modifier is sodium hydroxide, and the concentration of its solution is controlled at 9-12M; or, the modifier is phosphoric acid, and the concentration of its solution is controlled at 9-11M.

[0022] Preferably, sodium silicate is added to the modifier, wherein the mass percentage of sodium silicate in the total mass percentage of the modifier is 0 to 66.7%.

[0023] Preferably, a foaming agent is added to the modifier, wherein the foaming agent accounts for 0 to 3.3% of the total mass of the modifier.

[0024] Preferably, the coagulation and hardening is carried out at room temperature and pressure, and the hardening time is about 18 to 24 hours;

[0025] The hardened product is placed in a constant temperature box at 35-55° C. and continuously cured (≥72 hours) under the condition of humidity>50%.

[0026] According to another aspect of the present invention, there is also provided an adsorbent for removing heavy metals from exhaust gas prepared according to the above preparation method, wherein the specific surface area of ​​the adsorbent is 50.25 to 83.65 m 2 / g.

[0027] Compared with the adsorbent preparation methods provided in the prior art, which are all surface modification methods, the preparation method of the present invention does not belong to the category of surface modification. Its adsorption sites exist not only on the surface, but also mostly in the internal pore structure of the adsorbent, thus avoiding the defects of the traditional adsorbent surface active components after use, such as reduced active components and easy loss. Specifically, at least the following beneficial effects are achieved:

[0028] 1) The present invention uses industrial waste containing aluminosilicate as raw material. The silicon aluminum oxide component in the raw material can be modified and activated to form a new adsorption material with a porous structure. At the same time, other active components in the industrial waste (such as CaO, Fe2O3, etc.) can be effectively solidified on the pore structure and surface of the adsorbent. These active components can also provide adsorption reaction sites for various heavy metals in the waste gas, solving the problem of synergistic removal of various heavy metals in the waste gas. In addition, the increasing industrial waste in the process of industrial production development is fully utilized to maximize the resource utilization of industrial waste.

[0029] 2) The modifier used in the present invention not only has the function of changing the original aluminosilicate structure in the raw material and increasing the porosity, but also the acid / base properties of the modifier itself can be targeted at different types of heavy metals (cationic and anionic). In this way, while ensuring that the adsorbent forms a porous structure, the selectivity of the adsorbent is improved, which is beneficial to the separation and purification of different types of heavy metals in the exhaust gas.

[0030] 3) The curing temperature of the present invention is low, which is 25°C to 55°C. Under this non-high temperature working condition, the dispersion and activation of other active components such as silicon and aluminum in the raw materials can be ensured, which not only meets the adsorbent index requirements, but also greatly reduces the energy consumption cost in the preparation process.

[0031] 4) The preparation method of the heavy metal adsorbent of the present invention can control the adsorption performance of the adsorbent by adjusting the ratio of raw material components and the composition of the modifier. The method is simple to operate, easy to control, and has a low raw material cost, which makes the preparation process more flexible. It is beneficial to improve the removal efficiency of different heavy metals in waste gas under different working conditions or different waste gas conditions by simply replacing the adsorbent. At the same time, it expands the application scope of the adsorbent product and is suitable for industrial promotion.

[0032] 5) The adsorbent product prepared by the present invention has good thermal stability and mechanical strength, which solves the problem of secondary pollution caused by fine particles produced by traditional adsorbents when broken, and avoids the problems of adsorbent loss and surface deactivation under high-temperature gasification conditions.

[0033] In summary, the preparation process of the present invention is simple, the energy consumption cost of preparation is low, the raw materials are widely available and cheap, and the scale productivity is high. The prepared heavy metal adsorbent has a high specific surface area and a developed pore structure, and can effectively adsorb heavy metal ions in exhaust gas. The adsorption effect is equivalent to that of activated carbon. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0035] Figure 1 is a flow chart of the method for preparing the adsorbent of the present invention;

[0036] Figure 2aThe solidified adsorbent module (64 mm 3 ) The finished product picture of the sample; Figure 2b The adsorbent particles (d 50 =1mm) sample's actual finished product picture.

[0037] Figure 3a This is a SEM photo of the heavy metal adsorbent product of the present invention; Figure 3b This is a SEM photograph of the adsorbent of the present invention after adsorbing heavy metals. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0039] The term "heavy metals" used in this article refers to heavy metals suspended in various gaseous media in industrial exhaust gases, including arsenic, selenium, lead, chromium, chromium, etc., such as heavy metals on fine particles, heavy metals attached to aerosol particles, and heavy metal vapors.

[0040] The term "industrial solid waste" used in this article refers to solid waste with aluminosilicates as the main components, including waste molecular sieve catalysts, fly ash, slag, etc., among which silicon and aluminum oxides are the main components of such adsorbents.

[0041] With the continuous development of my country's industrial production, the number and types of industrial waste are increasing. If they are not managed scientifically, the toxic and harmful components in them will pollute the environment and endanger human health, and cause the loss of solid waste resources. Such as fly ash produced by coal-fired power plants, slag and steel slag discharged from iron and steel making and other smelting processes, waste molecular sieve catalysts produced in petrochemical catalytic processes, etc. The present invention uses an economical and effective method to make full use of the large amount of active components contained in industrial waste. After activation and modification, it has a very obvious application prospect as a raw material for composite adsorbents, and at the same time maximizes the resource utilization of industrial waste. Figure 1 A method for preparing an adsorbent for removing heavy metals from exhaust gas is shown as a preferred embodiment, which comprises the following steps:

[0042] The industrial waste raw materials containing silicon aluminum oxide are pre-treated to remove impurities and moisture, and then ground and sieved into micron-sized solid powder raw materials;

[0043] The solid powder raw material and the modifier are mixed in proportion, stirred to react to form an amorphous polymer with a high specific surface area, and solidified and hardened to form;

[0044] The hardened product after molding is cleaned and dried, and then continuously solidified at a constant temperature to obtain an adsorbent module, which is then crushed, ground, and sieved to produce a micron-sized adsorbent.

[0045] Based on the present embodiment, industrial solid waste containing aluminosilicates is used as raw material, and the silicon aluminum oxide component in the raw material can be modified and activated to form a new adsorption material with a porous structure. At the same time, other active components in the industrial solid waste (such as CaO, Fe2O3, etc.) can be effectively solidified on the pore structure and surface of the adsorbent. These active components can also provide adsorption reaction sites for various heavy metals in the exhaust gas, solving the problem of synergistic removal of various heavy metals in the exhaust gas, and realizing the simple, low-cost and high-efficiency preparation of heavy metal adsorbents.

[0046] Preferably, the oxide component ratios of the industrial solid waste raw materials are SiO2: 30-60%, Al2O3: 15-30%, CaO: 1-15%, and Fe2O3: 0.5-10%.

[0047] The industrial solid waste raw materials include waste molecular sieve and fly ash, wherein the mass ratio of the waste molecular sieve to the fly ash is 0.4-2.5, so as to maintain the Si / Al molar ratio in the raw materials at 2-3.5.

[0048] By selecting suitable industrial solid waste raw materials and blending them in different proportions within a certain range, the pore structure and active component content of the adsorbent can be pre-controlled within an appropriate range; the modifier can activate the aluminosilicate components in the industrial solid waste and evenly disperse other active components inside and on the surface of the pore structure of the adsorbent when a relatively small amount of the modifier is used.

[0049] For the raw materials after pretreatment, the solid powder raw materials account for 69-75.2% by mass, and the modifier accounts for 24.8-31%. By controlling the mass ratio of the modifier solution to the solid powder raw materials to be 0.33-0.45 (liquid-to-solid ratio), it is beneficial to the cohesive structure of the mixed slurry and its strength after hardening, while ensuring the strength and durability of the adsorbent.

[0050] The pretreatment of the industrial waste raw materials is: grinding, screening, washing, and drying in sequence. The pretreatment includes the steps of grinding, screening, washing, and drying, and the process is mainly to remove impurities and moisture in the raw materials; specifically, the raw materials are screened with 100 mesh, washed with clean water or weak acid to remove impurities generated during screening, and then dried at 105°C for 24 hours to remove residual moisture.

[0051] As another preferred embodiment, the modifier is selected from one or a mixture of any two or more of alkali metal hydroxides, silicates, carbonates, bicarbonates, phosphoric acid, sulfuric acid and hydrogen peroxide, etc., with the purpose of configuring different modifiers in proportion to make the mixed solution have strong alkalinity or strong acidity. Although the modifiers described in this article are all inorganic modifiers, the method is not limited to using other organic modifiers, and the purpose is to promote the formation of a porous structure of the adsorbent, improve the mechanical strength of the adsorbent, and improve the adsorption selectivity of different pollutants.

[0052] The modifier is sodium hydroxide, and the concentration of the solution is controlled at 9-12M (molar concentration). By controlling the concentration range, on the one hand, it is more conducive to the structural reorganization of the aluminosilicate in the raw material under relatively high concentration alkaline conditions, and on the other hand, it avoids the side effect of excessive alkalinity that destroys the pore structure of the adsorbent. After the alkaline modification within this parameter range, the negative charge on the surface of the adsorbent increases and is evenly dispersed over a large area on the pore surface, which is conducive to the cationic heavy metal (Pb 2+ 、Cd 2+ It should be noted that the prior art uses the sodium ions in the sodium salt to compete with the sodium ions in the clay containing aluminosilicates, thereby inhibiting the hydration expansion of the clay. However, the added sodium salt component cannot affect the crystal structure of the aluminosilicate.

[0053] Alternatively, the modifier is phosphoric acid, and the concentration of the solution is controlled at 9-11M. By controlling the concentration range, a high-strength porous adsorbent is produced under relatively high concentration acidic conditions, and the positive charge on the surface of the acid-modified adsorbent is increased and evenly dispersed over a large area on the pore surface, which is beneficial to the adsorption of anionic heavy metals (Cr2O7 2- etc.) adsorption effect.

[0054] The modifier provided in this embodiment produces an interactive effect of co-building a skeleton on the crystal structure of the aluminosilicate, promotes the formation of a porous structure of the adsorbent, increases the specific surface area of ​​the adsorbent, and is beneficial to the adsorption of the pore structure.

[0055] In order to improve the industrial production value, sodium silicate is added to the modifier, wherein the sodium silicate accounts for 0-66.7% of the total mass percentage of the modifier. When the modifier solution is ensured to be strongly alkaline or strongly acidic, a silicon source is added to improve the mechanical strength of the adsorbent product.

[0056] In addition, a foaming agent can be added to the modifier, wherein the foaming agent accounts for 0-3.3% of the total mass of the modifier. The foaming agent is sodium bicarbonate or hydrogen peroxide with a mass concentration of 2-5wt%, and its function is to improve the porous structure of the adsorbent by using the foaming principle.

[0057] In the process of mixing the solid powder raw material and the modifier in proportion, first add the sodium hydroxide solution, stir at a low speed of 50rpm for 2 to 3 minutes, then add the sodium silicate solution, stir at a low speed of 50rpm for 2 to 3 minutes, stir at a high speed of 100rpm for 1 to 2 minutes, and finally add the sodium bicarbonate solution, stir at a high speed of rpm for 1 to 2 minutes. In this way, the dual effect of synergistically improving the mechanical and adsorption properties of the adsorbent product is achieved.

[0058] In addition, the condensation hardening is carried out at room temperature and pressure, and the hardening time is about 18 to 24 hours; during this process, the raw materials and the modifiers continue to undergo activation reactions, which is conducive to the formation of a porous structure inside the adsorbent. Furthermore, the hardened product needs to be placed in a 35-55°C constant temperature box and continuously cured for at least 3 days under the condition of humidity >50%, which is conducive to improving the compressive strength and durability of the adsorbent.

[0059] Using the above-mentioned embodiment, an adsorbent can be prepared, especially an adsorbent for removing heavy metals in exhaust gas, which is a process in which industrial solid waste containing silicate is pretreated by the "modification activation" method and then evenly mixed with a modifier, and activated under non-high temperature conditions to form a porous structure adsorbent after solidification.

[0060] The specific surface area of ​​industrial waste raw materials is about 1 to 5 m 2 / g, the specific surface area of ​​the adsorbent prepared by the modified activation treatment of the present invention is 50.25-83.65m 2 / g. It has excellent application effect in heavy metal adsorption, and of course it can also be applied to other types of solid waste adsorption. In addition, the present invention has the characteristics of low production cost, short preparation cycle, easy operation, and batch production.

[0061] Several specific embodiments are provided below. First, the corresponding adsorbent is prepared according to the following specific process:

[0062] S1. Selecting industrial solid waste containing aluminosilicate as raw material and analyzing the proportion of different oxide components in the raw material to screen and obtain the required industrial solid powder waste as adsorbent raw material;

[0063] S2, pre-treating the industrial solid powdery waste raw material screened out in step S1, including grinding, screening, washing, drying and other steps, so as to remove impurities and moisture in the raw material and obtain a solid powdery raw material;

[0064] S3, uniformly mixing the solid powdered raw material pretreated in step S2 with the modifier in a certain proportion, and forming a slurry-like mixed material after stirring for 5 to 10 minutes, and modifying and adjusting the material structure;

[0065] S4, placing the slurry prepared in step S3 into a mold of a fixed shape, solidifying it, and demolding it after forming to obtain a hardened product;

[0066] S5, after cleaning the residual modifier on the surface of the hardened product obtained in step S4, naturally dry it, and continue to activate it at a constant temperature for at least 3 days to obtain a solid adsorbent module; such as 64mm 3 The shape of the adsorbent module made by the cubic mold is shown in Figure 2(a).

[0067] S6. The adsorbent module obtained in step S5 is crushed and sieved to obtain a granular adsorbent or powdered adsorbent or other adsorbents in specific shapes for adsorbing heavy metal ions in exhaust gas. For example, the shape of a granular adsorbent with a particle size of about 1 mm is shown in FIG2(b).

[0068] The following specific embodiments are formed and corresponding tests are performed:

[0069] Example 1

[0070] In this example, waste molecular sieves (with components of 55% SiO2, 17% Al2O3, 0.2% CaO, 0.2% Fe2O3, etc.) were selected as raw materials. After the selected raw materials were pre-treated by grinding, screening (100-200 mesh sieve), washing, and drying, a fine powder raw material with a certain particle size was obtained, which was the solid powder raw material; and the solid raw material powder raw material with an average particle size of less than 100μm was weighed; solid sodium hydroxide was added to water to prepare a 10M sodium hydroxide solution as a modifier. Add the configured modifier to the waste molecular sieve powder and stir evenly for 5 minutes. Control the stirring rate to 50-100rpm, and form a slurry after sufficient reaction. The mass ratio of the pre-treated waste molecular sieve solid powder raw material and the 10M sodium hydroxide modifier is 70% and 30% (liquid-to-solid ratio is 0.43). Pour the slurry into a 40x40x40mm 3 The mold is sealed and placed in a room with a humidity of ≥50% for 24 hours for curing at room temperature to solidify. After 24 hours, the mold is taken out and demoulded. The solid product after demoulding is rinsed with clean water to remove the residual modifier on the surface and dried naturally, and then placed in an insulated box for curing at 50°C for 3 days. The solidified solid product is crushed and sieved into granules or powdered adsorbents of different particle sizes. The adsorbent for adsorbing heavy metal ions in exhaust gas of the present invention is obtained, and it is sealed and packaged for standby use after cooling.

[0071] In the heavy metal adsorption experiment in the tail gas of a catalytic device of a petrochemical enterprise, the exhaust gas temperature is 50-150°C and the exhaust gas flow rate is 500Nm 3 / h, the exhaust gas contains chromium, cadmium and lead, with a concentration of about 1-5 mg / Nm 3 , the heavy metal adsorbent prepared by the above method is selected.

[0072] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0073] Example 2

[0074] In this embodiment, except that the formula is replaced by waste molecular sieve raw material and 10M sodium hydroxide modifier with a mass ratio of 75.2% and 24.8% (liquid-to-solid ratio of 0.33), everything else is the same as Example 1.

[0075] Example 3

[0076] In this embodiment, except that the formula is replaced by waste molecular sieve raw material and 10M sodium hydroxide modifier with a mass ratio of 73% and 27% (liquid-to-solid ratio of 0.37), everything else is the same as Example 1.

[0077] Example 4

[0078] In this embodiment, except that the formula is replaced by waste molecular sieve raw material and 10M sodium hydroxide modifier with a mass ratio of 71.5% and 28.5% (liquid-to-solid ratio of 0.40), everything else is the same as Example 1.

[0079] Example 5

[0080] In this embodiment, except that the formula is replaced by waste molecular sieve raw material and 10M sodium hydroxide modifier with a mass ratio of 69% and 31% (liquid-to-solid ratio of 0.45), everything else is the same as Example 1.

[0081] Example 6

[0082] In this embodiment, except that the waste molecular sieve in the raw material is replaced by fly ash at a ratio of 100%, the rest is the same as in Example 1. The fly ash raw material components added are 50.52% SiO2, 28.59% Al2O3, 3.82% CaO, 6.96% Fe2O3, etc. The mass ratio of the fly ash solid powder raw material and the 10M sodium hydroxide modifier is 70% and 30%.

[0083] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0084] Example 7

[0085] In this embodiment, except that 28.57% of the waste molecular sieve in the raw material is replaced by fly ash in the same proportion, the rest is the same as in Example 1. The added fly ash raw material components are 50.52% SiO2, 28.59% Al2O3, 3.82% CaO, 6.96% Fe2O3, etc. The mass ratios of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material, and the 10M sodium hydroxide modifier are 50%, 20%, and 30%.

[0086] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0087] Example 8

[0088] In this embodiment, except that 50% of the waste molecular sieve in the raw material is replaced by fly ash in the same proportion, the rest is the same as in Example 1. The fly ash raw material components added are 50.52% SiO2, 28.59% Al2O3, 3.82% CaO, 6.96% Fe2O3, etc. The mass ratios of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material, and the 10M sodium hydroxide modifier are 35%, 35%, and 30%.

[0089] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0090] Example 9

[0091] In this embodiment, except that 71.43% of the amount of waste molecular sieve in the raw material is replaced by fly ash in the same proportion, the rest is the same as in Example 1. The fly ash raw material components added are 50.52% SiO2, 28.59% Al2O3, 3.82% CaO, 6.96% Fe2O3, etc. The mass ratios of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material, and the 10M sodium hydroxide modifier are 20%, 50%, and 30%.

[0092] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0093] Example 10

[0094] In this embodiment, except that the modifier is completely replaced by sodium silicate, everything else is the same as in Example 9. The composition of the sodium silicate solution is 26.5% SiO2 and 10.6% Na2O. The mass ratios of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material and the sodium silicate solution are 20%, 50% and 30% respectively.

[0095] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0096] Embodiment 11

[0097] In this embodiment, except that 2 / 3 of 10M sodium hydroxide in the modifier is reduced and replaced with sodium silicate in the same proportion, the rest is the same as in Example 9. The components of the sodium silicate solution are 26.5% SiO2 and 10.6% Na2O. The mass ratios of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material, the 10M sodium hydroxide and the sodium silicate solution are 20%, 50%, 10% and 20%.

[0098] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0099] Example 12

[0100] In this embodiment, except that 1 / 2 of the 10M sodium hydroxide in the modifier is reduced and replaced with sodium silicate in the same proportion, the rest is the same as in Example 9. The components of the sodium silicate solution are 26.5% SiO2 and 10.6% Na2O. The mass ratios of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material, the 10M sodium hydroxide and the sodium silicate solution are 20%, 50%, 15% and 15%.

[0101] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0102] Example 13

[0103] In this embodiment, except that 1 / 3 of the 10M sodium hydroxide in the modifier is reduced and replaced with sodium silicate in the same proportion, the rest is the same as in Example 9. The components of the sodium silicate solution are 26.5% SiO2 and 10.6% Na2O. The mass ratios of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material, the 10M sodium hydroxide and the sodium silicate solution are 20%, 50%, 20% and 10%.

[0104] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0105] Embodiment 14

[0106] In this embodiment, except that 1 / 3 of the 10M sodium hydroxide in the modifier is reduced and replaced with sodium silicate and hydrogen peroxide in the same proportion, the rest is the same as in Example 4. The components of the sodium silicate solution are 26.5% SiO2 and 10.6% Na2O; the concentration of hydrogen peroxide is 5%. The mass proportions of the waste molecular sieve solid powder raw material, the fly ash solid powder raw material, 10M sodium hydroxide, sodium silicate and hydrogen peroxide are 20%, 50%, 20%, 9% and 1%.

[0107] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0108] Embodiment 15

[0109] In this embodiment, except that the modifier is replaced by 10M phosphoric acid solution, everything else is the same as in Example 1. 10M phosphoric acid solution is prepared by adding concentrated phosphoric acid to water.

[0110] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0111] Example 16

[0112] In this embodiment, except that the modifier is replaced by 10M phosphoric acid solution, everything else is the same as in Example 6. 10M phosphoric acid solution is prepared by adding concentrated phosphoric acid to water.

[0113] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0114] Embodiment 17

[0115] In this embodiment, except that the modifier is replaced by 10M phosphoric acid solution, everything else is the same as in Example 7. 10M phosphoric acid solution is prepared by adding concentrated phosphoric acid to water.

[0116] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0117] Embodiment 18

[0118] In this embodiment, except that the modifier is replaced by 10M phosphoric acid solution, everything else is the same as in Example 8. 10M phosphoric acid solution is prepared by adding concentrated phosphoric acid to water.

[0119] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0120] Embodiment 19

[0121] In this embodiment, except that the modifier is replaced by 10M phosphoric acid solution, everything else is the same as in Example 9. 10M phosphoric acid solution is prepared by adding concentrated phosphoric acid to water.

[0122] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0123] Embodiment 20

[0124] In this embodiment, except that the modifier is replaced by 10M phosphoric acid solution, everything else is the same as that of embodiment 13. 10M phosphoric acid solution is prepared by adding concentrated phosphoric acid to water.

[0125] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0126] Embodiment 21

[0127] Except that the modifier is replaced by 10M phosphoric acid solution, the other aspects of this embodiment are the same as those of embodiment 14. 10M phosphoric acid solution is prepared by adding concentrated phosphoric acid to water.

[0128] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0129] Comparative Example 1

[0130] This example is basically the same as Example 9, except that the modifier is replaced with 12.5M sodium hydroxide.

[0131] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0132] Comparative Example 2

[0133] This example is basically the same as Example 9, except that the modifier is replaced with 8.5M sodium hydroxide.

[0134] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0135] Comparative Example 3

[0136] This example is basically the same as Example 19, except that the modifier is replaced with 11.5M phosphoric acid.

[0137] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0138] Comparative Example 4

[0139] This example is basically the same as Example 19, except that the modifier is replaced with 8.5M phosphoric acid.

[0140] The raw material dosage, modifier configuration ratio and adsorption rate results are shown in Table 1.

[0141] Table 1 The addition ratio of raw materials and modifiers and the removal rate of heavy metals in waste gas (100-300℃)

[0142]

[0143]

[0144]

[0145] In addition, the present invention uses a scanning electron microscope to characterize the modified and activated adsorbent product and the product after heavy metal adsorption. Figure 3a As shown in the figure: the modified and activated product has obvious spherical particles with a rough surface and is surrounded by a large amount of flocculent material. The partial reticular structure indicates that the modifier has successfully activated and reorganized the aluminosilicate structure in the raw materials (fly ash, waste molecular sieve, etc.). Figure 3b As shown: after the adsorption of heavy metal waste gas, the spherical particle structure on the adsorbent is heavily covered with a layer of metal compounds inside and on the surface, indicating that the heavy metal is firmly adsorbed in the internal pore structure and surface of the adsorbent and will not fall off due to gas impact, thereby avoiding the mutual wear between the adsorbent particles and the loss of surface active components caused by the impact of the adsorbent particles when the waste gas passes through the adsorbent bed. It is calculated that the adsorption capacity of this new type of adsorbent for heavy metals in waste gas is about 28-34 mg / g.

[0146] Combined with Table 1, it can be seen that for different heavy metals, different property modifiers can be selected as "modification activation" agents to obtain selective heavy metal adsorbents. Moreover, the specific surface area in Table 1 can show that the pore structure of the adsorbent prepared by the present invention is relatively good, and it also proves that the present invention forms abundant adsorption sites in the internal pore structure and has high mechanical strength (compressive strength).

[0147] The above-mentioned ideal embodiments of the present invention are for inspiration. Through the above-mentioned description, relevant staff can make various changes and modifications without departing from the technical idea of ​​the present invention. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing an adsorbent for removing heavy metals from waste gas, It is characterized in that The following steps are included: The industrial waste raw materials containing silicon aluminum oxide are pre-treated to remove impurities and moisture, and then ground and sieved into micron-sized solid powder raw materials; The solid powder raw material and the modifier are mixed in proportion, stirred to react to form an amorphous polymer, and then coagulated and hardened to form; After the hardened product is cleaned and dried, it is continuously cured at a constant temperature to obtain an adsorbent module, which is then crushed, ground, and sieved to produce a micron-sized adsorbent; The coagulation and hardening is carried out at normal temperature and pressure, and the hardening time is 18 to 24 hours; The hardened product is placed in a constant temperature box at 25-55°C and continuously cured for no less than 72 hours under the condition of humidity >50%; For the pretreated raw material, the solid powder raw material accounts for 69-75.2% by mass, and the modifier accounts for 24.8-31% by mass; The industrial solid waste raw materials include waste molecular sieve and fly ash, wherein the mass ratio of the waste molecular sieve to the fly ash is 0.4-2.5, so as to maintain the Si / Al molar ratio in the raw materials at 2-3.5; The modifier is sodium hydroxide, and the concentration of the solution is controlled at 9-12M; or, the modifier is phosphoric acid, and the concentration of the solution is controlled at 9-11M.

2. The method for preparing an adsorbent for removing heavy metals from exhaust gas according to claim 1, Features: The oxide composition ratio of the industrial solid waste raw material is SiO 2 :30~60%,Al 2 O 3 : 15~30%, CaO: 1~15%, Fe 2 O 3 :0.5~10%.

3. The method for preparing an adsorbent for removing heavy metals from exhaust gas according to claim 1, Features: Sodium silicate is added to the modifier, wherein the sodium silicate accounts for 0 to 66.7% of the total mass percentage of the modifier; and / or; A foaming agent is added to the modifier, wherein the foaming agent accounts for 0 to 3.3% of the total mass of the modifier.

4. An adsorbent for removing heavy metals from waste gas, Features: Prepared by the preparation method according to any one of claims 1 to 3, the specific surface area of ​​the adsorbent is 50.25 to 83.65 m2 / g.