CrAlFe-based alloy target and preparation method thereof

Through the vacuum hot-pressing sintering process and high-energy ball milling technology, the cracking problem in the preparation of CrAlFe alloy targets is solved, the density and performance of the targets are improved, and a more uniform microstructure and higher bending strength are achieved.

CN116079055BActive Publication Date: 2024-10-11TARFILM HI-TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310083758.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-08
Publication Date
2024-10-11
Estimated Expiration
2043-02-08

AI Technical Summary

Technical Problem

Severe cracking occurs during the preparation of CrAlFe and CrAlFeX alloy targets, which affects the performance and service life of the targets.

Method used

Using a vacuum hot-pressing sintering process, the pressure is removed before cooling, and the Al powder and Fe powder are processed by high-energy ball milling to form AlFe alloy powder, which is then evenly mixed with Cr powder and other element powders, and hot-pressed and sintered to reduce the brittle alloy phase. of generation.

Benefits of technology

It effectively improves the cracking phenomenon of CrAlFe-based alloy targets, improves the density and structural uniformity of the targets, reduces the residual internal stress, and significantly improves the flexural strength and coating performance of the targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116079055B_ABST
    Figure CN116079055B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of powder metallurgy materials and their manufacturing, and specifically relates to a CrAlFe-based alloy target and a preparation method thereof, the preparation method comprising the following steps: S1, high-energy ball milling Al powder and Fe powder to obtain pre-alloyed AlFe alloy powder; S2, uniformly mixing the AlFe alloy powder and the remaining raw material powder of the CrAlFe-based alloy target to obtain CrAlFe-based alloy powder; S3, hot pressing and sintering the CrAlFe-based alloy powder under vacuum conditions, and after the hot pressing and sintering is completed, the pressure is released, and then the CrAlFe-based alloy sintered blank is cooled and demolded to obtain a CrAlFe-based alloy sintered blank; S4, machining the CrAlFe-based alloy sintered blank to obtain a CrAlFe-based alloy target. The present invention can improve the cracking phenomenon of the CrAlFe-based alloy target by releasing the pressure before cooling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy materials and manufacturing thereof, and specifically relates to a CrAlFe-based alloy target material and a preparation method thereof. Background Art

[0002] Since the 1960s, the deposition of superhard thin film materials on the surface of metal cutting tools through PVD technology can significantly improve cutting speed and wear resistance, extend tool life, and become the main method to improve tool performance. With the continuous development and progress of coating technology, it has developed from the first generation of TiN and CrN coatings to the current AlTiN and AlCrN composite coatings, and gradually tends to be diversified, nano- and multi-layered. By adding Fe elements to the AlCrN coating, the high-temperature oxidation resistance and thermal strength of the film layer can be significantly improved; adding refractory transition metal elements such as W, Mo, Ta, Nb, and V to the AlCrFeN coating can further improve the thermal hardness and high-temperature oxidation resistance of the coating, thereby significantly improving the cutting performance of the tool.

[0003] However, the technical barriers to the preparation of CrAlFe and CrAlFeX (X = one or more of W, Mo, Ta, Nb, V) alloy targets are very high. When prepared by conventional hot isostatic pressing, the target has severe cracking both on the outside and in the core. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a CrAlFe-based alloy target material and a preparation method thereof. The present invention adopts a vacuum hot pressing sintering process to release the pressure before cooling to prepare the CrAlFe-based alloy target material, thereby improving the cracking phenomenon of the CrAlFe-based alloy target material.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a CrAlFe-based alloy target, comprising the following steps:

[0007] S1, subjecting Al powder and Fe powder to high-energy ball milling to obtain pre-alloyed AlFe alloy powder;

[0008] S2. Evenly mixing the AlFe alloy powder and the remaining raw material powder of the CrAlFe-based alloy target to obtain a CrAlFe-based alloy powder, wherein the remaining raw material powder of the CrAlFe-based alloy target is Cr powder or consists of Cr powder and X powder, and the X powder includes at least one of W powder, Mo powder, Ta powder, Nb powder, and V powder;

[0009] S3, hot pressing and sintering the CrAlFe-based alloy powder under vacuum conditions, releasing the pressure after the hot pressing and sintering, and then cooling and demolding to obtain a CrAlFe-based alloy sintered billet;

[0010] S4. Machining the CrAlFe-based alloy sintered blank to obtain the CrAlFe-based alloy target.

[0011] The invention adopts a vacuum hot pressing sintering process to release pressure before cooling to prepare a CrAlFe-based alloy target material, thereby improving the cracking phenomenon of the CrAlFe-based alloy target material.

[0012] The present invention firstly performs high-energy ball milling on Al powder and Fe powder, and then uniformly mixes AlFe alloy powder, Cr powder and X powder, so that metal Fe and Al are fully alloyed to form AlFe alloy powder, effectively avoiding the heat release caused by the intense alloying reaction of pure Al powder and Fe powder, causing the Cr in the target material to react with the matrix Al to generate more brittle alloy phases, ensuring that the brittle alloy phase in the target material is less, and can effectively improve the brittleness of CrAlFe and CrAlFeX alloy target materials and improve the problem of billet cracking.

[0013] In the preparation method of the above-mentioned CrAlFe-based alloy target, as a preferred embodiment, the chemical composition of the CrAlFe-based alloy target, measured in atomic percentage, includes: Cr 10-70at% (for example, it can be 10at%, 30at%, 50at% or 70at%, etc.), Al 20-85at% (for example, it can be 20at%, 40at%, 60at% or 85at%, etc.), Fe0-20at% and not 0at% (for example, it can be 1at%, 3at%, 5at%, 10at%, 15at% or 20at%, etc.), X 0-20at% (for example, it can be 0at%, 5at%, 10at%, 15at% or 20at%, etc.), wherein X represents at least one of W, Mo, Ta, Nb, and V.

[0014] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, the mass of the required raw materials is calculated according to the atomic percentage of each element in the CrAlFe-based alloy target.

[0015] In the preparation method of the above-mentioned CrAlFe-based alloy target, as a preferred embodiment, the purity of the Fe powder is ≥99.5wt%, and the FSSS of the Fisher grain size is 5 to 8μm; the Al powder is air atomized aluminum powder, with a purity of ≥99.7wt% and a particle size of -200 mesh; the purity of the Cr powder is ≥99.8wt%, and the particle size is -200 mesh; the purity of the W powder is ≥99.9wt%, and the FSSS of the Fisher grain size is 5 to 8μm; the purity of the Mo powder is ≥99.9wt%, and the FSSS of the Fisher grain size is 5 to 8μm; the purity of the Ta powder is ≥99.8wt%, and D50 is 15 to 20μm; the purity of the Nb powder is ≥99.5wt%, and the particle size is -300 mesh; the purity of the V powder is ≥99.8wt%, and the particle size is -325 mesh.

[0016] The specific gravity of the components of ternary or higher alloy targets is greatly different, which easily leads to uneven structure. The present invention improves the fluidity between the mixed powders and reduces segregation by matching the powder particle size and morphology, such as using non-spherical aluminum powder, so as to make the prepared alloy target microstructure uniform and free of segregation.

[0017] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S1, the ball milling medium includes one of a zirconia ball, a steel ball, and a stainless steel ball, and the diameter of the ball milling medium is 20-30 mm, for example, 20 mm, 25 mm or 30 mm.

[0018] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S1, the mass ratio of the ball material is ball / powder raw material = (10-20):1, for example, it can be 10:1, 15:1 or 20:1, etc.

[0019] In the above-mentioned preparation method of CrAlFe-based alloy target material, as a preferred embodiment, in step S1, first pre-evacuate to a vacuum degree of ≤0.1Pa, then fill with 0.5-2Pa of Ar gas, and perform high-energy ball milling treatment under Ar gas protection. The ball milling speed is 100-150r / min (for example, it can be 100r / min, 120r / min or 150r / min, etc.), and the ball milling time is 20-50h (for example, it can be 20h, 40h or 50h, etc.). If the ball milling time is too long, the oxygen content in the target material will increase.

[0020] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S1, after the high-energy ball milling treatment is completed, the AlFe alloy powder is sieved to remove large particles of the powder, wherein the aperture of the sieve is 1-2 mm.

[0021] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S2, the mixing is carried out in a mixer, and zirconium oxide balls are added for dry mixing, and the ball-to-material mass ratio (the weight ratio of balls to mixed powder) corresponding to the zirconium oxide balls is 1:(5-10) (for example, it can be 1:5, 1:7 or 1:10, etc.), and the mixing time is 3-10h (for example, it can be 3h, 5h, 7h or 10h, etc.). The purpose of adding balls in the embodiment of the present invention is to accelerate the diffusion, convection and shear between powder particles, so as to quickly achieve the ideal mixing effect.

[0022] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, the mixer is at least one of a universal motion mixer, a three-dimensional mixer, and a double cone mixer, preferably a universal motion mixer.

[0023] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S3, the pressure relief includes maintaining the pressure and cooling to 400-460°C (for example, 400°C, 410°C, 430°C or 460°C, etc.), and then linearly reducing the pressure to a pressure of 0 MPa (removing the pressure applied to the CrAlFe-based alloy sintered billet).

[0024] Here, linear pressure relief refers to pressure relief at a fixed pressure relief rate.

[0025] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S3, the maximum sintering temperature of the hot pressing sintering is 500-600°C.

[0026] In the above-mentioned preparation method of the CrAlFe-based alloy target, as a preferred embodiment, in step S3, the hot pressing sintering includes: first, at room temperature, applying an initial pressure of 5-12Mpa (for example, 5MPa, 7MPa, 10MPa or 12MPa, etc.) to the CrAlFe-based alloy powder, and evacuating to 0.1-0.5Pa at the same time, and then performing vacuum hot pressing sintering, heating from room temperature to 120-180°C (for example, 120°C, 140°C, 160°C or 180°C, etc., if the temperature is too high, the O content in the target material will increase, preferably 120-150°C), the heating rate is 1-5°C / min, and when the vacuum degree reaches 0.01Pa-0.05Pa, the timing of heat preservation and pressure holding is started, the heat preservation and pressure holding time at 120-180°C and 5-12Mpa is 1-5h, and then the heating rate is continued to increase. The temperature is raised to a sintering temperature of 500-600°C (for example, 500°C, 510°C, 530°C, 550°C or 600°C. If the temperature is too low, the compact density is low, and there are many residual pores. During target coating, degassing and slag are easily caused, which affects the quality of the film layer. When the temperature is too high, Al reacts with other components to form a brittle alloy phase, and cracks begin to appear in the compact. At the same time, the pressure is linearly increased to a sintering pressure of 20-50MPa (for example, 20MPa, 30MPa, 40MPa or 50MPa, preferably 30-50MPa), and the temperature and pressure are maintained at 500-600°C and 20-50MPa for 1-6h (for example, 1h, 3h, 5h or 6h).

[0027] Here, the time for increasing the pressure from 5-12 MPa to 20-50 MPa is the same as the time for increasing the temperature from 120-180°C to the sintering temperature of 500-600°C.

[0028] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S3, the pressure relief time is 20 min-60 min (for example, it can be 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min or 60 min, etc.).

[0029] In the above-mentioned preparation method of the CrAlFe-based alloy target, as a preferred embodiment, in step S3, the cooling and demolding include: air cooling with the furnace after pressure relief, and demolding after the furnace temperature is lower than 200°C (for example, it can be 100°C, 120°C, 140°C, 160°C or 200°C, etc.).

[0030] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, the machining includes at least one of grinding, wire cutting, turning and milling.

[0031] In the above-mentioned preparation method of the CrAlFe-based alloy target, as a preferred embodiment, in step S3, the hot pressing and sintering of the CrAlFe-based alloy powder includes: filling the CrAlFe-based alloy powder into a mold, and then hot pressing and sintering, wherein the mold is a graphite mold, and the inner cavity size of the mold is (D108-D300) mm*(150-300) mm (mold depth).

[0032] In the above-mentioned method for preparing the CrAlFe-based alloy target, as a preferred embodiment, in step S4, the size of the CrAlFe-based alloy target is D (60-300) mm*(10-40) mm.

[0033] In a second aspect, the present invention provides a CrAlFe-based alloy target material, wherein the CrAlFe-based alloy target material is made by the preparation method provided in the first aspect.

[0034] In the above CrAlFe-based alloy target, as a preferred embodiment, the relative density of the CrAlFe-based alloy target is ≥ 99%. Relative density = actual density value / theoretical density value.

[0035] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:

[0036] (1) The present invention adopts a vacuum hot pressing sintering process to release the pressure before cooling to prepare a CrAlFe-based alloy target, thereby improving the cracking phenomenon of the CrAlFe-based alloy target.

[0037] (2) The fluidity of ternary and above alloy powders can be improved by controlling the particle size and morphology of the powder (such as using air atomized aluminum powder and selecting finer powder for mixing). At the same time, a mixer is used to improve the uniformity of powder mixing, effectively solving the problem of uneven structure in the alloy target.

[0038] (3) High-energy ball milling of Al powder and Fe powder allows the metal Fe to fully alloy with Al to form AlFe alloy powder, effectively avoiding the heat release caused by the intense alloying reaction of pure Al powder and Fe powder during hot pressing sintering, which causes the Cr in the target material to alloy with the matrix Al to generate more brittle alloy phases. This can effectively improve the brittleness of CrAlFe and CrAlFeX alloy targets and improve the cracking problem of the billet.

[0039] (4) The alloy target is prepared by hot pressing sintering process. Since the pressure head is lifted during cooling, the cooling process can be pressure-free. After cooling, the residual internal stress in the CrAlFe and CrAlFeX alloy targets is small. The prepared alloy target has high density, uniform structure and no cracking. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 The microstructure diagram of the CrAlFe alloy target provided in Example 1;

[0041] Figure 2 The microstructure diagram of the CrAlFe alloy target provided in Comparative Example 1;

[0042] Figure 3 This is the appearance picture of the CrAlFe alloy target product provided in Example 1;

[0043] Figure 4 This is an appearance diagram of the CrAlFe alloy target product provided in Comparative Example 1;

[0044] Figure 5 Another appearance picture of the CrAlFe alloy target product provided for Comparative Example 1. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0046] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0047] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0048] The process parameters in the following examples that do not specify specific conditions are usually based on conventional conditions. The experimental reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the amounts of the experimental reagents, unless otherwise specified, are all the amounts of reagents used in conventional experimental operations.

[0049] In a first aspect, the present invention provides a method for preparing a CrAlFe-based alloy target, comprising the following steps:

[0050] S1. Pre-evacuate to a vacuum degree of ≤0.1Pa, then fill with 0.5-2Pa of Ar gas, and under the protection of Ar gas, perform high-energy ball milling on Al powder and Fe powder. After the high-energy ball milling, sieve the AlFe alloy powder to remove large particles of powder, the aperture of the sieve is 1-2mm, and obtain pre-alloyed AlFe alloy powder, wherein the ball milling medium comprises one of zirconia balls, steel balls, and stainless steel balls, the diameter of the ball milling medium is 20-30mm, the ball-to-material mass ratio is ball / powder raw material=(10-20):1, the ball milling speed is 100-150r / min, and the ball milling time is 20-50h.

[0051] S2, the AlFe alloy powder and the Cr powder are uniformly mixed in a mixer, or the AlFe alloy powder, the Cr powder and the X powder are uniformly mixed in a mixer, and zirconia balls are added for dry mixing to obtain CrAlFe-based alloy powder, wherein the X powder includes at least one of W powder, Mo powder, Ta powder, Nb powder and V powder, the Fe powder has a purity of ≥99.5wt% and a Fisher particle size FSSS of 5 to 8μm; the Al powder is air atomized aluminum powder with a purity of ≥99.7wt% and a particle size of -200 mesh; the Cr powder has a purity of ≥99.8wt% and a particle size of -200 mesh; the W powder The purity of the Mo powder is ≥99.9wt%, and the FSSS is 5-8μm; the purity of the Mo powder is ≥99.9wt%, and the FSSS is 5-8μm; the purity of the Ta powder is ≥99.8wt%, and D50 is 15-20μm; the purity of the Nb powder is ≥99.5wt%, and the particle size is -300 mesh; the purity of the V powder is ≥99.8wt%, and the particle size is -325 mesh, the ball-to-material mass ratio (the weight ratio of the ball to the mixed powder) corresponding to the zirconia ball is 1:(5-10), the mixing time is 3-10h, and the mixer is at least one of a universal motion mixer, a three-dimensional mixer, and a double-cone mixer.

[0052] S3, under vacuum conditions, filling the CrAlFe-based alloy powder into a graphite mold, and then hot pressing and sintering, after the hot pressing and sintering is completed, the pressure is released, and then cooled and demolded to obtain a CrAlFe-based alloy sintered blank, wherein the inner cavity size of the graphite mold is (D108-D300) mm*(150-300) mm (mold depth), and the hot pressing and sintering includes: first, at room temperature, applying an initial pressure of 5-12 MPa to the CrAlFe-based alloy powder, and evacuating to 0.1-0.5 Pa, and then performing vacuum hot pressing and sintering, from room temperature to 120-180°C, the heating rate is 1-5°C / min, and when the vacuum After the temperature reaches 0.01Pa-0.05Pa, start timing the heat preservation and pressure holding, the heat preservation and pressure holding time at 120-180℃ and 5-12Mpa is 1-5h, and then continue to heat up to the sintering temperature of 500-600℃ at a heating rate of 2-10℃ / min, and linearly increase the pressure to the sintering pressure of 20-50MPa, and keep the heat and pressure at 500-600℃ and 20-50MPa for 1-6h. The pressure relief includes pressure holding and cooling to 400-460℃, and then linearly unloading the pressure to 0MPa, and the pressure relief time is 20min-60min. The cooling and demoulding include: air cooling with the furnace after pressure relief, and demoulding after the furnace temperature is lower than 200℃.

[0053] S4. Machining (grinding, wire cutting, turning, milling) the CrAlFe-based alloy sintered billet to obtain the CrAlFe-based alloy target, wherein the size of the CrAlFe-based alloy target is D(60-300) mm*(10-40) mm, and the chemical composition of the CrAlFe-based alloy target, in terms of atomic percentage, comprises: Cr 10-70 at%, Al 20-85 at%, Fe 0-20 at% and not 0 at%, X 0-20 at%, wherein X represents at least one of W, Mo, Ta, Nb, and V.

[0054] The invention adopts vacuum hot pressing sintering technology, and produces CrAlFe and CrAlFeX alloy targets with relative density ≥ 99%, uniform structure and no cracks through powder screening and powder mechanical alloying pretreatment, and the target has excellent coating performance.

[0055] The high-energy ball milling pre-alloying treatment of Al powder and Fe powder ensures that the alloy phase content in the target material is small and reduces the intrinsic brittleness of the target material; the pressure head is lifted during the cooling process of the hot pressing sintering process to ensure that the residual internal stress inside the pressed blank is small and the prepared target material is not easy to crack.

[0056] In a second aspect, the present invention provides a CrAlFe-based alloy target material, which is made by the preparation method provided in the first aspect, and has a relative density of ≥99%.

[0057] In order to further understand the present invention, the CrAlFe-based alloy target material and the preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0058] Example 1

[0059] The CrAlFe-based alloy target provided in this embodiment is a CrAlFe alloy target, and its chemical composition and atomic percentage are: Cr 40 Al 50 Fe 10 , that is, in atomic percentage: Cr 40at%, Al 50at%, Fe 10at%, in weight percentage: Cr 52.16wt%, Al 33.83wt%, Fe 14.01wt%.

[0060] The preparation method of the CrAlFe-based alloy target provided in this embodiment comprises the following steps:

[0061] S1. According to the chemical composition and atomic percentage of the CrAlFe-based alloy target provided in this embodiment, and according to the mass of the prepared CrAlFe-based alloy target, the raw materials required for preparing the CrAlFe-based alloy target are calculated and weighed, wherein the raw materials include Cr powder, Al powder and Fe powder, wherein the Fe powder has a purity of ≥99.5wt% and a Fisher particle size FSSS=6.0μm; the Al powder is air atomized aluminum powder, with a purity of ≥99.7wt% and a particle size of -200 mesh; the Cr powder has a purity of ≥99.8wt% and a particle size of -200 mesh;

[0062] Al powder and Fe powder were loaded into a high-energy ball mill for high-energy ball milling to obtain pre-alloyed AlFe alloy powder. The high-energy ball milling parameters were as follows: a steel ball with a diameter of D25 mm was used as the ball milling medium, the ball-to-material ratio was the mass ratio of the ball to the powder raw material = 15:1, and the ball milling process was first pre-evacuated to a vacuum degree of 0.05 Pa, and then 0.5 Pa of Ar gas was filled into the high-energy ball mill, and high-energy ball milling was performed under Ar gas protection. The ball milling speed was 120 r / min, and the ball milling time was 24 h. After the ball milling was completed, the alloy powder was sieved to remove large particles of the powder, and the sieve aperture was 1 mm.

[0063] S2. The AlFe alloy powder and Cr powder obtained in step S1 are uniformly mixed in a universal motion mixer to obtain CrAlFe alloy powder. The mixing is carried out by adding zirconium oxide balls for dry mixing. The ball-to-material ratio is ZrO2 ball weight: mixed powder weight = 1:10, and the mixing time is 6 hours.

[0064] S3, the CrAlFe alloy powder obtained in the above step S2 is uniformly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm (the effective inner diameter of the mold is 165mm, and the depth is 200mm), and hot pressing sintering is performed under vacuum conditions. Vacuuming is continuously performed during the hot pressing sintering process. After the hot pressing sintering is completed, the pressure is maintained and the furnace is cooled to 450°C, and then the pressure is linearly relieved to 0MPa, and the pressure relief time is 30min, and then the furnace is naturally cooled to 150°C, and the furnace is demolded to obtain a high-density CrAlFe sintered blank. The hot pressing sintering includes: first, at room temperature, the C An initial pressure of 10 MPa was applied to the rAlFe alloy powder, and the pressure was evacuated to 0.1 Pa at the same time. The vacuum hot pressing sintering program was then started, and the temperature was raised from room temperature to 150°C at a heating rate of 2°C / min. When the vacuum degree reached 0.05 Pa, the timing of heat preservation and pressure holding began. The temperature was kept at 150°C and 10 MPa for 3 hours, and then the temperature was continued to be raised to the sintering temperature of 535°C (the heating rate was 4°C / min). At the same time, the pressure was linearly increased to 35 MPa. The time for increasing the pressure from 10 MPa to 35 MPa was the same as the time for increasing the temperature from 150°C to the sintering temperature of 535°C. The temperature was kept at 535°C and 35 MPa for 2.5 hours.

[0065] S4. The CrAlFe sintered blank is subjected to grinding, wire cutting, turning and milling to obtain a CrAlFe alloy target (finished target) that meets the size and surface quality requirements. The target is a round target with dimensions: diameter D156.3 mm and height 20 mm.

[0066] Figure 1 The microstructure diagram (SEM diagram) of the CrAlFe alloy target provided in this embodiment is as follows: Figure 3 The appearance of the CrAlFe alloy target product provided in this embodiment is shown in FIG. Figure 1 and Figure 3 It can be seen that the CrAlFe alloy target material provided in this embodiment has a uniform structure, no alloying reaction occurs between Cr and Al matrix, and no cracking phenomenon occurs in the target material.

[0067] Example 2

[0068] The CrAlFe-based alloy target provided in this embodiment is a CrAlFeMo alloy target, and its chemical composition and atomic percentage are: Cr 15 Al 60 Fe 20 Mo5, that is, calculated by atomic percentage: Cr 15at%, Al 60at%, Fe 20at%, Mo5at%, calculated by weight percentage: Cr 19.52wt%, Al 40.51wt%, Fe 27.96wt%, Mo 12.01wt%.

[0069] The preparation method of the CrAlFe-based alloy target provided in this embodiment comprises the following steps:

[0070] S1. According to the chemical composition and atomic percentage of the CrAlFe-based alloy target provided in this embodiment and the mass of the prepared CrAlFe-based alloy target, the raw materials required for preparing the CrAlFe-based alloy target are calculated and weighed, wherein the raw materials include Cr powder, Al powder, Fe powder and Mo powder, wherein the Fe powder has a purity of ≥99.5wt% and a FSSS particle size of 6.0μm; the Al powder is air atomized aluminum powder with a purity of ≥99.7wt% and a particle size of -200 mesh; the Cr powder has a purity of ≥99.8wt% and a particle size of -200 mesh; the Mo powder has a purity of ≥99.9wt% and a FSSS particle size of 6.7μm;

[0071] Al powder and Fe powder were loaded into a high-energy ball mill for high-energy ball milling to obtain pre-alloyed AlFe alloy powder. The high-energy ball milling parameters were as follows: a steel ball with a diameter of D25 mm was used as the ball milling medium, the ball-to-material ratio was the mass ratio of the ball to the powder raw material = 15:1, and the ball milling process was first pre-evacuated to a vacuum degree of 0.05 Pa, and then 0.5 Pa of Ar gas was filled into the high-energy ball mill, and high-energy ball milling was performed under Ar gas protection. The ball milling speed was 120 r / min, and the ball milling time was 24 h. After the ball milling was completed, the alloy powder was sieved to remove large particles of the powder, and the sieve aperture was 1 mm.

[0072] S2. The AlFe alloy powder obtained in step S1 is uniformly mixed with Cr powder and Mo powder in a universal motion mixer to obtain CrAlFeMo alloy powder. The mixing is carried out by adding zirconium oxide balls for dry mixing. The ball-to-material ratio is ZrO2 ball weight: mixed powder weight = 1:10, and the mixing time is 6 hours.

[0073] S3, the CrAlFeMo alloy powder obtained in the above step S2 is uniformly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm, and hot pressing sintering is performed under vacuum conditions. During the hot pressing sintering process, vacuum is continuously drawn. After the hot pressing sintering is completed, the pressure is maintained and the furnace is cooled to 450°C, and then the pressure is linearly relieved to a pressure of 0MPa, and the pressure relief time is 0.5h. Then, the furnace is naturally cooled to 150°C, and the mold is removed from the furnace to obtain a high-density CrAlFeMo sintered blank. The hot pressing sintering includes: first, at room temperature, the CrAlFeMo alloy is An initial pressure of 8 MPa was applied to the gold powder, and the temperature was evacuated to 0.1 Pa. The vacuum hot pressing sintering program was then started, and the temperature was raised from room temperature to 135°C at a heating rate of 2°C / min. When the vacuum degree reached 0.03 Pa, the timing of heat preservation and pressure holding began. The temperature was kept at 135°C and 8 MPa for 4 hours, and then the temperature was continued to be raised to the sintering temperature of 520°C (the heating rate was 5°C / min). At the same time, the pressure was linearly increased to 40 MPa. The time for increasing the pressure from 8 MPa to 40 MPa was the same as the time for increasing the temperature from 135°C to the sintering temperature of 520°C. The temperature was kept at 520°C and 40 MPa for 3 hours.

[0074] S4. The CrAlFeMo sintered blank is subjected to grinding, wire cutting, turning and milling to obtain a CrAlFeMo alloy target (finished target) that meets the size and surface quality requirements. The target is a round target with dimensions of: diameter D160 mm and height 14 mm.

[0075] The microstructure of the CrAlFeMo alloy target prepared in this embodiment is similar to that of Embodiment 1. The alloy target prepared in this embodiment has a uniform structure, no alloying reaction occurs between Cr and Al, and no cracking occurs in the target.

[0076] Example 3

[0077] The CrAlFe-based alloy target provided in this embodiment is a CrAlFeNb alloy target, and its chemical composition and atomic percentage are: Cr 55 Al 40 Fe3Nb2, that is, in atomic percentage: Cr 55at%, Al 40at%, Fe 3at%, Nb 2at%, in weight percentage: Cr 66.63wt%, Al 25.14wt%, Fe 3.9wt%, Nb 4.33wt%.

[0078] The preparation method of the CrAlFe-based alloy target provided in this embodiment comprises the following steps:

[0079] S1. According to the chemical composition and atomic percentage of the CrAlFe-based alloy target provided in this embodiment, and according to the mass of the prepared CrAlFe-based alloy target, the raw materials required for preparing the CrAlFe-based alloy target are calculated and weighed, wherein the raw materials include Cr powder, Al powder, Fe powder and Nb powder, wherein the Fe powder has a purity of ≥99.5wt% and a Fisher particle size FSSS=6.0μm; the Al powder is air atomized aluminum powder, with a purity of ≥99.7wt% and a particle size of -200 mesh; the Cr powder has a purity of ≥99.8wt% and a particle size of -200 mesh; the Nb powder has a purity of ≥99.5wt% and a particle size of -300 mesh;

[0080] Al powder and Fe powder were loaded into a high-energy ball mill for high-energy ball milling to obtain pre-alloyed AlFe alloy powder. The high-energy ball milling parameters were as follows: a steel ball with a diameter of D25 mm was used as the ball milling medium, the ball-to-material ratio was the mass ratio of the ball to the powder raw material = 15:1, and the ball milling process was first pre-evacuated to a vacuum degree of 0.05 Pa, and then 0.5 Pa of Ar gas was filled into the high-energy ball mill, and high-energy ball milling was performed under Ar gas protection. The ball milling speed was 120 r / min, and the ball milling time was 24 h. After the ball milling was completed, the alloy powder was sieved to remove large particles of the powder, and the sieve aperture was 1 mm.

[0081] S2. The AlFe alloy powder obtained in step S1 is uniformly mixed with Cr powder and Nb powder in a universal motion mixer to obtain CrAlFeNb alloy powder. The mixing is carried out by adding zirconium oxide balls for dry mixing. The ball-to-material ratio is ZrO2 ball weight: mixed powder weight = 1:10, and the mixing time is 6 hours.

[0082] S3, the CrAlFeNb alloy powder obtained in the above step S2 is uniformly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm (the effective inner diameter of the mold is 165mm, and the depth is 200mm), and hot pressing and sintering are performed under vacuum conditions. Vacuuming is continuously performed during the hot pressing and sintering process. After the hot pressing and sintering is completed, the pressure is maintained and cooled to 450°C with the furnace, and then the pressure is linearly relieved to 0MPa, and the pressure relief time is 0.5h, and then the furnace is naturally cooled to 150°C, and the mold is removed from the furnace to obtain a high-density CrAlFeNb sintered blank. The hot pressing and sintering includes: first, at room temperature, An initial pressure of 10 MPa was applied to the CrAlFeNb alloy powder, and the temperature was evacuated to 0.1 Pa. The vacuum hot pressing sintering program was then started, and the temperature was raised from room temperature to 170°C at a heating rate of 2°C / min. When the vacuum degree reached 0.02 Pa, the timing of heat preservation and pressure holding was started. The temperature was kept at 170°C and 10 MPa for 3 hours, and then the temperature was continued to be raised to the sintering temperature of 550°C (the heating rate was 4°C / min). At the same time, the pressure was linearly increased to 35 MPa. The time for increasing the pressure from 10 MPa to 35 MPa was the same as the time for increasing the temperature from 170°C to the sintering temperature of 550°C. The temperature was kept at 550°C and 35 MPa for 1.5 hours.

[0083] S4. The CrAlFeNb sintered blank is subjected to grinding, wire cutting, turning and milling to obtain a CrAlFeNb alloy target (finished target) that meets the size and surface quality requirements. The target is a round target with dimensions: diameter D160.0 mm and height 12 mm.

[0084] The microstructure of the CrAlFeNb alloy target prepared in this embodiment is similar to that of Embodiment 1. The alloy target prepared in this embodiment has a uniform structure, no alloying reaction occurs between Cr and Al, and no cracking occurs in the target.

[0085] Example 4

[0086] The CrAlFe-based alloy target provided in this embodiment is a CrAlFeV alloy target, and its chemical composition and atomic percentage are: Cr 22 Al 60 Fe3V 15 , that is, in atomic percentage: Cr 22at%, Al 60at%, Fe 3at%, V 15at%, and in weight percentage: Cr 30.96wt%, Al 43.82wt%, Fe 4.54wt%, V 20.68wt%.

[0087] The preparation method of the CrAlFe-based alloy target provided in this embodiment comprises the following steps:

[0088] S1. According to the chemical composition and atomic percentage of the CrAlFe-based alloy target provided in this embodiment, and according to the mass of the prepared CrAlFe-based alloy target, the raw materials required for preparing the CrAlFe-based alloy target are calculated and weighed, wherein the raw materials include Cr powder, Al powder, Fe powder and V powder, wherein the Fe powder has a purity of ≥99.5wt% and a Fisher particle size FSSS=6.0μm; the Al powder is air atomized aluminum powder, with a purity of ≥99.7wt% and a particle size of -200 mesh; the Cr powder has a purity of ≥99.8wt% and a particle size of -200 mesh; the V powder has a purity of ≥99.8wt% and a particle size of -325 mesh;

[0089] Al powder and Fe powder were loaded into a high-energy ball mill for high-energy ball milling to obtain pre-alloyed AlFe alloy powder. The high-energy ball milling parameters were as follows: a steel ball with a diameter of D25 mm was used as the ball milling medium, the ball-to-material ratio was the mass ratio of the ball to the powder raw material = 15:1, and the ball milling process was first pre-evacuated to a vacuum degree of 0.05 Pa, and then 0.5 Pa of Ar gas was filled into the high-energy ball mill, and high-energy ball milling was performed under Ar gas protection. The ball milling speed was 120 r / min, and the ball milling time was 32 h. After the ball milling was completed, the alloy powder was sieved to remove large particles of the powder, and the sieve aperture was 1 mm.

[0090] S2. The AlFe alloy powder obtained in step S1 is uniformly mixed with Cr powder and V powder in a universal motion mixer to obtain CrAlFeV alloy powder. The mixing is carried out by adding zirconium oxide balls for dry mixing. The ball-to-material ratio is ZrO2 ball weight: mixed powder weight = 1:10, and the mixing time is 6 hours.

[0091] S3, the CrAlFeV alloy powder obtained in the above step S2 is uniformly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm (the effective inner diameter of the mold is 165mm, and the depth is 200mm), and hot pressing sintering is performed under vacuum conditions. Vacuuming is continuously performed during the hot pressing sintering process. After the hot pressing sintering is completed, the pressure is maintained and the furnace is cooled to 450°C, and then the pressure is linearly relieved to 0MPa, and the pressure relief time is 0.5h, and then the furnace is naturally cooled to 150°C, and the furnace is demolded to obtain a high-density CrAlFeV sintered blank. The hot pressing sintering includes: first, at room temperature, An initial pressure of 12 MPa was applied to the CrAlFeV alloy powder, and the temperature was evacuated to 0.1 Pa. The vacuum hot pressing sintering program was then started, and the temperature was raised from room temperature to 160°C at a heating rate of 2°C / min. When the vacuum degree reached 0.05 Pa, the timing of heat preservation and pressure holding was started. The temperature was kept at 160°C and 12 MPa for 4 hours, and then the temperature was continued to be raised to the sintering temperature of 530°C (the heating rate was 4°C / min). At the same time, the pressure was linearly increased to 35 MPa. The time for increasing the pressure from 12 MPa to 35 MPa was the same as the time for increasing the temperature from 160°C to the sintering temperature of 530°C. The temperature was kept at 530°C and 35 MPa for 3 hours.

[0092] S4. The CrAlFeV sintered blank is subjected to grinding, wire cutting, turning and milling to obtain a CrAlFeV alloy target (finished target) that meets the size and surface quality requirements. The target is a round target with dimensions: diameter D154.0 mm and height 20 mm.

[0093] The microstructure of the CrAlFeV alloy target prepared in this embodiment is similar to that of Embodiment 1. The alloy target prepared in this embodiment has a uniform structure, no alloying reaction occurs between Cr and Al, and no cracking occurs in the target.

[0094] Example 5

[0095] The CrAlFe-based alloy target provided in this embodiment is a CrAlFe alloy target, and its chemical composition and atomic percentage are: Cr 70 Al 25 Fe5, that is, in atomic percentage: Cr 70at%, Al 25at%, Fe 5at%, in weight percentage: Cr 79.24wt%, Al 14.68wt%, Fe 6.08wt%.

[0096] The preparation method of the CrAlFe-based alloy target provided in this embodiment comprises the following steps:

[0097] S1. Prepare pre-alloyed AlFe alloy powder by referring to step S1 of Example 1.

[0098] S2. The AlFe alloy powder and Cr powder obtained in step S1 are uniformly mixed in a universal motion mixer to obtain CrAlFe alloy powder. The mixing is carried out by adding zirconium oxide balls for dry mixing. The ball-to-material ratio is ZrO2 ball weight: mixed powder weight = 1:5, and the mixing time is 4 hours.

[0099] S3, the CrAlFe alloy powder obtained in the above step S2 is uniformly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm (the effective inner diameter of the mold is 165mm, and the depth is 200mm), and hot pressing and sintering are performed under vacuum conditions. Vacuuming is continuously performed during the hot pressing and sintering process. After the hot pressing and sintering is completed, the pressure is maintained and cooled to 450°C with the furnace, and then the pressure is linearly relieved to 0MPa, and the pressure relief time is 0.5h, and then the furnace is naturally cooled to 100°C, and the furnace is demolded to obtain a high-density CrAlFe sintered blank. The hot pressing and sintering includes: first, at room temperature, An initial pressure of 10 MPa was applied to the CrAlFe alloy powder, and the powder was evacuated to 0.1 Pa. The vacuum hot pressing sintering program was then started, and the temperature was raised from room temperature to 150°C at a heating rate of 2°C / min. When the vacuum degree reached 0.01 Pa, the timing of heat preservation and pressure holding was started. The powder was kept at 150°C and 10 MPa for 4 hours, and then the temperature was continued to be raised to the sintering temperature of 600°C (the heating rate was 4°C / min). At the same time, the pressure was linearly increased to 25 MPa. The time for increasing the pressure from 10 MPa to 25 MPa was the same as the time for increasing the temperature from 150°C to the sintering temperature of 600°C. The powder was kept at 600°C and 25 MPa for 5 hours.

[0100] S4. The CrAlFe sintered blank is subjected to grinding, wire cutting, turning and milling to obtain a CrAlFe alloy target (finished target) that meets the size and surface quality requirements. The target is a round target with dimensions: diameter D156.3 mm and height 20 mm.

[0101] The microstructure of the CrAlFe alloy target prepared in this embodiment is similar to that of Embodiment 1. The alloy target prepared in this embodiment has a uniform structure, no alloying reaction occurs between Cr and Al, and no cracking occurs in the target.

[0102] Comparative Example 1

[0103] The CrAlFe-based alloy target provided in this comparative example is a CrAlFe alloy target, and its chemical composition and atomic percentage are: Cr 40 Al 50 Fe 10 , that is, in terms of atomic percentage: Cr 40at%, Al 50at%, Fe 10at%, and in terms of weight percentage: Cr 52.16wt%, Al 33.83wt%, Fe 14.01wt%.

[0104] The preparation method of the CrAlFe-based alloy target provided in this comparative example is a HIP process, which specifically includes the following steps:

[0105] S1. According to the chemical composition and atomic percentage of the CrAlFe-based alloy target provided in this embodiment and the mass of the prepared CrAlFe-based alloy target, the raw materials required for preparing the CrAlFe-based alloy target are calculated and weighed, wherein the raw materials include Cr powder, Al powder and Fe powder, wherein the Fe powder has a purity of ≥99.5wt% and a Fisher particle size FSSS=6.0μm; the Al powder is air atomized aluminum powder with a purity of ≥99.7wt% and a particle size of -200 mesh; the Cr powder has a purity of ≥99.8wt% and a particle size of -200 mesh; the Al powder, Fe powder and Cr powder are mixed in a universal motion mixer for 6 hours with a ball-to-material ratio of 1:10 to obtain CrAlFe alloy powder.

[0106] S2. The powder prepared in step S1 is packaged and degassed in a degassing furnace at a degassing temperature of 350° C., a degassing vacuum of 0.005 Pa, and a degassing holding time of 4 hours. After the package is sealed and welded, hot isostatic pressing (HIP) is performed at a HIP temperature of 450° C. and a pressure of 115 MPa for 4 hours. The powder is then cooled to 150° C. with the furnace, the pressure is released, the powder is emptied, and the powder is taken out of the furnace. After being taken out of the furnace, the powder is first cooled to room temperature, and then the package skin is removed to obtain a CrAlFe-based alloy sintered billet.

[0107] S3. Performing wire cutting and turning / milling processing on the CrAlFe-based alloy sintered billet to obtain the CrAlFe-based alloy target.

[0108] Figure 2 The microstructure diagram (SEM diagram) of the CrAlFe alloy target provided in this comparative example is as follows: Figure 4 This is the appearance of the CrAlFe alloy target product provided in this comparative example. Figure 5 Another appearance picture of the CrAlFe alloy target product provided in this comparative example is shown in FIG. Figure 2 , Figure 4 and Figure 5 It can be seen that the CrAlFe alloy target material provided in this comparative example has a large number of annular cracks on the outer circle and the core, and a large number of cracks on the edges of the Cr particles, with serious cracking. The applicant speculates that the reason may be that: the reaction between Al and Fe releases heat, resulting in alloying of Cr and Al, generating more alloy phases, increasing the brittleness of the target material and making it easy to crack; because the conventional hot isostatic pressing process is to cool down under pressure, the residual stress in the target material is large after cooling, and the brittle target material is easy to crack.

[0109] Comparative Example 2

[0110] The CrAlFe-based alloy target provided in this comparative example is a CrAlFe alloy target, and its chemical composition and atomic percentage are the same as those in Example 1, specifically: Cr 40 Al 50 Fe 10 , that is, calculated by atomic percentage: Cr 40at%, Al 50at%, Fe 10at%.

[0111] The preparation method of the CrAlFe-based alloy target provided in this comparative example is basically the same as that in Example 1, except that all alloy powders are mixed together, specifically comprising the following steps:

[0112] S1. According to the chemical composition and atomic percentage of the CrAlFe-based alloy target provided in this embodiment, and according to the mass of the prepared CrAlFe-based alloy target, the raw materials required for preparing the CrAlFe-based alloy target are calculated and weighed, wherein the raw materials include Cr powder, Al powder and Fe powder, wherein the Fe powder has a purity of ≥99.5wt% and a Fisher particle size FSSS=6.0μm; the Al powder is air atomized aluminum powder, with a purity of ≥99.7wt% and a particle size of -200 mesh; the Cr powder has a purity of ≥99.8wt% and a particle size of -200 mesh;

[0113] Al powder, Fe powder and Cr powder were mixed evenly in a universal motion mixer to obtain CrAlFe alloy powder. The mixing was carried out by adding zirconium oxide balls for dry mixing. The ball-to-material ratio was ZrO2 ball weight: mixed powder weight = 1:10, and the mixing time was 8 hours.

[0114] S2 is the same as step S3 in Example 1.

[0115] S3 is the same as step S4 in Example 1.

[0116] The CrAlFe alloy target material provided in this comparative example has alloying reaction between Cr and Al inside, and microcracks inside the target material.

[0117] Comparative Example 3

[0118] The CrAlFe-based alloy target provided in this comparative example is a CrAlFe alloy target, and its chemical composition and atomic percentage are the same as those in Example 1, specifically: Cr 40 Al 50 Fe 10 , that is, calculated by atomic percentage: Cr 40at%, Al 50at%, Fe 10at%.

[0119] The preparation method of the CrAlFe-based alloy target provided in this comparative example is basically the same as that in Example 1, except that the temperature is raised from room temperature to 300° C. in step S3, which specifically includes the following steps:

[0120] S1-S2 are the same as steps S1-S2 in Example 1.

[0121] S3, the CrAlFe alloy powder obtained in the above step S2 is evenly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm (the effective inner diameter of the mold is 165mm, and the depth is 200mm), and hot pressing and sintering are carried out under vacuum conditions. Vacuuming is continuously performed during the hot pressing and sintering process. After the hot pressing and sintering is completed, the pressure is maintained and cooled to 450°C with the furnace, and then the pressure is linearly relieved to 0MPa, and the pressure relief time is 0.5h, and then naturally cooled to 150°C with the furnace, and demolded to obtain a high-density CrAlFe sintered blank. The hot pressing and sintering process is as follows: The pressure sintering includes: first, at room temperature, applying an initial pressure of 10 MPa to the CrAlFe alloy powder, and evacuating the pressure to 0.1 Pa, then starting the vacuum hot pressing sintering program, heating the temperature from room temperature to 300°C, with a heating rate of 2°C / min, and starting the timing of heat preservation and pressure maintenance when the vacuum degree reaches 0.05 Pa, and maintaining the temperature and pressure at 300°C and 10 MPa for 3 hours, and then continuing to heat and maintain the temperature to a sintering temperature of 535°C (heating rate of 4°C / min), and at the same time linearly increasing the pressure to a sintering pressure of 35 MPa, and maintaining the temperature and pressure at 535°C and 35 MPa for 2.5 hours.

[0122] S4 is the same as step S4 in Example 1.

[0123] Comparative Example 4

[0124] The CrAlFe-based alloy target provided in this comparative example is a CrAlFe alloy target, and its chemical composition and atomic percentage are the same as those in Example 1, specifically: Cr 40 Al 50 Fe 10 , that is, calculated by atomic percentage: Cr 40at%, Al 50at%, Fe 10at%.

[0125] The preparation method of the CrAlFe-based alloy target provided in this comparative example is basically the same as that in Example 1, except that the sintering temperature in step S3 is 660° C., and specifically comprises the following steps:

[0126] S1-S2 are the same as steps S1-S2 in Example 1.

[0127] S3, the CrAlFe alloy powder obtained in the above step S2 is evenly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm (the effective inner diameter of the mold is 165mm, and the depth is 200mm), and hot pressing and sintering are carried out under vacuum conditions. Vacuuming is continuously performed during the hot pressing and sintering process. After the hot pressing and sintering is completed, the pressure is maintained and cooled to 450°C with the furnace, and then the pressure is linearly relieved to 0MPa, and the pressure relief time is 0.5h, and then naturally cooled to 150°C with the furnace, and demolded to obtain a high-density CrAlFe sintered blank. The hot pressing The sintering process includes: first, applying an initial pressure of 10 MPa to the CrAlFe alloy powder at room temperature, and evacuating the temperature to 0.1 Pa, then starting a vacuum hot pressing sintering program, heating the temperature from room temperature to 150°C, with a heating rate of 2°C / min, and starting the timing of heat preservation and pressure maintenance when the vacuum degree reaches 0.05 Pa, and maintaining the temperature at 150°C and 10 MPa for 3 hours, then continuing to heat and maintain the temperature to a sintering temperature of 660°C (with a heating rate of 4°C / min), and linearly increasing the pressure to a sintering pressure of 35 MPa, and the heat preservation and pressure maintenance time at 660°C and 35 MPa is 1 hour.

[0128] S4 is the same as step S4 in Example 1.

[0129] The CrAlFe alloy target material provided in this comparative example has serious alloying of Cr and Al inside, and microcracks appear in the target material.

[0130] Comparative Example 5

[0131] The CrAlFe-based alloy target provided in this comparative example is a CrAlFe alloy target, and its chemical composition and atomic percentage are the same as those in Example 1, specifically: Cr 40 Al 50 Fe 10 , that is, calculated by atomic percentage: Cr 40at%, Al 50at%, Fe 10at%.

[0132] The preparation method of the CrAlFe-based alloy target provided in this comparative example is basically the same as that in Example 1, except that the ball milling time in step S1 is 60 hours, and specifically comprises the following steps:

[0133] S1 is basically the same as step S1 in Example 1, except that the ball milling time is 60 h.

[0134] S2-S4 are the same as steps S2-S4 in Example 1.

[0135] Comparative Example 6

[0136] The CrAlFe-based alloy target provided in this comparative example is a CrAlFe alloy target, and its chemical composition and atomic percentage are: Cr 40 Al50 Fe 10 , that is, in atomic percentage: Cr 40at%, Al 50at%, Fe 10at%, in weight percentage: Cr 52.16wt%, Al 33.83wt%, Fe 14.01wt%.

[0137] The preparation method of the CrAlFe-based alloy target provided in this comparative example is basically the same as that in Example 1, except that, in step S3, after the hot pressing sintering is completed, the target is naturally cooled to 150° C. with the furnace, the pressure is released, and the target is taken out of the furnace and demolded, which specifically includes the following steps:

[0138] Steps S1 and S2 are the same as steps S1 and S2 in Example 1.

[0139] S3, the CrAlFe alloy powder obtained in the above step S2 is uniformly filled into a circular graphite mold, the effective size of the mold cavity is D165*200mm (the effective inner diameter of the mold is 165mm, and the depth is 200mm), and hot pressing and sintering is performed under vacuum conditions. Vacuuming is continuously performed during the hot pressing and sintering process. After the hot pressing and sintering is completed, the powder is naturally cooled to 150°C with the furnace, and then linearly depressurized to a pressure of 0MPa for 30min, and then removed from the furnace and demolded to obtain a CrAlFe sintered blank. The hot pressing and sintering comprises: first, at room temperature, the CrAlFe alloy powder is Apply an initial pressure of 10 MPa, and evacuate to 0.1 Pa at the same time, then start the vacuum hot pressing sintering program, heat from room temperature to 150°C, with a heating rate of 2°C / min. When the vacuum degree reaches 0.05 Pa, start timing the heat preservation and pressure holding. Keep the temperature at 150°C and 10 MPa for 3 hours, then continue to heat to the sintering temperature of 535°C (heating rate of 4°C / min), and linearly increase the pressure to 35 MPa at the same time. The time for increasing the pressure from 10 MPa to 35 MPa is the same as the time for increasing the temperature from 150°C to the sintering temperature of 535°C. Keep the temperature at 535°C and 35 MPa for 2.5 hours.

[0140] Step S4 is the same as step S4 in Example 1.

[0141] The alloy target prepared in this comparative example had cracks with a depth of 2-3 mm on its surface.

[0142] Performance Testing

[0143] The relative density, target brittleness and oxygen content of the CrAlFe alloy targets provided in Examples 1-5 and Comparative Examples 1-5 were tested. The test results are shown in Table 1.

[0144] Relative density detection method: Relative density is calculated by dividing the measured density of the target material by the theoretical density. The measured density is measured by the Archimedes drainage method.

[0145] Target brittleness (bending strength) detection method: Instron 3369 universal material testing machine is used to measure the mechanical properties according to the industry standard YB / T 5349-2014 "Methods for testing the bending mechanical properties of metal materials".

[0146] The O content in the target was measured by inert gas fusion infrared thermal conductivity method.

[0147] Table 1

[0148]

[0149] From Table 1, we can see the following points:

[0150] (1) The alloy targets prepared in Examples 1-5 have a lower oxygen content, a greater bending strength and a higher density. The higher the degree of alloying in the target, the higher the relative density of the target, which usually exceeds the theoretical density value. Therefore, in the comparative example, a relative density greater than 100% will occur.

[0151] (2) It can be seen from Example 1 and Comparative Example 2 that the present invention can effectively improve the brittleness of the CrAlFe alloy target material and improve the flexural strength of the target material by first subjecting the Al powder and the Fe powder to high-energy ball milling treatment and then evenly mixing the AlFe alloy powder and the Cr powder. The higher the flexural strength of the target material, the stronger the material's crack resistance. The applicant speculates that the reason may be that the present invention first subjects the Al powder and the Fe powder to high-energy ball milling treatment and then evenly mixes the AlFe alloy powder and the Cr powder so that the metal Fe and Al are fully alloyed to form the AlFe alloy powder, effectively avoiding the heat release of the intense alloying reaction of the pure Al powder and the Fe powder, causing the Cr in the target material to react with the matrix Al to generate more brittle alloy phases, ensuring that there are fewer brittle alloy phases in the target material, thereby reducing the brittleness of the target material and improving the flexural strength of the target material.

[0152] (3) It can be seen from Example 1 and Comparative Example 3 that during the hot pressing sintering process, when the temperature of the first heating is too high, the oxygen content in the target material will increase.

[0153] (4) It can be seen from Example 1 and Comparative Example 4 that during the hot pressing sintering process, when the second heating temperature (sintering temperature) is too high, the bending strength of the target material will be reduced.

[0154] (5) It can be seen from Example 1 and Comparative Example 5 that when the ball milling time is too long, the oxygen content in the target material will increase.

[0155] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing a CrAlFe-based alloy target, characterized in that: The following steps are involved: S1, subjecting Al powder and Fe powder to high-energy ball milling to obtain pre-alloyed AlFe alloy powder; In step S1, first pre-evacuate to a vacuum degree of ≤0.1Pa, then fill with 0.5-2Pa of Ar gas, and perform high-energy ball milling under Ar gas protection, with a ball milling speed of 100-150r / min and a ball milling time of 20-40h; S2. Evenly mixing the AlFe alloy powder and the remaining raw material powder of the CrAlFe-based alloy target to obtain a CrAlFe-based alloy powder, wherein the remaining raw material powder of the CrAlFe-based alloy target is Cr powder or consists of Cr powder and X powder, and the X powder includes at least one of W powder, Mo powder, Ta powder, Nb powder, and V powder; The chemical composition of the CrAlFe-based alloy target material, in terms of atomic percentage, includes: Cr 10-70at%, Al 20-85at%, Fe 0-20at% and not 0at%, X 0-20at%, wherein X represents at least one of W, Mo, Ta, Nb, and V; S3, hot pressing and sintering the CrAlFe-based alloy powder under vacuum conditions, releasing the pressure after the hot pressing and sintering, and then cooling and demolding to obtain a CrAlFe-based alloy sintered billet; The pressure relief includes maintaining the pressure and cooling to 400-460°C, and then linearly releasing the pressure to a pressure of 0 MPa; the maximum sintering temperature of the hot pressing sintering is 500-600°C; The hot pressing sintering comprises: firstly, applying an initial pressure of 5-12Mpa to the CrAlFe-based alloy powder at room temperature, and evacuating the pressure to 0.1-0.5Pa, and then performing vacuum hot pressing sintering, heating the temperature from room temperature to 120-180°C, with a heating rate of 1-5°C / min, and starting the timing of heat preservation and pressure holding when the vacuum degree reaches 0.01Pa-0.05Pa, and the heat preservation and pressure holding time at 120-180°C and 5-12Mpa is 1-5h, and then continuing to heat and hold the temperature at a heating rate of 2-10°C / min to a sintering temperature of 500-600°C, and at the same time linearly increasing the pressure to a sintering pressure of 20-50MPa, and keeping the temperature and pressure at 500-600°C and 20-50MPa for 1-6h; S4, machining the CrAlFe-based alloy sintered blank to obtain the CrAlFe-based alloy target; The purity of the Fe powder is ≥99.5wt%, and the FSSS of the Fisher grain size is 5-8μm; the Al powder is air atomized aluminum powder, with a purity of ≥99.7wt% and a particle size of -200 mesh; the purity of the Cr powder is ≥99.8wt%, and the particle size is -200 mesh; the purity of the W powder is ≥99.9wt%, and the FSSS of the Fisher grain size is 5-8μm; the purity of the Mo powder is ≥99.9wt%, and the FSSS of the Fisher grain size is 5-8μm; the purity of the Ta powder is ≥99.8wt%, and D50 is 15-20μm; the purity of the Nb powder is ≥99.5wt%, and the particle size is -300 mesh; the purity of the V powder is ≥99.8wt%, and the particle size is -325 mesh.

2. The method for preparing a CrAlFe-based alloy target according to claim 1, characterized in that: In step S1, the ball milling medium includes one of a zirconia ball, a steel ball, and a stainless steel ball, and the diameter of the ball milling medium is 20-30 mm.

3. The method for preparing a CrAlFe-based alloy target according to claim 1, characterized in that: In step S1, the mass ratio of the ball to the material is (10-20):

1.

4. The method for preparing a CrAlFe-based alloy target according to claim 1, characterized in that: In step S1, after the high-energy ball milling treatment is completed, the AlFe alloy powder is sieved to remove large particles of the powder, wherein the aperture of the sieve is 1-2 mm.

5. The method for preparing a CrAlFe-based alloy target according to claim 1, characterized in that: In step S2, the mixing is carried out in a mixer by adding zirconium oxide balls for dry mixing, the ball-to-material mass ratio of the zirconium oxide balls is 1:(5-10), and the mixing time is 3-10 hours, wherein the mixer is at least one of a universal motion mixer, a three-dimensional mixer, and a double cone mixer.

6. The method for preparing a CrAlFe-based alloy target according to claim 1, characterized in that: In step S3, the pressure relief time is 20 min-60 min.

7. The method for preparing a CrAlFe-based alloy target according to claim 1, characterized in that: In step S3, the cooling and demoulding include: air cooling in the furnace after pressure relief, and demoulding after the furnace temperature is below 200°C.

8. The method for preparing a CrAlFe-based alloy target according to claim 1, characterized in that: In step S4, the size of the CrAlFe-based alloy target is D (60-300) mm*(10-40) mm.

9. A CrAlFe-based alloy target, characterized in that: The CrAlFe-based alloy target is made by the preparation method described in any one of claims 1-8.