Lithium ion battery aqueous binder, and preparation and application of negative electrode plate
By reacting in situ with the oxide on the copper foil surface, the problem of insufficient performance of the negative electrode binder of lithium-ion battery in the electrochemical process is solved, and the cycle stability and first circle of the electrode are improved Coulomb efficiency reduces the risk of electrode depowder and optimizes the mechanical properties of the electrode, achieving environmentally friendly and economical battery performance improvement.
Patent Information
- Application Number
- CN202410877360.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-08
AI Technical Summary
Existing lithium-ion battery negative electrode binders such as PVDF and PAA have insufficient performance in the electrochemical process, resulting in poor electrode cycle stability, low first-circuit Coulon efficiency and electrode depowder problems, and their cost and environmental impact are poor.
Partially neutralized polyacrylic acid (PAA) is used as the binder to form strong ionic bonds by reacting in situ with oxides on the copper foil surface, improving the bonding force between the electrode and the current collector, and optimizing the electrode by adjusting the neutralization degree mechanical and electrochemical properties.
It significantly improves the first-circle Coulomb efficiency and cycle stability of the electrode, extends the cycle life of the electrode, reduces the risk of cracking and depowdering of the electrode, and reduces production costs, and is environmentally friendly.
Smart Images

Figure CN118909573A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy materials, and in particular relates to an aqueous binder for a negative electrode of a lithium ion battery, a preparation method and an application test. Background Art
[0002] As fossil fuel depletion and environmental pollution problems worsen, the world attaches great importance to the development and popularization of electric vehicles. Among many energy storage devices, lithium-ion batteries stand out with their advantages of high energy efficiency, long life, portability and light weight, and have achieved great success in the past few decades. Among them, binders, as auxiliary materials in batteries, play a key role. The cost of binders is relatively low, generally accounting for only 2% to 5% of the total active material. Its main function is to firmly bond the electrode material to the metal current collector to enhance the close contact between the active material, the conductive agent and the current collector. At the same time, it stabilizes the electrode plate structure of the battery. Studies have found that although the binder accounts for a relatively small proportion in the battery, it plays a vital role in battery performance. Specifically, the binder can effectively prevent the active material from loosening or falling off during the charge and discharge process, thereby improving the cycle stability of the plate. In addition, the binder can also reduce the impedance of the battery, promote the diffusion rate of lithium ions, indirectly increase the specific capacity of the battery, and reduce capacity loss. Therefore, although the binder accounts for a small proportion in the overall formula, its importance in lithium-ion batteries cannot be ignored.
[0003] At present, the negative electrode current collector of commercial lithium-ion batteries mainly uses copper foil as the main material. The bonding strength of the negative electrode binder to the copper foil current collector directly affects the battery's cycle stability, initial performance (first efficiency) and cycle life. Polyvinylidene fluoride (PVDF) binder is one of the earliest commercial binders used in lithium-ion batteries, with excellent chemical stability and easy dispersion. Therefore, PVDF was widely used in graphite negative electrodes and became a standard polymer binder. However, PVDF can only use N-methylpyrrolidone (NMP) as a solvent, and NMP has a high volatile temperature and toxicity, which is unfavorable to the environment and has a high cost. In addition, the electrode active material is easily covered by partially crystallized polyvinylidene fluoride, in which the polyvinylidene fluoride in the crystallized area hinders the release or insertion of lithium ions. At the same time, due to the weak interaction between the active material and polyvinylidene fluoride, the distribution of the active material is uneven and agglomerates are easily formed. In addition, the swelling rate of PVDF in the electrolyte is high, and its mechanical properties and adhesion are poor, which has an adverse effect on the long-term use of the battery.
[0004] In recent years, polyacrylic acid (PAA) has become a research hotspot for negative electrode binders of lithium-ion batteries. It has a simple molecular structure, is easy to synthesize, has low cost, and is soluble in a variety of solvents such as water, ethanol and NMP. In carbonates, PAA exhibits low swelling and high elastic modulus. Because it contains abundant carboxyl groups (-COOH), it can form strong hydrogen bonds with the hydroxyl groups on the surface of the active material, giving it superior adhesion and mechanical properties, which is better than the traditional binder PVDF. In addition, PAA can also form one or more coating layers on the surface of the active material, acting as an artificial SEI, which helps to improve the performance of the battery. However, the first effect of the battery is usually affected by the content of carboxyl groups (-COOH) in the battery binder, because the carboxyl groups may undergo oxidation or reduction side reactions during the electrochemical process. Secondly, the rheological properties of the battery negative electrode slurry are also affected by the content of carboxyl groups (-COOH) in the battery binder, causing it to exhibit the characteristics of a non-Newtonian fluid at different strain rates, increasing the difficulty of stirring and mixing, and thus leading to uneven coating distribution. In addition, PAA has low viscosity to the copper foil current collector and is very brittle, which can easily cause cracks in the negative electrode during the charge and discharge process. Moreover, its performance is significantly affected by conditions such as the electrode material ratio and pH value. Summary of the invention
[0005] The present invention develops a process for adjusting the degree of neutralization of a polyacrylic acid (PAA) binder in a lithium-ion battery and for in-situ cross-linking of a current collector. The process is simple, controllable, economical, and suitable for the preparation of negative electrode sheets. The tensile test verified that the binder can effectively enhance the bonding force between the electrode and the copper foil. The results of rheological mechanics tests showed that the process can adjust the stability of the slurry. By assembling a graphite-metal lithium half-cell using electrodes prepared with PAA and conducting a first-cycle constant current charge and discharge test, it was demonstrated that the process significantly improved the first-cycle coulomb efficiency performance of the electrode. In the long-cycle test, the PAA-graphite electrode designed by the process showed stable cycle performance, and no capacity decay occurred within 400 hours (100 cycles). It provides an effective solution to solve the cycle powder shedding of lithium-ion batteries and improve the first-cycle coulomb efficiency, and has excellent electrochemical properties.
[0006] A lithium ion battery negative electrode binder comprises PAA and water, wherein the carboxyl groups of the PAA are partially neutralized, and the neutralization degree is 0-100%.
[0007] The neutralization degree is preferably 50-95%, more preferably 70-80%.
[0008] In the binder, the mass percentage of PAA is in the range of 1-10%, preferably 3-8%.
[0009] The preparation method of the above-mentioned binder comprises the following steps: adding PAA into water and stirring the water at a stirring speed of 50-800 r / min, a stirring temperature of 20-90° C., and a stirring time of 1-10 hours.
[0010] The molecular weight of PAA is 10-10 million.
[0011] Partially neutralized PAA refers to PAA obtained by partially neutralizing it with an alkaline substance; the steps include: weighing and calculating the amount of carboxyl substances in an aqueous solution, and adding an alkali metal or alkaline earth metal hydroxide salt according to a stoichiometric ratio to carry out a neutralization reaction to obtain it.
[0012] The alkaline substance is K-containing + 、Na + NH4 + , Ca 2+ 、Al 3+ One or more bases.
[0013] A method for regulating the bonding force between PAA and copper foil, wherein the surface of the copper foil contains a copper oxide layer, and the bonding force decreases with the increase of the neutralization degree of PAA and increases with the decrease of the neutralization degree of PAA; the step of bonding between PAA and copper foil comprises: applying the PAA adhesive on the copper sheet, heating and drying; the heating and drying conditions are: heating at 60-100°C for 2-4h.
[0014] A negative electrode slurry for a lithium battery comprises an electrode active material, a conductive agent, the above-mentioned binder and water.
[0015] The weight ratio of the electrode active material, the conductive agent and the above-mentioned binder is 85-98:0.5-2:1-8.
[0016] The solid content of the slurry is 40-45% by mass.
[0017] The electrode active material is graphite; the conductive agent is carbon black.
[0018] A method for preparing a lithium battery graphite electrode comprises the following steps:
[0019] Step 1: Graphite electrode slurry is applied on copper foil using wire rod coating method with a loading of 7-9 mg / cm 2 ;
[0020] Step 2, air drying, placing in an air drying oven, and baking;
[0021] Step 3: punching the pole piece into an electrode;
[0022] Step 4: vacuum drying.
[0023] A method for regulating the bending resistance of a lithium battery graphite electrode comprises the following steps: preparing the electrode by regulating a binder containing PAA with different neutralization degrees, wherein the bending resistance increases with increasing neutralization degree and decreases with decreasing neutralization degree.
[0024] A method for improving the cohesion of a lithium battery graphite electrode comprises the following steps: preparing the electrode by regulating a binder containing PAA with different neutralization degrees, wherein the neutralization degree is preferably 70-80%.
[0025] Beneficial Effects
[0026] Using partially neutralized PAA aqueous solution as a binder for graphite electrodes has multiple advantages. First, through in-depth research, we found that the increase in neutralization can significantly improve the first-cycle coulomb efficiency of the electrode, which can be increased to 93.24% when gradually increasing from 0% to 100%; second, the increase in neutralization helps to improve the stability of electrode cycles, and high-neutralized graphite electrodes show a high level of stability in both specific capacity and efficiency; third, the unneutralized carboxyl groups can react in situ with trace copper oxide on the surface of the copper foil as the current collector, thereby improving the bonding force between the electrode and the current collector and improving the cracking and powdering problems of the electrode during the cyclic charge and discharge process. In order to strike a balance between electrochemical and mechanical properties, we chose a PAA binder with a neutralization degree of 75%. In terms of electrochemical properties such as specific capacity, first-cycle coulomb efficiency and cycle stability, the 75% neutralized PAA showed a performance level close to that of the 100% neutralized PAA. In addition, rheological studies also show that with the increase of neutralization degree, the graphite slurry has a higher viscosity at low shear speed, so the slurry is less likely to settle, which improves the stability of the slurry and makes it more conducive to scale-up production. Therefore, we use a polyacrylic acid binder with a neutralization degree of 75% to consider both the mechanical and electrochemical properties of the electrode and improve the energy density and cycle stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 .Reaction mechanism diagram of multi-polymers of acrylic acid and its derivatives.
[0028] Figure 2 Morphology of commercial copper foil. a) Optical photo of copper foil; (b, c) SEM image of copper foil surface; d) SEM image of copper foil cross section.
[0029] Figure 3 Characterization of copper foil surface composition. a) Cu2p spectrum of copper foil surface XPS. b) LMM spectrum of copper foil surface XPS. c) XRD spectrum of copper foil surface. (d, e) EDS spectrum of copper foil surface and cross section.
[0030] Figure 4Pictures of PAA with a neutralization degree of 40% and copper oxide mixed and stirred at different temperatures. a) Picture of stirring at room temperature for 30 minutes. b) Picture of stirring at 70℃ for 30 minutes. c) Picture of stirring at 80℃ for 30 minutes. d) Picture of stirring at 80℃ for 30 minutes and then settling.
[0031] Figure 5 Images of PAA with different neutralization degrees mixed with copper oxide at 80°C for 30 min. (a-f) are PAA with 0%, 15%, 40%, 60%, 75%, and 100% neutralization degrees, respectively.
[0032] Figure 6 Rheological and mechanical properties test diagram. a) Mechanical test diagram of the bonding force between PAA and copper sheet with different neutralization degrees. b) Mechanical test diagram of the bonding force between PAA and copper sheet at different temperatures. c, d) Rheological property curves of graphite electrode slurry configured with PAA with different neutralization degrees. e, f) Rheological property curves of PAA aqueous solutions with different neutralization degrees.
[0033] Figure 7 Electrode bending resistance test diagram. a) Schematic diagram of electrode bending. b) Effect diagram of graphite electrodes with different neutralization degrees of PAA after bending 30,000 times. c) Electron micrograph of graphite electrode with 75% neutralization degree of PAA before bending. d) Electron micrograph of graphite electrode with 75% neutralization degree of PAA after bending.
[0034] Figure 8 Pole cohesion test diagram. a) Schematic diagram of pole cohesion test. b, c) Graphite electrode cohesion test diagram of 0%, 15%, 75% neutralization degree PAA. d) Photo of the tape state after the graphite electrode cohesion test of 0%, 15%, 75% neutralization degree PAA. e) Graphite electrode cohesion test diagram of 100% neutralization degree PAA. f) Photo of the pole piece and tape state after the graphite electrode cohesion test of 100% neutralization degree PAA.
[0035] Fig. 9 Bending test of PAA graphite electrode with 75% neutralization degree. a) Electrode after coating. b) Prepared electrode sheet. c) Schematic diagram of electrode sheet bent once, twice, and three times. d) Schematic diagram of electrode sheet unfolded after bending.
[0036] Fig.10 Capacity-voltage diagrams of the first-cycle charge-discharge of half-cells assembled with graphite electrodes using PAA with different neutralization degrees. (a-f) PAA with neutralization degrees of 0%, 15%, 40%, 60%, 75%, and 100% respectively.
[0037] Fig.11Electrochemical test performance diagram. a) Cyclic specific capacity diagram of PAA assembled half-cells with different neutralization degrees. b) Cyclic efficiency diagram of PAA assembled half-cells with different neutralization degrees. c) AC impedance diagram of PAA assembled half-cells with different neutralization degrees. d) Cyclic voltammetry test diagram of PAA assembled half-cell with 75% neutralization degree. e) Cyclic efficiency-specific capacity diagram of 100 cycles of PAA assembled half-cell with 75% neutralization degree.
[0038] Fig.12 Comparison of the electrode pieces before and after cycling using a graphite electrode with a neutralization degree of 75% PAA. a) Photo and SEM image of the electrode piece before cycling. b) Photo and SEM comparison of the electrode piece after cycling. DETAILED DESCRIPTION
[0039] Lithium-ion batteries generally face the challenge of volume expansion of electrode active materials in practical applications, which in turn leads to cracking and powdering of electrode sheets. In addition, the first-cycle coulomb efficiency of the battery is also a crucial issue. A low first-cycle coulomb efficiency may cause excessive lithium insertion capacity, resulting in additional loss of positive electrode active materials, thereby reducing the energy density of the battery. Currently, the widely used binders, such as PVDF, CMC, SBR, etc., mainly have intermolecular forces between them and copper foil, which are relatively weak, so it is difficult to effectively overcome the problem of electrode powdering during the cycle.
[0040] Copper foil is a metal that is easily oxidized, and there is usually a trace amount of oxide (CuO) on its surface. This technology proposes a PAA binder containing carboxyl groups, which reacts in situ with the oxide on the surface of the copper foil to transform the interaction between the electrode and the current collector from intermolecular forces to stronger ionic bonds, thereby improving the mechanical properties of the electrode.
[0041] Synthesis of polyacrylate:
[0042] In the following examples, the PAA (without neutralization treatment) used is synthesized in the following manner, and its basic physical and chemical parameters are: the PAA used is a water-based binder of polyacrylic acid or polyacrylate obtained by copolymerization of monomer acrylic acid and functional monomer, characterized in that the water-based binder comprises: 1-100 parts of monomer acrylic acid, 0-100 parts of functional monomer, 50-500 parts of water, 0-10 parts of cross-linking agent, 0.1-10 parts of initiator, and 0-20 parts of emulsifier. The functional monomer is one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, isooctyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, propylene acetate, acrylonitrile, methacrylonitrile, styrene, methyl styrene, and acrylamide. The initiator is one or more of potassium persulfate, ammonium persulfate, sodium persulfate, benzoyl peroxide, lauroyl peroxide, dimethyl azobisisobutyrate, and azobisisobutyronitrile. The emulsifier is one or more of phosphate, alkylbenzene sulfonate, and polyoxyethylene ether. The PAA preparation method comprises: reacting monomer acrylic acid, functional monomer, water, crosslinking agent, initiator, and emulsifier at a reaction temperature of 20 to 90° C. and a stirring speed of 50 to 800 r / min for 1 to 10 hours to obtain a water-based binder of polyacrylic acid or polyacrylate.
[0043] like Figure 1 , the reaction mechanism diagram of acrylic acid and its derivative multi-polymer, specifically: acrylic acid monomer or acrylate monomer or acrylic acid functional monomer, one or more monomers undergo polymerization reaction. The polymerization reaction is carried out in solvent water, in the presence of a crosslinker, initiator, and emulsifier, and the reaction conditions are a reaction temperature of 20 to 100 degrees Celsius, a stirring speed of 50 to 2000 r / min, and a reaction time of 1 to 8 hours. Its reaction mechanism is that the initiator is heated and decomposed to produce free radicals, which serve as the beginning of the polymerization reaction and cause a series of chain reactions, such as one or more monomers polymerizing into polymers, and polymers and monomers or polymers forming long chains. When there are no free radicals in the outside world or the free radical concentration is too low, the polymerization reaction cannot continue to expand, and the chain reaction gradually decays until it stops.
[0044] In the following examples, the preparation process of PAA used is:
[0045] Step 1) Prepare the reaction solution: add 670 g of water, 8 g of acrylic acid, and 56 g of potassium polyacrylate into a 1000 mL beaker and stir evenly.
[0046] Step 2) Prepare an initiator aqueous solution: add 0.3 g of potassium persulfate to 60 g of water and dissolve.
[0047] Step 3) Build a reaction apparatus: Add the reaction solution into a 1000 mL four-necked round-bottom flask and install a mechanical stirrer, a thermometer, a constant pressure dropping funnel, and a condenser.
[0048] Step 4) Reaction: Heat the reaction solution to 70-73°C, stir at 500 r / min, and start dripping the initiator aqueous solution at a drip rate of 1 mL / min. Continue the reaction for 7 hours, then turn off the heating, cool to room temperature, and collect the material.
[0049] According to the above preparation method of PAA, PAA with different neutralization degrees is synthesized, and the neutralization degrees are 0%, 15%, 40%, 60%, 75%, and 100% from small to large.
[0050] Comparative test of the reaction between PAA and copper oxide:
[0051] First, commercial copper foil was selected as the experimental material. It has a smooth surface and a thickness of about 15 microns. Figure 2 To verify whether there is oxide on the surface of the copper foil, X-ray photoelectron spectroscopy was used to characterize the surface of the copper foil. Figure 3 (a) is the XPS spectrum of Cu2p orbital, in which strong copper oxide signals and Cu 2+ The satellite peaks of Figure 3 No signal related to cuprous oxide was observed in the Auger electron scanning spectrum of copper in (b). This shows that there is usually a trace layer of oxide on the surface of copper foil, and the oxide is copper oxide rather than cuprous oxide. The surface of copper foil was characterized and analyzed using X-ray diffraction technology. The X-ray diffractometer used was Bruker D8, with Cu Kα as the radiation source, a scanning range of 20-80°, and a scanning speed of 2°min -1 .exist Figure 3 In (c), 44.51°, 50.53° and 73.97° correspond to the 111 plane, 200 plane and 220 plane of copper, respectively, while a weak signal appears at 38.73°, which is consistent with the characteristic peak of copper oxide (PDF#01-089-2529). The copper foil surface was further tested using energy spectrum analysis, such as Figure 3 As shown in (d), there is a signal of oxygen on the surface of the copper foil. It can be seen that there is usually a trace layer of oxide on the surface of the copper foil, and the oxide is cupric oxide rather than cuprous oxide. Figure 3 (e) shows a fresh cross-section of the cut copper foil. After being placed in air at room temperature for one day, the energy spectrum shows the presence of oxygen signals, indicating that the copper foil is extremely easy to oxidize.
[0052] In the present invention, the specific steps of neutralizing PAA are as follows: First, the amount of carboxyl substances in the aqueous solution is weighed and calculated. Then, sodium hydroxide powder is added in proportion, and a stirrer is used at room temperature with a rotation speed maintained in the range of 50-800 r / min for 0.5 to 2 hours. The neutralization degree is calculated as the amount of neutralized carboxyl substances / the total amount of carboxyl substances.
[0053] In order to further study the reaction conditions between the carboxyl group in PAA and copper oxide, this experimental scheme selected PAA with a neutralization degree of 40% and diluted it into a 0.6% aqueous solution by mass. The specific operation is to take 100g of 0.6% PAA aqueous solution and 0.1g of copper oxide powder and place them in a round-bottom flask, heat them in an oil bath, and stir them with a rotor. After stirring at room temperature for 30 minutes, Figure 4 As shown in (a), the solution did not show obvious changes; after stirring at 70°C for 30 minutes, Figure 4 As shown in (b), the solution did not change significantly; after stirring at 80°C for 30 minutes, Figure 4 As shown in (c), the solution turned blue obviously, and a blue clear solution was obtained after standing and settling. It can be concluded that the carboxyl groups in PAA react more easily with copper oxide at 80°C. Subsequently, we used PAA with different neutralization degrees, diluted it into a 0.6% by mass aqueous solution, and stirred it with copper oxide powder at 80°C for 30 minutes. Figure 5 As shown in the figure, as the neutralization degree of PAA decreases, the color of the solution changes from a colorless and transparent solution with 100% neutralization to a dark blue solution with 0% neutralization. This is because as the neutralization degree decreases, the number of unneutralized carboxyl groups increases, which reacts with more copper oxide, causing the blue color in the solution to deepen, indicating an increase in the concentration of copper ions. Therefore, we conclude that copper oxide reacts with unneutralized carboxyl groups in PAA, and the more carboxyl groups there are, the stronger the reaction.
[0054] Comparative test of adhesion:
[0055] The bonding strength between PAA and copper foil was tested. Since copper foil is relatively soft, this technology uses a copper plate of the same material as copper foil, with a specification of 1×20×70mm. Figure 6 The copper plates coated with the adhesive were stacked together as shown in (a), and the middle was coated with a 5% by mass PAA adhesive, with a coating area of 20×40 mm. The copper plates coated with the adhesive were stacked together, placed on a heating table and heated for 4 hours, and then subjected to a tensile test. First, we conducted a tensile strength test between the PAA with different neutralization degrees and the copper plates, as shown in Figure 6As shown in (a), its tensile strength was tested. The results showed that the tensile strengths of PAA with a neutralization degree of 0%, 15%, 75%, and 100% were 191N, 100N, 51N, and 38N, respectively. The lower the neutralization degree of the PAA binder, the more carboxyl groups it contains. The bonding force between the binder and the current collector is effectively improved by the in-situ reaction of the carboxyl groups with the oxides on the surface of the copper plate. In addition, we tested the tensile strength of PAA with a neutralization degree of 75% with the copper plate at different temperatures, as shown in FIG. Figure 6 As shown in (b), the bonding force of PAA to the copper plate at 60°C and 70°C is similar, 27N and 30N respectively. When the temperature rises to 80°C and 90°C, the bonding force of PAA to the copper plate increases significantly, 51N and 53N respectively. This further proves that the unneutralized carboxyl groups of PAA can react with the oxides on the surface of the copper plate, significantly increasing the interaction between the binder and the current collector, and the reaction temperature is 80°C, which is consistent with the reaction temperature of PAA and copper oxide powder mentioned above.
[0056] Rheological properties comparison test:
[0057] The test was conducted with 5% PAA binder. In order to apply the binder to the negative electrode of lithium-ion batteries, we selected the most widely used commercial graphite electrode as the main material and prepared graphite electrode slurries using PAA binders with different neutralization degrees.
[0058] The preparation steps of graphite slurry are as follows: 1) Weigh a certain mass of graphite powder, Super P conductive carbon black powder and 5% PAA aqueous solution (PAA in the mass ratio is the mass of pure PAA) in a mass ratio of 95:2:3. In this process, the amount of PAA aqueous solution added is calculated based on the pure PAA solid mass and solution concentration; 2) Put the weighed mixture into a beaker and stir it mechanically by using a stirrer to ensure that it is evenly dispersed. In this process, the stirring condition is a speed of 800r and a stirring time of 8 hours.
[0059] The fluid properties at room temperature were tested by rheometer. Figure 6 (c, d) show that the higher the neutralization degree of PAA, the stronger the shear force of the corresponding graphite slurry and the greater the viscosity, which is more obvious at low shear speed. The higher the neutralization degree, the higher the viscosity of the graphite slurry at low shear speed, the less likely the slurry will settle, and the better the stability. Therefore, PAA binders with high neutralization degree are easier to scale up the production and preparation of graphite electrodes.
[0060] In addition, the rheological properties of PAA aqueous solution also have a significant correlation with the degree of neutralization, such as Figure 6(e, f) show the rheological characteristic curves of pure PAA aqueous solution. The results show that the higher the neutralization degree, the stronger the shear force of the PAA aqueous solution and the greater the viscosity. In the previous test of the bonding strength between PAA and the copper plate, the higher the neutralization degree of PAA, the weaker the bonding strength, which is opposite to the change rule that the higher the neutralization degree of PAA, the greater the viscosity in the rheological test. This further proves that in the test of the bonding strength between PAA and the copper plate, the bonding strength has nothing to do with the viscosity of PAA, and the bonding strength is positively correlated with the amount of carboxyl groups in PAA, that is, the unneutralized carboxyl groups of PAA can react with the oxide layer on the surface of the copper plate to improve its bonding strength.
[0061] Pole piece bending resistance test:
[0062] The bending resistance of graphite electrodes with different neutralization degrees of PAA was tested. Figure 7 (a) is a schematic diagram of a bending test, in which the prepared graphite electrode is repeatedly bent 30,000 times using a bending test machine.
[0063] The graphite electrode preparation method is as follows: 1) Weigh a certain mass of graphite powder, Super P conductive carbon black powder and 5% PAA aqueous solution (PAA in the mass ratio is the mass of pure PAA) in a mass ratio of 95:2:3. In this process, the amount of PAA aqueous solution added is calculated based on the pure PAA solid mass and the solution concentration; 2) Put the weighed mixture into a beaker and stir it mechanically using a stirrer to ensure that it is evenly dispersed. In this process, the stirring condition is a speed of 800r and a stirring time of 8 hours. 3) The prepared slurry is evenly coated on the copper foil by wire rod coating, and the active material loading is 7-9mg / cm -2 4) Place the coated electrode in a forced air oven at 85°C for 2 hours for drying test.
[0064] After the graphite electrodes prepared with different neutralization degrees of PAA were bent 30,000 times, Figure 7 (b), the graphite electrode with 0% PAA neutralization degree cracked severely and showed obvious powdering; the graphite electrode with 15% PAA neutralization degree showed slight cracking and powdering; the graphite electrodes with 75% and 100% PAA neutralization degrees did not show obvious cracking and powdering. Further, the microstructure of the graphite electrode with 75% PAA neutralization degree before and after bending was tested using a scanning electron microscope, as shown in Figure 2. Figure 7 As shown in (c, d), after the pole piece was magnified to 100-2000 times, it was found that the microscopic morphology of the pole piece did not change significantly before and after bending. This test shows that the higher the neutralization degree of PAA, the stronger the bending resistance of the corresponding graphite electrode. Although the neutralization degree of 0% and 15% has a stronger force with the current collector, it will weaken the cohesion between the graphite electrode powders.
[0065] Pole cohesion test:
[0066] The cohesion test was conducted on graphite electrodes with different neutralization degrees of PAA. The graphite electrodes are the same as those used in the bending resistance test of the electrode. Figure 8 (a) shows a schematic diagram of the cohesion test. The electrode is cut into 20*70mm strips, the copper foil side is pasted on the hard copper plate, and fixed to the clip below the tensile testing machine. A 15mm wide tape is pasted on the graphite electrode side and fixed above the tensile testing machine for a 180° tensile peeling test.
[0067] The cohesion test results are as follows: Figure 8 As shown in (b, c), the cohesive forces of graphite electrodes with 0%, 15% and 75% PAA neutralization degrees are 0.055 N, 0.527 N and 1.259 N respectively. The higher the neutralization degree, the stronger the cohesive force of the electrode and the correspondingly stronger the bending resistance. Figure 8 (d) is the tape state diagram after the graphite electrodes with 0%, 15% and 75% PAA neutralization degree were tested. It can be seen that the graphite electrode with 0% PAA neutralization degree has the most tape peeling powder, while the graphite electrode with 75% neutralization degree has the least tape peeling powder, which further illustrates that the higher the PAA neutralization degree, the stronger the cohesion of the electrode. However, when using PAA with a neutralization degree of 100%, such as Figure 8 The measured peeling force shown in (e) is only 0.591N. This is because the force between the 100% neutralized PAA and the current collector is small, causing the tape to peel the powder off the copper foil surface. Figure 8 (f) The graphite electrode with 100% neutralization degree of PAA exposed the yellow copper foil current collector after being taped, and the amount of powder after the tape was peeled off was greater than that of the corresponding graphite electrode with 75% neutralization degree. Therefore, the higher the neutralization degree of PAA, the better. When the neutralization degree is 100%, the interaction between the electrode and the current collector is weak, which is not conducive to large-scale production and application.
[0068] Furthermore, we conducted destructive bending tests on graphite electrodes bonded with 75% neutralized PAA. Fig. 9 (a) and (b) show the coated large graphite electrode and the electrode disc impacted by the grinding tool. After 1 to 3 bending tests (such as Fig. 9 After unfolding, it was observed that the electrode did not lose powder or crack at the fold (as shown in c). Fig. 9d), which indicates that the electrode material and the current collector are tightly bonded. In previous tests, we have demonstrated that the carboxyl groups in the PAA binder can react with copper oxide at relatively low temperatures. At the same time, the surface of the copper foil usually has a layer of copper oxide. Therefore, the tight bond between the electrode material and the current collector in this experiment is attributed to the small amount of carboxyl groups (-COOH) retained in the PAA binder, which can react in situ with the copper oxide (CuO) on the surface of the copper foil current collector at an appropriate temperature to form a covalent crosslinking effect (-COO – ···Cu 2+ ··· – OOC-), thereby significantly improving the bonding force between the electrode material and the current collector, and obtaining a graphite electrode with stronger mechanical properties.
[0069] Assembly and performance testing of half-cells:
[0070] Graphite electrodes were prepared using PAA binders with different neutralization degrees, and graphite‖metal lithium half-cells were further assembled.
[0071] The preparation method of graphite negative electrode sheet is as follows: 1) Weigh a certain mass of graphite powder, Super P conductive carbon black powder and PAA aqueous solution respectively according to the mass ratio of 95:2:3, wherein the amount of PAA aqueous solution added is calculated according to the pure PAA solid mass and solution concentration. 2) Put the weighed graphite and Super P into a mortar and grind them to mix evenly, and then add the above-mentioned PAA binder. 3) Add an appropriate amount of deionized water and grind to ensure that the mixture is evenly dispersed. 4) Spread the copper foil flat on the glass plate, and use the wire rod coating method to scrape the ground graphite slurry, with an active material loading of 7-9 mg / cm -2 5) Place the coated electrode in a blast oven at 85°C and heat for 2 hours. 6) Punch the electrode into an electrode with a diameter of 8mm using a manual slicer for button cells. 7) Vacuum dry the electrode in a vacuum oven at 120°C for 8 hours and quickly transfer it to a glove box. The atmosphere in the glove box is high-purity argon, and the water and oxygen content is less than 0.01ppm.
[0072] The assembly method of graphite ‖ metal lithium half-cell is as follows: assemble according to the following battery structure: CR2025 negative electrode shell, spring, gasket, lithium sheet, commercial PP separator, graphite electrode and CR2025 positive electrode shell. During the assembly process, first attach the lithium sheet to the surface of the gasket, and then use a punch to apply pressure to ensure close contact between the current collector and the lithium sheet. Pour the electrolyte for lithium-ion batteries (1M LiPF6 in DEC:DMC:EC=1:1:1Vol%with 5%FEC). Use a battery packaging machine for sealing. Both the spring and gasket are made of stainless steel. The entire assembly process is carried out in a glove box with a high-purity argon atmosphere and a water and oxygen content of less than 0.01ppm.
[0073] The batteries were tested with a CT3002A blue battery test system for the first cycle of constant current charge and discharge at a test rate of 0.05C. Fig.10 In the experiment, the first cycle coulombic efficiency of graphite-metal lithium half-cells with neutralization degrees of 0%, 15%, 40%, 60%, 75%, and 100% were 78.74%, 87.64%, 90.05%, 90.81%, 92.26%, and 93.24%, respectively. The increase in neutralization degree is conducive to the improvement of the first cycle coulombic efficiency. The first cycle charge specific capacity of different neutralization degrees is all within 340mA hg -1 The discharge capacity of half-cells using 0% and 15% PAA exceeded 400 mA hg -1 , resulting in a first-cycle coulombic efficiency of less than 90%. This is because the hydrogen on the unneutralized carboxyl groups in the binder has high activity and is easily replaced by lithium. During the battery discharge process, lithium ions are released from the lithium sheets and embedded in the graphite interlayers, while the hydrogen on the unneutralized carboxyl groups is replaced by lithium, resulting in additional discharge capacity, which reduces the first-cycle coulombic efficiency of the battery. Half-cells assembled using 75% and 100% PAA have similar first-cycle coulombic efficiencies, with the 75% neutralization degree being slightly lower.
[0074] In order to evaluate the cycling performance of PAAs with different neutralization degrees in the battery, we conducted a constant current charge and discharge test on the above half-cell at a charge and discharge rate of 0.5C. Fig.11 In (a), the cycle specific capacity diagram of the battery using different neutralization degrees of PAA is shown. In the initial 50 cycles, the lower the neutralization degree, the smaller the specific capacity. In particular, the specific capacity of the electrode with a neutralization degree of 15% is the lowest, only 200mA hg -1 However, the PAAs with 75% and 100% neutralization degree showed close and stable specific capacity performance in the battery, which could be maintained at a specific capacity of 340 mAh / g. Fig.11The coulombic efficiency test results shown in (b) show that the coulombic efficiency of the electrode with a neutralization degree of 15% fluctuates greatly during the cycle, indicating its poor stability. In contrast, PAA binders with neutralization degrees of 40%, 60%, 75%, and 100% exhibit high coulombic efficiencies close to 99.9% during the cycle. In order to test the effect of the binder on the battery impedance, we performed AC impedance tests on the graphite ‖ metal lithium half-cell. Fig.11 (c) shows an AC impedance graph, where the impedance of the PAA graphite half-cells with 0% to 100% neutralization degree is similar. Therefore, it can be concluded that the neutralization degree of the PAA binder has little effect on the half-cell impedance.
[0075] According to experimental data, the electrochemical performance of PAA with a neutralization degree of 75% and 100% in graphite‖lithium metal half-cells is relatively close, and the rheological curves of their electrode slurries meet the needs of large-scale coating. Therefore, under the premise of taking into account the mechanical and electrochemical properties of the electrode, we choose to use a PAA binder with a neutralization degree of 75% to ensure the electrochemical performance of the battery while improving the mechanical properties of the electrode, thereby effectively preventing cracking and powdering problems of the electrode during cycling. Fig.11 In (d), a cyclic voltammetry test using a half-cell with a neutralization degree of 75% PAA is shown. The battery can reach a relatively stable and strong cycling potential in the third cycle. Fig.11 As shown in (e), the battery using 75% neutralized PAA exhibits good cycling stability with a capacity of more than 340 mA hg -1 The specific capacity and coulombic efficiency are higher than 99.9%. Fig.12 The comparison of the negative electrode sheet of the graphite electrode after 100 cycles is shown. The electrode after the cycle was taken out and rinsed with dimethyl carbonate, and then vacuum-baked at 120°C for 2 hours before scanning electron microscopy. The results showed that the electrode did not crack after the cycle, and the small particles on the surface of the electrode became rough after the cycle, which may be due to the formation of a stable solid electrolyte layer on the electrode surface during the battery cycle. Overall, the graphite electrode using a 75% neutralized PAA binder showed good mechanical properties in long-term cycles.
[0076] In summary, the present invention proposes a novel lithium-ion battery polyacrylic acid system binder, a preparation method and an application test, which belong to the technical field of lithium-ion battery negative electrode binder materials. In the present invention, the polyacrylic acid binder is subjected to a partial neutralization process of sodium hydroxide and contains carboxyl groups, thereby improving the bonding force between the electrode and the copper foil without negatively affecting the performance of the electrode. By assembling a graphite-metal lithium half-cell, a longer cycle life can be achieved, while optimizing the first-cycle coulomb efficiency performance of the electrode, effectively solving the problem of electrode powder shedding. In addition, the process can also optimize the stability of the electrode slurry and has the potential for large-scale production.
Claims
1. A lithium ion battery negative electrode binder, characterized in that: Its components include PAA and water, and the carboxyl group of the PAA is partially neutralized with a neutralization degree of 0 to 100%.
2. The negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The neutralization degree is preferably 50-95%, more preferably 70-80%; the mass percentage of PAA is in the range of 1-10%, preferably 3-8%.
3. The negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The molecular weight of PAA is 10-10 million; partially neutralized PAA refers to PAA obtained by neutralizing part of the alkaline substance; the steps include: weighing and calculating the amount of carboxyl substances in the aqueous solution, and adding alkali metal or alkaline earth metal hydroxide salt according to the stoichiometric ratio to carry out neutralization reaction to obtain it.
4. The negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The alkaline substance is K-containing + 、Na + NH4 + , Ca 2+ 、Al 3+ One or more bases.
5. The method for preparing the negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The method comprises the following steps: adding PAA into water and stirring the water; the stirring speed is 50-800 r / min, the stirring temperature is controlled at 20-90° C., and the stirring time is 1-10 hours.
6. A method for regulating the bonding force between PAA and copper foil, characterized in that: The surface of the copper foil contains a copper oxide layer, and the bonding force decreases as the neutralization degree of PAA increases, and increases as the neutralization degree of PAA decreases; The step of bonding the PAA and the copper foil comprises: applying the PAA adhesive to the copper sheet, heating and drying; The conditions for heating and drying are: heating at 60-100℃ for 2-4h.
7. A negative electrode slurry for a lithium battery, comprising an electrode active material, a conductive agent, the binder according to claim 1 and water; the weight ratio of the electrode active material, the conductive agent and the above-mentioned binder is 85-98:0.5-2:1-8.
8. A method for preparing a lithium battery graphite electrode, characterized in that: The steps include: Step 1: Graphite electrode slurry is applied on copper foil using wire rod coating method with a loading of 7-9 mg / cm 2 ; Step 2, air drying, placing in an air drying oven, and baking; Step 3: punching the pole piece into an electrode; Step 4: vacuum drying.
9. A method for regulating the bending resistance of a lithium battery graphite electrode, characterized in that: The method comprises the following steps: preparing an electrode by regulating the lithium ion battery negative electrode binder according to claim 1 containing PAA with different neutralization degrees, and the bending resistance increases with the increase of the neutralization degree and decreases with the decrease of the neutralization degree.
10. A method for improving the cohesion of a lithium battery graphite electrode, characterized in that: The method comprises the following steps: preparing an electrode by adjusting the negative electrode binder of the lithium ion battery according to claim 1 containing PAA with different neutralization degrees, and the neutralization degree is preferably 70-80%.
Citation Information
Cited By
Binder and preparation method thereof, positive plate and battery
CN120484731A