A battery assembly, a photovoltaic assembly and a method for preparing the same

By using a multi-functional glue layer to cover the connecting wires and cells in photovoltaic modules, combined with different types of glue layers and process design, the problem of poor welding wire fixation is solved, and the power stability and production efficiency of the module are improved.

CN116093167BActive Publication Date: 2024-10-15HEYU RENEWABLE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211638376.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2024-10-15
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

In existing photovoltaic modules, the welding wire fixation method without main grid design has problems of point deviation and poor bonding, resulting in poor contact between the welding wire and the cells and auxiliary grid lines, affecting the production efficiency and electrical performance of the module.

Method used

Use a multi-functional glue layer to cover the connecting wires and cells. Through continuous or segmented full coverage design, different types of glue layers (adhesive layer, temperature-resistant layer, weather-resistant layer, photo-curing layer, etc.) are combined to improve adhesion and Stability, and through the process of heating, melting, and divided coating and solidification, ensures a firm connection between the welding wire and the battery piece.

Benefits of technology

It achieves stable fixation of the welding wire and the cells, improves the power stability and production efficiency of the module, reduces solar loss, and improves the fixation effect of the welding wire and the high toughness and toughness of the glue layer without affecting the power of the module. Weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116093167B_ABST
    Figure CN116093167B_ABST
Patent Text Reader

Abstract

The present invention discloses a battery assembly, a photovoltaic assembly and a preparation method thereof, wherein the battery assembly comprises a battery cell without a main grid and a welding wire, which are connected by a multifunctional glue layer, wherein the multifunctional glue layer covers the welding wire in a continuous full coverage or continuous segmented coverage in the length direction, and covers the welding wire in a full coverage in the width direction, and the multifunctional glue layer is distributed in sequence from the battery cell without a main grid to the welding wire as an adhesive layer and a composite layer, and the photovoltaic assembly comprises the above-mentioned battery assembly. The present invention adopts a design of full coverage of the welding wire in the battery assembly by a multifunctional layer, and through the design of the performance, function and thickness of the multifunctional layer, the welding wire and the battery cell can be stably and durably bonded together; in addition, the preparation of the photovoltaic assembly adopts the use of glue in batches and multiple coatings, which can not only solve the function of stabilizing and fixing the welding wire, but also take into account the hardness, flexibility and weather resistance of the entire ultra-thick glue coating, and the photovoltaic assembly has no obvious power attenuation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a photovoltaic module and a preparation method thereof, and in particular to a battery module, a photovoltaic module and a preparation method thereof. Background Art

[0002] In order to reduce costs and improve market competitiveness, existing photovoltaic modules have gradually eliminated the welding of the main grid of the battery cell and adopted a main grid-free design. The most critical point of the main grid-free design of the battery cell is that it does not require welding. How to fix the welding wire on the battery cell and ensure that the welding wire does not shift during the assembly process, and the welding wire can always be firmly bonded to the battery cell and the secondary grid line. Currently, most studies are on fixing the welding wire by dispensing glue, but none of them consider the problems of simply fixing the welding wire by dispensing glue.

[0003] Patent CN114765229 uses the steps of glue dispensing, wiring (welding wire), and fixing to directly contact the welding wire with the secondary grid line. This patent first dispenses glue and then wires. The glue at the dispensing position will inevitably lift the welding wire and vacate it on the battery cell and the fine grid line, thereby increasing the risk of poor contact between the welding wire and the battery cell and the secondary grid line. The more glue is dispensed and the more points are arranged, the greater the risk; the less glue is dispensed and the less points are arranged, the smaller the adhesion between the welding wire and the battery cell, and the greater the risk of poor contact caused by the welding wire offsetting the battery cell and the secondary grid line.

[0004] Patent CN114023842 adopts the method of first laying the welding wire, then hot pressing and melting, making the welding wire directly contact with the battery cell and the auxiliary grid line, and finally applying glue and curing. This patent improves the poor contact problem caused by applying glue first and then laying the welding wire. However, it is impossible to avoid the problem of offset during the application of glue and the inability to firmly bond the welding wire, battery cell and auxiliary grid line; in addition, most of the current glue application for bonding welding wire without main grid is not for the use of battery cell assembly factories. The thickness of the glue application is mostly much higher than the diameter of the welding wire, at least 300 microns or even thicker. Such thick glue application has a series of problems such as slow curing speed, poor adhesion, and poor weather resistance, which affects the production rhythm of the photovoltaic assembly factory and cannot guarantee the yield of the electrical performance of the welding wire and the auxiliary grid line. In addition, once some glue application fails to meet the standards in the batch construction process, it cannot be discovered in time, which is likely to cause rework of the entire component or even problems at the terminal. Summary of the invention

[0005] Purpose of the invention: In order to solve the technical problems existing in the prior art, the present invention aims to provide a battery assembly with high adhesion, excellent stability and no impact on performance. In addition, the present invention also provides a photovoltaic assembly composed of the battery assembly and a method for preparing the photovoltaic assembly.

[0006] Technical solution: The battery assembly described in the present invention includes a battery cell without a main grid and a welding wire. The battery cell without a main grid and the welding wire are covered and connected by a multifunctional glue layer. Within the length range of the multifunctional glue layer spread on each battery cell, the coverage mode in the length direction of the welding wire is continuous full coverage or continuous segmented coverage, and the coverage mode in the width direction of the welding wire is full coverage.

[0007] Furthermore, the coverage rate of the segmented coverage in the length direction is ≥70%, preferably, the coverage rate is ≥85%.

[0008] Furthermore, the thickness of the multifunctional glue layer is 0.4-2 times the height of the welding wire, and the width of the multifunctional glue layer is 1.1-2.5 times the width of the welding wire.

[0009] Furthermore, the multifunctional glue layer has a light transmittance of ≥85% and a refractive index of 1.40-1.52. Preferably, the light transmittance is ≥90% and the refractive index is 1.41-1.49. The volume resistivity of the multifunctional glue layer is 1.0×10 13-15 Ω·cm.

[0010] Furthermore, the multifunctional glue layer is distributed in sequence from the battery cell without main grid to the welding wire as a bonding layer and a composite layer, the bonding layer is coated with bonding glue, the composite layer is composed of more than one functional glue layer, preferably, the bonding glue is a light-curing glue, the composite layer is composed of one or more of a heat-resistant glue layer, a weather-resistant glue layer, and a high-toughness glue layer, preferably, the multifunctional glue layer includes a bonding layer, a heat-resistant glue layer and a weather-resistant glue layer, the bonding layer, the heat-resistant glue layer and the weather-resistant glue layer The thickness ratio of the weather-resistant glue layer to the height of the welding wire is (0.2-0.5):(0.2-1):(0.2-0.5); preferably, the multifunctional glue layer includes a bonding layer, a high-toughness glue layer, a weather-resistant glue layer and a heat-resistant glue layer, and the thickness ratio of the light-curing glue layer, the high-toughness glue layer, the heat-resistant glue layer and the weather-resistant glue layer to the height of the welding wire is (0.2-0.5):(0.1-0.8):(0.1-0.5):(0.1-0.5).

[0011] Furthermore, the raw materials of the light-curing glue include the following components by mass: 50-60 parts of aliphatic polyurethane acrylate, 20-30 parts of multifunctional acrylate monomer, 1-3 parts of secondary thiol, 1-2 parts of adhesion promoter, 1-2 parts of gas silicone and 8-10 parts of photoinitiator.

[0012] Furthermore, the raw materials of the heat-resistant glue include the following components in parts by mass: 60-70 parts of aliphatic polyurethane acrylate, 10-20 parts of propoxylated monofunctional acrylate monomer, 5-10 parts of aliphatic epoxy acrylate, 1-3 parts of secondary thiol PE-1, 0.1-1 parts of MAVT, 0.5-2 parts of antioxidant, 1-3 parts of gas silicon, 1-3 parts of ultraviolet light initiator, and 1-2 parts of cationic light initiator.

[0013] Furthermore, the raw materials of the weather-resistant glue include the following components by mass: 50-70 parts of aliphatic polyurethane acrylate, 20-40 parts of monofunctional acrylate monomer, 0.5-2 parts of secondary thiol, 1-3 parts of ultraviolet light absorber, 2-4 parts of gas silicon, and 1-4 parts of photoinitiator.

[0014] Furthermore, the raw materials of the high-toughness glue include the following components by mass: 40-60 parts of aliphatic polyurethane acrylate, 20-40 parts of propoxylated monofunctional acrylate monomer, 0.5-2 parts of secondary thiol PE-1, 2-4 parts of gas silicon H20, and 1-4 parts of photoinitiator.

[0015] The photovoltaic module of the present invention includes the above-mentioned battery module, and the preparation method includes the following steps:

[0016] (1) Arrange the welding wire on the battery cell according to the design requirements, and preliminarily connect the welding wire to the battery cell by heating and melting to achieve a certain electrical conduction;

[0017] (2) coating the welding wire with adhesive glue and then curing it to obtain an adhesive layer;

[0018] (3) coating the bonding layer and the welding wire with functional glue, and forming a composite layer after curing, that is, obtaining a battery cell and welding wire coated with a multifunctional glue layer, that is, a battery assembly;

[0019] (4) Connecting several battery modules in series to form interconnected units, coating and laminating them, assembling frames, and connecting components to form photovoltaic modules.

[0020] Furthermore, in the steps (1) to (4), the coating is performed in batches or multiple times.

[0021] Furthermore, compared with photovoltaic modules manufactured by conventional welding processes, the power attenuation of the photovoltaic modules is ≤0.01%, and there is no obvious power attenuation.

[0022] Principle of the invention: The glue dispensing process currently used to fix the welding wire has problems such as point offset and failure of some points that cannot be discovered in time, which poses a great hidden danger to the power stability of photovoltaic modules. The full-coverage welding wire used in the present invention completely avoids the risk of poor contact between the welding wire and the drain grid line. At the same time, in order to meet the functional requirements of fully covering and fixing high-thickness welding wires, the present invention has made adaptive development of the type and function of glue to meet the welding wire fixing glue required in different environments.

[0023] The multifunctional glue layer of the present invention has a light transmittance of ≥85%, or even ≥90%, which blocks little sunlight and greatly reduces the loss of sunlight reaching the battery cell. In order to better refract sunlight onto the battery cell and reduce light loss, the refractive index of the multifunctional glue layer of the present invention is controlled at 1.40-1.52, preferably 1.41-1.49, which can better change the light path and make greater use of the light source. The insulating effect of the multifunctional glue layer for fixing the welding wire affects the power loss of the battery assembly and can reduce the risk of local overheating of the welding wire and breakdown of the multifunctional glue layer. The volume resistivity of the multifunctional glue layer of the present invention is as high as 1.0×10 13-15 Ω·cm, which can better meet the needs of photovoltaic modules.

[0024] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0025] (1) The present invention adopts a design of full coverage of the multifunctional layer for the welding wire in the battery assembly. Through the performance, function and thickness design of the multifunctional layer, the welding wire and the battery cell can be stably and durably bonded together;

[0026] (2) The preparation of the photovoltaic module of the present invention adopts the method of applying glue in batches and multiple times, which can not only solve the function of stabilizing and fixing the welding wire, but also take into account the high toughness, temperature resistance and weather resistance of the entire ultra-thick glue coating, and the light transmittance of the glue after curing reaches ≥85%.

[0027] (3) The present invention has the effect of reducing the cost of busbar-free battery modules without affecting the module power. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a cross-sectional view of a battery cell and welding wire without a main grid in a battery assembly of the present invention;

[0029] Figure 2 This is a cross-sectional view of the battery cell and the bonding wire coated with the bonding layer in Example 1 of the present invention;

[0030] Figure 3 It is a cross-sectional view of a battery cell and a welding wire coated with an adhesive layer and a composite layer in Example 1 of the present invention;

[0031] Figure 4It is a cross-sectional view of the battery cell and welding wire coated adhesive layer and multi-layer composite layer in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with specific embodiments and drawings.

[0033] Example 1: Figure 1 As shown, the battery assembly of the present invention includes a battery cell without a main grid and a welding wire. The battery cell without a main grid is covered and connected with the welding wire by a multifunctional glue layer. The multifunctional glue layer provides continuous and full coverage to the welding wire in the length direction and full coverage to the welding wire in the width direction. The thickness of the multifunctional glue layer is 1.5 times the height of the welding wire, and the width of the multifunctional glue layer is 2.5 times the width of the welding wire.

[0034] The multifunctional glue layer is distributed in the direction from the battery cell without main grid to the welding wire in sequence: a light-curing glue layer, a heat-resistant glue layer and a weather-resistant glue layer. The thickness ratio of the light-curing glue layer, the heat-resistant glue layer and the weather-resistant glue layer to the welding wire height is 0.3:0.6:0.6 respectively.

[0035] The raw materials of the light-curing glue include the following components by mass: 60 parts of 16-functional aliphatic polyurethane acrylate CN2302NS, 26 parts of multifunctional acrylate monomer SR399NS, 2 parts of secondary thiol PE-1, 2 parts of adhesion promoter G40, 2 parts of gas silicon H20, 6 parts of photoinitiator 184 and 2 parts of photocatalyst TPO-L;

[0036] The raw materials of the heat-resistant glue include the following components by mass: 60 parts of aliphatic polyurethane acrylate CN9290NS, 20 parts of propoxylated monofunctional acrylate monomer SR611NS, 10 parts of aliphatic epoxy acrylate TTA16, 2 parts of secondary thiol PE-1, 0.5 parts of MAVT, 1.5 parts of antioxidant Irganox1010, 2 parts of gas silicon H20, 1 part of photoinitiator 184 and 2 parts of photoinitiator TPO-L, 1 part of cationic initiator Omnicat 320;

[0037] The raw materials of the weather-resistant glue include the following components by mass: 60 parts of aliphatic polyurethane acrylate CN9014NS, 30 parts of monofunctional acrylate monomer SR506HPNS, 1 part of secondary thiol PE-1, 2 parts of ultraviolet light absorber Tinuvin1130, 1 part of ultraviolet light absorber Tinuvin152, 2 parts of gas silicon H20, 3 parts of photoinitiator 184 and 1 part of photoinitiator TPO-L.

[0038] The photovoltaic module of the present invention includes the above-mentioned battery module, and the preparation method includes the following steps:

[0039] (1) Arrange the welding wire on the battery cell according to the design requirements, and initially connect the welding wire to the battery cell by heating and melting to achieve a certain electrical conduction, such as Figure 1 As shown;

[0040] (2) Apply light-curing glue to the welding wire and the battery cell through a screen with a set pattern, control the thickness of the light-curing glue to be 0.3 times the thickness of the welding wire, and then perform rapid light curing to fix the welding wire. After completion, a bonding layer is obtained, such as Figure 2 As shown;

[0041] (3) A composite layer (heat-resistant glue) is coated on the bonding layer and the welding wire, and the thickness of the composite layer (heat-resistant glue) is controlled to be 0.6 times the thickness of the welding wire, and then pre-curing is performed. After the pre-curing is completed, a composite layer (heat-resistant glue layer) is obtained. Figure 3 As shown;

[0042] (4) coating the composite layer (heat-resistant glue layer) and the welding wire with a composite layer (weather-resistant glue), controlling the thickness of the composite layer (weather-resistant glue) to be 0.6 times the thickness of the welding wire, and then curing the composite layer (weather-resistant glue layer) to obtain a composite layer (weather-resistant glue layer), that is, a battery cell and welding wire coated with a multifunctional glue layer, such as Figure 4 As shown, the battery assembly is obtained;

[0043] (5) Connecting several battery modules in series to form an interconnected unit, coating and laminating them, assembling them into a frame, and connecting them into a photovoltaic module. The multifunctional layer is heated and cured during the lamination of the module to complete the complete curing of the multifunctional glue layer.

[0044] Example 2: The battery assembly of the present invention includes a battery cell without a main grid and a welding wire. The battery cell without a main grid is covered and connected to the welding wire by a multifunctional glue layer. The coverage of the multifunctional glue layer on the length direction of the welding wire is continuous and segmented, with a coverage rate of 85%; the coverage on the width direction of the welding wire is full coverage, the thickness of the multifunctional glue layer is 0.4 times the height of the welding wire, and the width of the multifunctional glue layer is 1.1 times the width of the welding wire.

[0045] The multifunctional layer is composed of a multifunctional glue layer which is distributed in sequence from the battery cell without main grid to the welding wire, and is composed of two layers in total. The thickness ratio of the photocurable glue layer, the weather-resistant glue layer and the welding wire height is 0.2:0.2.

[0046] The raw materials of the light-curing glue include the following components by mass: 55 parts of 16-functional aliphatic polyurethane acrylate CN2302NS, 30 parts of multifunctional acrylate monomer SR399NS, 3 parts of secondary thiol PE-1, 1 part of adhesion promoter G40, 2 parts of gas silicon H20, 6 parts of photoinitiator 184 and 3 parts of photocatalyst TPO-L;

[0047] The raw materials of the weather-resistant glue include the following components by mass: 60 parts of aliphatic polyurethane acrylate CN9014NS, 30 parts of monofunctional acrylate monomer SR506HPNS, 0.5 parts of secondary thiol PE-1, 1 part of ultraviolet light absorber Tinuvin1130, 1 part of ultraviolet light absorber Tinuvin152, 3.5 parts of gas silicon H20, 1 part of photoinitiator 184 and 3 parts of photoinitiator TPO-L.

[0048] The photovoltaic module of the present invention includes the above-mentioned battery module, and the preparation method includes the following steps:

[0049] (1) Arrange the welding wire on the battery cell according to the design requirements, and initially connect the welding wire to the battery cell by heating and melting to achieve a certain electrical conduction, such as Figure 1 As shown;

[0050] (2) Apply light-curing glue to the welding wire and the battery cell through a screen with a set pattern, control the thickness of the light-curing glue to be 0.2 times the thickness of the welding wire, and then perform rapid light curing to fix the welding wire. After completion, a bonding layer is obtained, such as Figure 2 As shown;

[0051] (3) coating the bonding layer and the welding wire with a composite layer (weather-resistant glue), controlling the coating thickness of the composite layer (weather-resistant glue) to be 0.2 times the thickness of the welding wire, and then pre-curing, after which the composite layer (weather-resistant glue layer) is obtained, i.e., the battery cell and welding wire coated with the multifunctional glue layer are obtained, such as Figure 3 As shown, the battery assembly is obtained;

[0052] (4) Connecting several battery modules in series to form an interconnected unit, coating and laminating them, assembling them into a frame, and connecting them into a photovoltaic module. The multifunctional layer is heated and cured during the lamination of the module to complete the complete curing of the multifunctional glue layer.

[0053] Embodiment 3: The battery assembly of the present invention comprises a battery cell without a main grid and a welding wire. The battery cell without a main grid is connected to the welding wire by covering with a multifunctional glue layer. The covering mode of the multifunctional glue layer on the length direction of the welding wire is continuous segmented covering with a coverage rate of 70%; the covering mode on the width direction of the welding wire is full coverage, the thickness of the multifunctional glue layer is twice the height of the welding wire, and the width of the multifunctional glue layer is twice the width of the welding wire.

[0054] The multifunctional layer is composed of a multifunctional glue layer which is distributed in sequence from the battery cell without main grid to the welding wire, and is composed of 4 layers in total. The thickness ratios of the photocurable glue layer, the high-toughness glue layer, the heat-resistant glue layer and the weather-resistant glue layer to the welding wire height are 0.5:0.8:0.3:0.4 respectively.

[0055] The raw materials of the light-curing glue include the following components by mass: 60 parts of 16-functional aliphatic polyurethane acrylate CN2302NS, 30 parts of multifunctional acrylate monomer SR399NS, 1 part of secondary thiol PE-1, 1 part of adhesion promoter G40, 1 part of gas silicon H20, 2 parts of photoinitiator 184 and 5 parts of photocatalyst TPO-L;

[0056] The raw materials of the high-toughness glue include the following components by mass: 55 parts of aliphatic polyurethane acrylate CN8888NS, 40 parts of propoxylated monofunctional acrylate monomer SR395NS, 1 part of secondary thiol PE-1, 2 parts of gas silicon H20, 1 part of photoinitiator 184 and 1 part of photoinitiator TPO-L;

[0057] The raw materials of the heat-resistant glue include the following components by mass: 70 parts of aliphatic polyurethane acrylate CN9290NS, 15 parts of propoxylated monofunctional acrylate monomer SR611NS, 5 parts of aliphatic epoxy acrylate TTA16, 1 part of secondary thiol PE-1, 0.1 parts of MAVT, 2 parts of antioxidant Irganox1010, 2.9 parts of gas silicon H20, 1 part of photoinitiator 184 and 2 parts of photoinitiator TPO-L, 1 part of cationic initiator Omnicat 320;

[0058] The raw materials of the weather-resistant glue include the following components by mass: 70 parts of aliphatic polyurethane acrylate CN9014NS, 20 parts of monofunctional acrylate monomer SR506HPNS, 1.5 parts of secondary thiol PE-1, 0.5 parts of ultraviolet light absorber Tinuvin1130, 0.5 parts of ultraviolet light absorber Tinuvin152, 4 parts of gas silicon H20, 2 parts of photoinitiator 184 and 1.5 parts of photoinitiator TPO-L.

[0059] The photovoltaic module of the present invention includes the above-mentioned battery module, and the preparation method includes the following steps:

[0060] (1) Arrange the welding wire on the battery cell according to the design requirements, and preliminarily connect the welding wire to the battery cell by heating and melting to achieve a certain electrical conduction; Figure 1 As shown;

[0061] (2) Apply light-curing glue to the welding wire and the battery cell through a screen with a set pattern, control the thickness of the light-curing glue to be 0.5 times the thickness of the welding wire, and then perform rapid light curing to fix the welding wire. After completion, a bonding layer is obtained, such as Figure 2 As shown;

[0062] (3) A composite layer (high-toughness glue) is coated on the bonding layer and the welding wire, and the thickness of the composite layer (high-toughness glue) is controlled to be 0.8 times the thickness of the welding wire, and then pre-curing is performed. After the pre-curing is completed, a composite layer (high-toughness glue layer) is obtained. Figure 3 As shown;

[0063] (4) Coating the composite layer (high-toughness glue layer) and the welding wire with a composite layer (heat-resistant glue), controlling the coating thickness of the composite layer (heat-resistant glue) to be 0.3 times the thickness of the welding wire, and then pre-curing, after which the composite layer (heat-resistant glue layer) is obtained, such as Figure 4 As shown;

[0064] (5) coating the composite layer (heat-resistant glue layer) and the welding wire with a composite layer (weather-resistant glue), controlling the thickness of the composite layer (weather-resistant glue) to be 0.4 times the thickness of the welding wire, and then curing the composite layer (weather-resistant glue layer), and obtaining the composite layer (weather-resistant glue layer) after the curing, that is, obtaining the battery cell and welding wire coated with the multifunctional glue layer, that is, obtaining the battery assembly;

[0065] (6) Connecting several battery modules in series to form an interconnected unit, coating and laminating them, assembling them into a frame, and connecting them into components to form a photovoltaic module, wherein the multifunctional layer is heated and cured during the lamination of the module to complete the thorough curing of the multifunctional glue layer.

[0066] Embodiment 4: The battery assembly of the present invention comprises a battery cell without a main grid and a welding wire. The battery cell without a main grid is connected to the welding wire by covering it with a multifunctional glue layer. The multifunctional glue layer provides continuous and full coverage to the welding wire in the length direction and full coverage to the welding wire in the width direction. The thickness of the multifunctional glue layer is twice the height of the welding wire, and the width of the multifunctional glue layer is 2.5 times the width of the welding wire.

[0067] The multifunctional layer is composed of three layers, namely, a photocurable glue layer, a high-toughness glue layer, and a second high-toughness glue layer, which are distributed in sequence from the battery cell without a main grid to the welding wire. The thickness ratio of the photocurable glue layer, the high-toughness glue layer, and the second high-toughness glue layer to the welding wire height is 0.2:0.9:0.9 respectively.

[0068] The raw materials of the light-curing glue include the following components by mass: 60 parts of 16-functional aliphatic polyurethane acrylate CN2302NS, 30 parts of multifunctional acrylate monomer SR399NS, 1 part of secondary thiol PE-1, 1 part of adhesion promoter G40, 1 part of gas silicon H20, 2 parts of photoinitiator 184 and 5 parts of photocatalyst TPO-L;

[0069] The raw materials of the high-toughness glue include the following components by mass: 55 parts of aliphatic polyurethane acrylate CN8888NS, 40 parts of propoxylated monofunctional acrylate monomer SR395NS, 1 part of secondary thiol PE-1, 2 parts of gas silicon H20, 1 part of photoinitiator 184 and 1 part of photoinitiator TPO-L;

[0070] The photovoltaic module of the present invention includes the above-mentioned battery module, and the preparation method includes the following steps:

[0071] (1) Arrange the welding wire on the battery cell according to the design requirements, and preliminarily connect the welding wire to the battery cell by heating and melting to achieve a certain electrical conduction; Figure 1 As shown;

[0072] (2) Apply light-curing glue to the welding wire and the battery cell through a screen with a set pattern, control the thickness of the light-curing glue to be 0.2 times the thickness of the welding wire, and then perform rapid light curing to fix the welding wire. After completion, a bonding layer is obtained, such as Figure 2 As shown;

[0073] (3) A composite layer (high-toughness glue layer) is coated on the bonding layer and the welding wire, and the thickness of the composite layer (high-toughness glue layer) is controlled to be 0.9 times the thickness of the welding wire, and then pre-curing is performed. After the pre-curing is completed, the composite layer (high-toughness glue layer) is obtained. Figure 3 As shown;

[0074] (4) The composite layer (high-toughness glue layer) and the welding wire are coated with a composite layer (high-toughness glue layer) for the second time, and the thickness of the second composite layer (high-toughness glue layer) is controlled to be 0.9 times the thickness of the welding wire, and then pre-curing is performed. After the second composite layer (high-toughness glue layer) is obtained, that is, the battery cell and welding wire coated with the multifunctional glue layer are obtained, such as Figure 4 As shown, the battery assembly is obtained;

[0075] (5) Connecting several battery modules in series to form an interconnected unit, coating and laminating them, assembling them into a frame, and connecting them into a photovoltaic module. The multifunctional layer is heated and cured during the lamination of the module to complete the complete curing of the multifunctional glue layer.

[0076] Comparative Example 1: The difference from Example 1 is that the battery cell without main grid is connected to the welding wire only by dispensing commercial glue.

[0077] Comparative Example 2: The difference from Example 1 is that in the preparation method of the photovoltaic module: the glue is applied once, the coverage is 60%, the thickness of the glue layer is 0.1 times the thickness of the welding wire, and the width of the glue layer is 1.05 times the width of the welding wire.

[0078] Comparative Example 3: The difference from Example 1 is that the thickness ratio of the photocurable glue layer to the functional glue layer is 0.6:2.0, and the width of the multifunctional glue layer is 3 times the width of the welding wire.

[0079] The photovoltaic modules prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to performance tests, and the results are shown in Table 1. It can be seen from Table 1 that the transmittance of the multifunctional glue layer of Examples 1 to 4 is ≥85%, and the bonding strength is reliable. Even after the TC500 experiment, the welding wire remains firmly fixed, and the power of the photovoltaic module does not decrease. Comparative Example 1 uses commercial glue through a dispensing process, and the bonding stability of the welding wire is unreliable, especially after the TC cycle, the situation is more serious, and the power of the module is reduced to varying degrees during the whole process. Comparative Example 2 uses one printing of glue, and the glue coverage is too low and the thickness of the glue layer is too thin, resulting in limited welding wire fixing effect. After the TC cycle, the welding wire has poor bonding, and the module also has a power reduction phenomenon. It can be seen from Comparative Example 3 that although the multifunctional glue layer is too thick and has a positive effect on the fixation of the welding wire, it has a significant decrease in the transmittance of the glue layer and a significant decrease in the power of the module.

[0080] Table 1 Performance table of Examples 1 to 4 and Comparative Examples 1 to 3

[0081]

Claims

1. A photovoltaic module, characterized in that: The battery assembly comprises a battery cell without a main grid and a welding wire, wherein the battery cell without a main grid and the welding wire are connected by a multifunctional glue layer, wherein the multifunctional glue layer covers the welding wire in a continuous and full manner in the length direction and covers the welding wire in a full manner in the width direction, wherein the thickness of the multifunctional glue layer is 1.5 times the height of the welding wire, and the width of the multifunctional glue layer is 2.5 times the width of the welding wire; The multifunctional glue layer is distributed in the direction from the battery cell without main grid to the welding wire in sequence as a light-curing glue layer, a heat-resistant glue layer and a weather-resistant glue layer. The thickness ratio of the light-curing glue layer, the heat-resistant glue layer and the weather-resistant glue layer to the height of the welding wire is 0.3:0.6:0.6 respectively. The raw materials of the light-curing glue include the following components by mass: 60 parts of 16-functional aliphatic polyurethane acrylate CN2302NS, 26 parts of multifunctional acrylate monomer SR399NS, 2 parts of secondary thiol PE-1, 2 parts of adhesion promoter G40, 2 parts of gas silicon H20, 6 parts of photoinitiator 184 and 2 parts of photocatalyst TPO-L; The raw materials of the heat-resistant glue include the following components by mass: 60 parts of aliphatic polyurethane acrylate CN9290NS, 20 parts of propoxylated monofunctional acrylate monomer SR611NS, 10 parts of aliphatic epoxy acrylate TTA16, 2 parts of secondary thiol PE-1, 0.5 parts of MAVT, 1.5 parts of antioxidant Irganox1010, 2 parts of gas silicon H20, 1 part of photoinitiator 184 and 2 parts of photoinitiator TPO-L, 1 part of cationic initiator Omnicat320; The raw materials of the weather-resistant glue include the following components by mass: 60 parts of aliphatic polyurethane acrylate CN9014NS, 30 parts of monofunctional acrylate monomer SR506HPNS, 1 part of secondary thiol PE-1, 2 parts of ultraviolet light absorber Tinuvin1130, 1 part of ultraviolet light absorber Tinuvin152, 2 parts of gas silicon H20, 3 parts of photoinitiator 184 and 1 part of photoinitiator TPO-L; The photovoltaic module includes the above-mentioned battery module, and the preparation method includes the following steps: Arrange the welding wire on the battery cell according to the design requirements, and preliminarily connect the welding wire to the battery cell by heating and melting to achieve a certain electrical conduction; The light-curing glue is applied to the welding wire and the battery cell through a screen with a set pattern, and the thickness of the light-curing glue is controlled to be 0.3 times the thickness of the welding wire. The welding wire is then fast-cured and fixed, and a bonding layer is obtained after completion. A heat-resistant glue layer is applied to the bonding layer and the welding wire, and the thickness of the heat-resistant glue layer is controlled to be 0.6 times the thickness of the welding wire, and then pre-curing is performed to obtain a heat-resistant glue layer; A weather-resistant glue layer is coated on the temperature-resistant glue layer and the welding wire, and the thickness of the weather-resistant glue layer is controlled to be 0.6 times the thickness of the welding wire, and then cured. After the curing, a weather-resistant glue layer is obtained, that is, a battery cell and welding wire coated with a multifunctional glue layer, that is, a battery assembly is obtained; Several battery modules are connected in series to form an interconnected unit, and then coated and laminated and assembled into a photovoltaic module, wherein the multifunctional layer is heated and cured during the lamination of the module to complete the thorough curing of the multifunctional glue layer.