Copper foil with resin layer, and laminates using it.

By forming a resin layer with a specific composition and thickness on the surface of copper foil, the problems of thickness and performance requirements of resin insulating sheets are solved, and the insulation, plating adhesion and moisture absorption and heat resistance are improved, supporting the high density and thinness of printed circuit boards and semiconductor component substrates.

CN116096805BActive Publication Date: 2026-11-17MITSUBISHI GAS CHEM CO INC +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202180056838.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-13
Filing Date
2021-08-07
Publication Date
2026-11-17
Estimated Expiration
2041-08-07

AI Technical Summary

Technical Problem

In the existing technology, the thickness of resin insulating sheets is required to be at least 12μm, making it difficult to achieve further thinning while simultaneously meeting the requirements for insulation, coating adhesion, and moisture absorption and heat resistance.

Method used

By forming a first resin layer on the surface of the copper foil, adjusting its composition and the surface roughness of the copper foil, specifically including the use of polyphenylene ether compounds, polyimide resins and maleimide compounds, and controlling the thickness and composition of the first resin layer and the second resin layer, the insulation, plating adhesion and moisture absorption and heat resistance of the copper foil are ensured.

Benefits of technology

It achieves excellent performance in insulation, plating adhesion and moisture absorption and heat resistance, supporting the demand for high density and thinness of printed circuit boards and semiconductor component substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116096805B_ABST
    Figure CN116096805B_ABST
Patent Text Reader

Abstract

This invention provides a resin-coated copper foil with excellent insulation, plating adhesion, and moisture absorption and heat resistance, as well as a laminate using the same. The resin-coated copper foil 10 of this invention comprises: a copper foil 11, a first resin layer 12 deposited on the copper foil 11, and a second resin layer 13 deposited on the first resin layer 12. The first resin layer 12 contains: a polyphenylene ether compound (A), a polyimide resin (B), and a maleimide compound (C). The ten-point average roughness Rz of the surface of the copper foil 11 is 0.3 μm or more and 10 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a resin-coated copper foil and a laminate using the same. More specifically, this invention relates to a resin-coated copper foil useful for use as a substrate for printed circuit boards or semiconductor components, and a laminate using the same. [Background Technology]

[0002] In recent years, printed circuit boards (PCBs) or substrates for semiconductor components, widely used in electronic and communication equipment, personal computers, etc., have been continuously developing towards higher density, higher integration, and thinner designs. Consequently, the manufacturing methods for PCBs or substrates for semiconductor components widely employ additive layering, which involves alternately stacking conductor layers and insulating layers (interlayer insulating layers) to form circuits; the formation of circuit patterns mostly uses semi-additive methods capable of forming fine patterns.

[0003] For insulating layers used in printed circuit boards, one known type is an insulating layer formed by multilayering resin composition layers (see, for example, Patent Document 1). Patent Document 1 relates to a resin insulating sheet in which the etching amount of each layer is controlled to improve the performance of the multilayered insulating layer.

[0004] [Previous Technical Documents]

[0005] [Patent Literature]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 2017-50561 [Summary of the Invention]

[0007] [The technical problem that the invention aims to solve]

[0008] However, the resin insulating sheet described in Patent Document 1 requires the total thickness of all layers to be at least 12 μm. Therefore, there is a continuous pursuit to develop technologies that can be further thinned (e.g., less than 10 μm) and can meet requirements for insulation, coating adhesion, and moisture absorption and heat resistance.

[0009] The present invention is based on such a problem and aims to provide a resin-coated copper foil with excellent insulation, plating adhesion and moisture absorption and heat resistance, as well as a laminate using the same.

[0010] [Technical means]

[0011] The inventors have discovered that by adjusting the composition of the first resin layer and the surface roughness of the copper foil, which has a copper foil and a resin-attached layer of a first resin layer deposited on the surface of the copper foil, the above-mentioned problems can be solved, thereby completing the present invention.

[0012] That is, the present invention is as follows.

[0013] [1] A copper foil with a resin layer, comprising a copper foil and a first resin layer deposited on the surface of the copper foil; characterized in that

[0014] The aforementioned first resin layer contains: polyphenylene ether compound (A), polyimide resin (B), and maleimide compound (C);

[0015] The average roughness Rz of the aforementioned copper foil surface at ten points is between 0.3 μm and 10 μm.

[0016] [2] The copper foil with a resin layer as described in [1], wherein the first resin layer is provided with a second resin layer containing a thermosetting resin.

[0017] [3] The copper foil with a resin layer as described in [1], wherein the proportion of polyphenylene ether compound (A) in the aforementioned first resin layer is more than 3 parts by mass and less than 20 parts by mass relative to 100 parts by mass of resin solids.

[0018] [4] The copper foil with a resin layer as described in [1], wherein the first resin layer does not contain inorganic filler or contains inorganic filler with a content of less than 35% by volume.

[0019] [5] The copper foil with resin layer as described in [4], wherein the aforementioned inorganic filler contains at least one selected from magnesium hydroxide, magnesium oxide, silicon dioxide, molybdenum compound, aluminum oxide, aluminum nitride, glass, talc, titanium compound, and zirconium oxide.

[0020] [6] The copper foil with a resin layer as described in [1], wherein the thickness of the first resin layer is more than 1.5 μm and less than 5 μm.

[0021] [7] The copper foil with a resin layer as described in [2], wherein the aforementioned second resin layer contains at least one selected from the group consisting of epoxy compounds, cyanate compounds, maleimide compounds, phenolic compounds, polyphenylene ether compounds, benzoxazine compounds, organic-modified silicone compounds, and compounds having polymerizable unsaturated groups.

[0022] [8] The copper foil with a resin layer as described in [2], wherein the aforementioned second resin layer is free of inorganic filler or contains inorganic filler with a content of less than 36% by volume.

[0023] [9] The copper foil with resin layer as described in [8], wherein the aforementioned inorganic filler contains at least one selected from magnesium hydroxide, magnesium oxide, silicon dioxide, molybdenum compound, aluminum oxide, aluminum nitride, glass, talc, titanium compound, and zirconium oxide.

[0024]

[10] The copper foil with a resin layer as described in [2], wherein the thickness of the aforementioned second resin layer is more than 1 μm and less than 15 μm.

[0025]

[11] A laminate, characterized in that it has a conductor layer and an extension layer formed using a copper foil with a resin layer as described in [1].

[0026] [Invention Effects]

[0027] According to the present invention, a copper foil with a resin layer and a laminate using the same are provided, wherein the copper foil with the resin layer is excellent in terms of insulation, plating adhesion and moisture absorption and heat resistance. [Attached Image Description]

[0028] Figure 1 This is a schematic diagram illustrating the structure of the copper foil with a resin layer according to an embodiment of the present invention.

[0029] Figure 2 This is a schematic diagram illustrating an example of a stacked body according to an embodiment of the present invention.

[0030] Figure 3 This is a schematic diagram illustrating an example of a multilayer coreless substrate according to an embodiment of the present invention.

Detailed Implementation Methods

[0031] The following describes in detail the embodiments used to implement the present invention (hereinafter referred to as "this embodiment"), but the present invention is not limited thereto, and various modifications can be made without departing from the spirit of the present invention. In this specification, the layers of the laminated system are bonded to each other, but the layers can also be peeled off as needed.

[0032] In this embodiment, unless otherwise specified, "resin solids" refers to the components in the first resin layer 12 or the second resin layer 13 other than solvents and inorganic fillers; "100 parts by mass of resin solids" means that the total amount of the components in the first resin layer 12 or the second resin layer 13 other than solvents and inorganic fillers is 100 parts by mass.

[0033] [Copper foil with resin layer]

[0034] Figure 1 This diagram illustrates the structure of a resin-coated copper foil 10 according to an embodiment of the present invention. The resin-coated copper foil 10 includes a copper foil 11 and a first resin layer 12 deposited on the surface of the copper foil 11. Ideally, a second resin layer 13 is provided on the first resin layer 12.

[0035] The copper foil 10 with the resin layer is useful, for example, as a material for forming an insulating layer on a circuit pattern (conductor layer), and can be used, for example, as a material for forming an insulating layer on a printed circuit board or a substrate for mounting semiconductor components in the manufacture of electronic devices, communication devices, and personal computers. For example, in the case of manufacturing a printed circuit board, the copper foil 10 with the resin layer is placed on a substrate on which a circuit pattern is formed, with the second resin layer 13 in contact with the conductor layer. Then, it is heated and pressed (pressed) to harden the first resin layer 12 and the second resin layer 13, thereby forming an insulating layer on the conductor layer.

[0036] The first resin layer 12 is a layer that maintains the insulation between the conductor layer and the copper foil 11, and also maintains the distance between the copper foil 11 and the conductor layer after pressing during the formation of the laminate. The second resin layer 13 is a layer containing a resin that is fluid during pressing, and is a layer in which the conductor layer with circuit patterns and other uneven parts are embedded. Since the second resin layer 13 functions as an embedded layer, it is ideal that at least one of its constituent components and physical properties is different from that of the first resin layer 12. Although there is no particular limitation, examples of different first resin layers 12 and second resin layers 13 include: the first resin layer 12 using polyimide resin, and the second resin layer 13 using epoxy compound, etc., where the composition is different due to different types of resins; the physical properties are different due to the mixing ratio of the components contained in each layer, or the curing state (for example, by changing the coating conditions of each layer, the first resin layer 12 is fully cured, and the second resin layer 13 is in a semi-cured state); and such composite cases, etc.

[0037] [Copper foil]

[0038] The copper foil 11 can be any type of copper foil, as long as it is used for a typical printed circuit board, such as electrolytic copper foil, rolled copper foil, and copper alloy film. Common surface treatments such as matte finishing, corona treatment, nickel treatment, and cobalt treatment can also be applied to the copper foil 11. Commercially available products can be used for the copper foil 11 in this embodiment, such as: JX Metals Co., Ltd.'s "GHY5" (trade name, 12μm thick copper foil) and "JXUT-I" (trade name, 1.5μm thick copper foil); Mitsui Metals & Mining Co., Ltd.'s "MT-FL" (trade name, 3μm thick copper foil), "3EC-VLP" (trade name, 12μm thick copper foil), "3EC-III" (trade name, 12μm thick copper foil), and "3EC-M2S-VLP" (trade name, 12μm thick copper foil); and Furukawa Electric Industries Co., Ltd.'s copper foil "GTS-MP" (trade name, 12μm thick copper foil).

[0039] The ten-point average roughness Rz of the surface of the copper foil 11, that is, the ten-point average roughness Rz of the surface of the copper foil 11 on the side where the first resin layer 12 is formed, is ideally between 0.3 μm and 10 μm. This is because setting it to 0.3 μm or more improves plating adhesion. Furthermore, if it is greater than 10 μm, the thickness of the first resin layer 12 must be increased to ensure insulation. A further ideal range for the ten-point average roughness Rz of the surface of the copper foil 11 is, for example, between 0.6 μm and 2.5 μm. Ideally, the ten-point average roughness Rz of the surface of the copper foil 11 is less than the thickness of the first resin layer 12. This is to improve insulation. The ten-point average roughness Rz of the surface of the copper foil 11 can be measured using a commercially available shape measuring microscope (laser microscope, such as the "VK-X1000" (trade name) manufactured by Keynes Corporation).

[0040] While there is no particular limitation on the thickness of the copper foil 11, considering the surface roughening treatment, it is ideal to be in the range of 1μm to 18μm to obtain a suitable thin printed circuit board and semiconductor component mounting substrate, and even more ideally in the range of 2μm to 15μm.

[0041] [First resin layer]

[0042] The first resin layer 12 contains: a polyphenylene ether compound (A), a polyimide resin (B), and a maleimide compound (C). Furthermore, the first resin layer 12 may, as needed, contain at least one of other resin components, inorganic fillers, and other components. While the thickness of the first resin layer 12 is not particularly limited, from a thin-film perspective, it is ideally 5 μm or less; if insulation is also considered, it is ideally 1.5 μm or more. The thickness of the first resin layer 12 can be determined, for example, by hardening a copper foil 10 with the resin layer to prepare a test sample, cutting it to expose a vertical cross-section, grinding it, and then observing the vertical cross-section under a microscope. For example, a length measurement method is to take the distance from the surface opposite to the copper foil 11 of the first resin layer 12 to the interface with the copper foil 11 in the vertical direction, and the distance from the average position of the uneven interface between the first resin layer 12 and the copper foil 11 to the surface opposite to the copper foil 11 of the first resin layer 12 as the thickness of the first resin layer 12. The first resin layer 12 can be in a semi-cured state (B-Stage) or a fully cured state (C-Stage). The first resin layer 12 can be formed, for example, by conventional means such as coating.

[0043] <Polyphenylene ether compound (A)>

[0044] The polyphenylene ether compound (A) in this embodiment is a compound represented by the general formula (1). By containing the polyphenylene ether compound (A), insulation, coating adhesion, and moisture absorption and heat resistance can be improved. The polyphenylene ether compound (A) represented by the general formula (1) used in this embodiment ideally has a number-average molecular weight of 1,000 to 7,000. By setting the number-average molecular weight to 7,000 or less, the compatibility of the resins can be controlled. Furthermore, by setting the number-average molecular weight to 1,000 or more, the excellent insulation and moisture absorption and heat resistance inherent in polyphenylene ether resins can be obtained. In order to obtain even better compatibility, insulation, and moisture absorption and heat resistance, the number-average molecular weight of the polyphenylene ether compound (A) can be 1,100 to 5,000. The number-average molecular weight of the polyphenylene ether compound (A) is further ideally 4,500 or less, and the number-average molecular weight of the polyphenylene ether compound (A) is even more ideally 3,000 or less. The number-average molecular weight was determined using a gel permeation chromatography instrument according to conventional methods.

[0045] [Chemistry 1]

[0046]

[0047] (In general formula (1), X represents aryl (aromatic group), -(YO)n2- represents polyphenylene ether moiety, R1, R2, and R3 each independently represent hydrogen atom, alkyl, alkenyl, or alkynyl, n2 represents integers from 1 to 100, n1 represents integers from 1 to 6, and n3 represents integers from 1 to 4. Ideally, n1 can be an integer greater than or equal to 1 and less than or equal to 4, and even more ideally, n1 can be 1 or 2. In the ideal case, n1 can be 1. In addition, ideally, n3 can be an integer greater than or equal to 1 and less than or equal to 3, and even more ideally, n3 can be 1 or 2. In the ideal case, n3 can be 2.)

[0048] The polyphenylene ether compound (A) represented by general formula (1) is ideally a polymer containing constituent units represented by the following general formula (2).

[0049] [Chemistry 2]

[0050]

[0051] (In general formula (2), R) 901 R 902 R 903 R 904 Each of these groups independently represents an alkyl, aryl, halogen atom, or hydrogen atom having 6 or fewer carbon atoms.

[0052] The aforementioned aggregate may further contain at least one structural unit selected from the group of structural units represented by general formula (3) and general formula (4).

[0053] [Chemistry 3]

[0054]

[0055] (In general formula (3), R) 905 R 906 R 907 R 911 R 912 Each of these groups independently represents an alkyl or phenyl group having 6 or fewer carbon atoms. R 908 R 909 R 910 Each of these can be used independently to represent a hydrogen atom or an alkyl or phenyl group having 6 or fewer carbon atoms.

[0056] [Chemistry 4]

[0057]

[0058] (In general formula (4), R) 913 R 914 R 915 R 916 R 917 R 918 R 919 R 920 Each group independently represents a hydrogen atom and an alkyl or phenyl group with 6 or fewer carbon atoms. The -A- group consists of straight-chain, branched, or cyclic divalent hydrocarbon groups with 20 or fewer carbon atoms.

[0059] In relation to general formula (1), the above general formulas (2), (3), and (4) are ideally -(YO)- of general formula (1). -(YO)- is a repeating unit with a number of (1 to 100) of n2.

[0060] In general formula (1), the aryl group in X can be an aromatic hydrocarbon group. Specifically, it can be a group formed by removing n3 hydrogen atoms from a ring structure selected from benzene ring structure, biphenyl ring structure, indene ring structure, and naphthyl ring structure (e.g., phenyl, biphenyl, indene, and naphthyl), ideally biphenyl. Here, the aryl group may also contain: diphenyl ether group, etc., which are bonded by oxygen atoms, or diphenyl ketone group, etc., which are bonded by carbonyl groups, or 2,2-diphenylpropane group, etc., which are bonded by alkylene groups. In addition, the aryl group can also be substituted by general substituents such as alkyl (ideally alkyl with 1 to 6 carbon atoms, especially methyl), alkenyl, ynyl or halogen atoms. However, since the aforementioned "aryl" is partially substituted by polyphenylene ether via oxygen atoms, the number of general substituents is limited by the number of polyphenylene ether moieties.

[0061] The polyphenylene ether compound (A) is particularly ideal to contain polyphenylene ether represented by the structure of the following general formula (5).

[0062] [Chemistry 5]

[0063]

[0064] (In general formula (5), X is aryl (aromatic group), -(YO)n2- series respectively represent polyphenylene ether moiety, and n2 series respectively represent integers from 1 to 100.)

[0065] -(YO)n2- and n2 are synonyms with those in general formula (1). Compounds may also contain various different n2.

[0066] X in general formula (1) and general formula (5) is ideally general formula (6), general formula (7), or general formula (8); -(YO)n2- in general formula (1) and general formula (5) is further ideally a structure arranged in general formula (9) or general formula (10), or a structure randomly arranged in general formula (9) and general formula (10).

[0067] [Chemistry 6]

[0068]

[0069] [Chemistry 7]

[0070]

[0071] (In general formula (7), R) 921 R 922 R 923 R 924 Each group independently represents a hydrogen atom or a methyl group. The -B- group consists of straight-chain, branched, or cyclic divalent hydrocarbon groups with 20 or fewer carbon atoms.

[0072] [Chemistry 8]

[0073]

[0074] (In general formula (8), -B- is a straight-chain, branched, or cyclic divalent hydrocarbon group with 20 or fewer carbon atoms.)

[0075] [Chemistry 9]

[0076]

[0077] [Chemistry 10]

[0078]

[0079] There are no particular limitations on the method of manufacturing modified polyphenylene ether having a structure represented by general formula (5). For example, it can be manufactured by vinyl benzyl etherification of the terminal phenolic hydroxyl groups of a difunctional phenylene ether oligomer obtained by oxidative coupling of a difunctional phenol compound and a monofunctional phenol compound.

[0080] In addition, commercially available products can be used for such modified polyphenylene ether systems, such as OPE-2St1200 and OPE-2St2200 manufactured by Mitsubishi Gas Chemical Co., Ltd.

[0081] In this embodiment, the proportion of polyphenylene ether compound (A) relative to 100 parts by weight of resin solids in the first resin layer 12 is ideally 1 part by weight or more, and more ideally 3 parts by weight or more. Furthermore, the upper limit of the aforementioned content is ideally less than 20 parts by weight. By setting it within such a range, interlayer adhesion, plating adhesion, and moisture absorption and heat resistance can be effectively improved. The first resin layer 12 may contain only one type of polyphenylene ether compound (A), or it may contain two or more types of polyphenylene ether compounds (A). In the case of containing two or more types, the total amount is ideally within the above-mentioned range.

[0082] <Polyimide Resin (B)>

[0083] The polyimide resin (B) can be used with commercially available products, such as solvent-soluble polyimide resins synthesized by the manufacturing method described in Japanese Patent Application Publication No. 2005-15629. Specifically, the solvent-soluble polyimide resin can be obtained by polycondensation in the presence of a tertiary amine compound with one or more of an aliphatic tetracarboxylic dianhydride represented by formula (11), an aliphatic tetracarboxylic acid represented by formula (12), and a derivative of the aliphatic tetracarboxylic acid with one or more diamine compounds.

[0084] [Chemistry 11]

[0085]

[0086] (In the formula, R refers to a tetravalent aliphatic hydrocarbon group with 4 to 16 carbon atoms.)

[0087] [Chemistry 12]

[0088]

[0089] (In the formula, R is a tetravalent aliphatic hydrocarbon group with 4 to 16 carbon atoms, and Y1 to Y4 are independently hydrogen or hydrocarbon groups with 1 to 8 carbon atoms.)

[0090] In the aforementioned manufacturing method, nearly equimolar amounts of an aliphatic tetracarboxylic acid and a diamine compound are heated in a solvent in the presence of a tertiary amine compound to carry out polycondensation. Furthermore, the molar ratio of the aliphatic tetracarboxylic acid to the diamine compound is ideally in the range of 95–105 mol%, relative to one of them.

[0091] In the manufacture of general polyimide resins, tetracarboxylic acid dianhydrides are commonly used as the tetracarboxylic acid. However, in the aforementioned manufacturing method, in addition to aliphatic tetracarboxylic acid dianhydrides, aliphatic tetracarboxylic acids or esters of aliphatic tetracarboxylic acids and alcohols can also be used to manufacture practical polyimide resins. Using aliphatic tetracarboxylic acids directly is advantageous in terms of production equipment and cost.

[0092] In addition, aliphatic tetracarboxylic dianhydrides represented by formula (11) can be exemplified by, for example, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,4,5-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, etc.

[0093] Furthermore, aliphatic tetracarboxylic acids and their derivatives represented by formula (12) can be exemplified by, for example, 1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,4,5-cyclopentanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic acid, and their alcohol esters. These can be used alone or in combination of two or more types. Among these, ideally, 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride and 1,2,4,5-cyclohexanetetracarboxylic acid can be cited.

[0094] In the aforementioned manufacturing method, other tetracarboxylic acids and their derivatives may be mixed in without affecting the solvent solubility. Examples include: pyrocalcite, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(2,3-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane, bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)sulfone, etc. Bis(2,3-dicarboxyphenyl) ether, 3,3',4,4'-diphenylone tetracarboxylic acid, 2,2',3,3'-diphenylone tetracarboxylic acid, 4,4-(p-phenylenedioxy)phthalic acid, 4,4-(m-phenylenedioxy)phthalic acid, ethylene tetracarboxylic acid, 3-carboxymethyl-1,2,4-cyclopentane tricarboxylic acid, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)methane, and their derivatives. Ideally, the proportion of other tetracarboxylic acid components in these tetracarboxylic acid components should be less than 50 mol% of the total tetracarboxylic acid components.

[0095] The aforementioned diamine compounds are ideally aromatic diamine compounds containing 6 to 28 carbon atoms, or aliphatic diamine compounds containing 2 to 28 carbon atoms. Diamine compounds, for example, include: p-phenylenediamine, m-phenylenediamine, 4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-dimethylbiphenyl, 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diamino-2,2'-ditrifluoromethylbiphenyl, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ketone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]sulfone, etc. Aromatic diamine compounds such as [4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, bis[4-(3-aminophenoxy)phenyl]sulfone, and 9,9-bis(4-aminophenyl)pyroxene; and aliphatic diamine compounds such as ethylenediamine, hexamethylenediamine, polyethylene glycol bis(3-aminopropyl) ether, polypropylene glycol bis(3-aminopropyl) ether, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 4,4'-diaminodicyclohexylmethane, 3(4),8(9)-bis(aminomethyl)-tricyclo[5.2.1.02,6]decane, m-phenylenediamine, p-phenylenediamine, isophorone diamine, norbornene diamine, and siloxane diamines. These can be used alone or in combination with two or more classes. Among these diamine compounds, the ideal aromatic diamine compounds are 4,4'-diamine-3,3'-dimethylbiphenyl, 4,4'-diamine-2,2'-ditrifluoromethylbiphenyl, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane; the ideal aliphatic diamine compounds are 4,4'-diaminodicyclohexylmethane and 3(4),8(9)-bis(aminomethyl)-tricyclo[5.2.1.02,6]decane.

[0096] In the aforementioned manufacturing method, it is ideal to use 0.001 to 1.0 moles of a tertiary amine compound relative to 1 mole of the aliphatic tetracarboxylic acid component used, and more ideally, 0.01 to 0.2 moles of a tertiary amine compound.

[0097] Examples of the aforementioned tertiary amine compounds include: trimethylamine, triethylamine, tripropylamine, tributylamine, triethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, triethylenediamine, N-methylpyrrolidine, N-ethylpyrrolidine, N-methylpiperidine, N-ethylpiperidine, imidazole, pyridine, quinoline, isoquinoline, etc. Among these tertiary amine compounds, triethylamine is particularly desirable.

[0098] Solvents used in the aforementioned manufacturing method may include, for example, γ-butyrolactone, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, hexamethylphosphoramide, sulfolane, p-chlorophenol, m-cresol, 2-chloro-4-hydroxytoluene, etc. These may be used alone or in combination of two or more types. Among these, γ-butyrolactone, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone are ideal, and γ-butyrolactone and N,N-dimethylacetamide are even more ideal. Furthermore, unsuitable solvents for polyimide resins may also be used, to the extent that the polymer will not precipitate. Examples of unsuitable solvents include, for example, hexane, heptane, benzene, toluene, xylene, chlorobenzene, o-dichlorobenzene, etc.

[0099] In the aforementioned manufacturing method, the amount of solvent used, relative to the total mass of the reaction solution, is ideally 1 to 50% by mass of the aliphatic tetracarboxylic acid component and the diamine component, and more ideally 20 to 45% by mass.

[0100] There are no particular limitations on the method of adding aliphatic tetracarboxylic acid components and diamine compounds. It can be done by adding both components at once, or by gradually adding the other component in a solid or solution state to a solution containing one component (not necessarily completely dissolved). In particular, adding both components at once shortens the addition time, which is advantageous in terms of productivity.

[0101] For tertiary amine compounds to fully exert their catalytic effect, it is ideal to add them after heating but before reaching the target temperature. In particular, it is ideal to add them simultaneously with the solvent, the aliphatic tetracarboxylic acid component, and the diamine compound.

[0102] The aforementioned method of adding solvent is not particularly limited and can be carried out individually or in combination with the following methods: adding it to the reaction tank beforehand; adding it to a reaction tank containing either an aliphatic tetracarboxylic acid component or a diamine compound, or a reaction tank containing both; dissolving either the aliphatic tetracarboxylic acid component or the diamine component beforehand and then adding it to the reaction tank, etc. Furthermore, depending on the purpose, the solvent described above can be added to a solvent-soluble polyimide resin solution in the state during the reaction process, or to a solvent-soluble polyimide resin solution remaining in the reaction tank after the reaction, or to a solvent-soluble polyimide resin solution removed from the reaction tank after the reaction.

[0103] Furthermore, the polyimide resin (B) used in this embodiment may, for example, be a block copolymer polyimide resin. Examples of block copolymer polyimide resins include, for instance, the block copolymer polyimide resin described in International Publication No. WO2010-073952. Specifically, the block copolymer polyimide resin is not particularly limited as long as it is a copolymer polyimide resin having alternating structures B1 and B2, wherein structure B1 has an imide oligomer composed of a second structural unit bonded to the end of an imide oligomer composed of a first structural unit, and structure B2 has an imide oligomer composed of a first structural unit bonded to the end of an imide oligomer composed of a second structural unit. Also, the second structural unit is different from the first structural unit. These block copolymer polyimide resins can be synthesized by reacting tetracarboxylic dianhydride with diamine in a polar solvent to form an imide oligomer, followed by the addition of tetracarboxylic dianhydride and other diamines, or the addition of other tetracarboxylic dianhydrides and diamines, to carry out a successive polymerization reaction of imidization.

[0104] Although there is no particular limitation on the proportion of polyimide resin (B) in the first resin layer 12, from the viewpoint of heat resistance and curing properties, it is ideally in the range of 10 to 80 parts by mass relative to 100 parts by mass of resin solids in the first resin layer 12, and particularly ideally in the range of 30 to 70 parts by mass.

[0105] The first resin layer 12 may contain only one type of polyimide resin (B), or it may contain two or more types of polyimide resin (B). In the case of containing two or more types, the total amount is ideally within the range described above.

[0106] <Maleimide compound (C)>

[0107] By incorporating a maleimide compound (C), interlayer adhesion, insulation, coating adhesion, and moisture absorption and heat resistance can be improved. The maleimide compound (C) is not particularly limited as long as it is a compound having one or more maleimide groups per molecule (ideally 2 to 12, further ideally 2 to 6, even further ideally 2 to 4, even further ideally 2 or 3, and even further ideally 2). Any conventionally known maleimide compound can be used.

[0108] Specific examples of maleimide compounds (C) include, for example, bis(4-maleimidephenyl)methane, 2,2-bis{4-(4-maleimidephenoxy)-phenyl}propane, bis(3,5-dimethyl-4-maleimidephenyl)methane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, bis(3,5-diethyl-4-maleimidephenyl)methane, and other bismaleimide compounds; polyphenylmethane maleimide. Furthermore, maleimide compounds (C) can also be blended in the form of prepolymers of these compounds, or prepolymers of these compounds with amine compounds. These maleimide compounds (C) can be used individually or in a suitable mixture of two or more.

[0109] Of these, from the viewpoint of heat resistance, bismaleimide compounds are ideal, with 2,2-bis[4-(4-maleimidephenoxy)-phenyl]propane and bis(3-ethyl-5-methyl-4-maleimidephenyl)methane being even more ideal.

[0110] Although there is no particular limitation on the proportion of maleimide compound (C) in the first resin layer 12, from the viewpoint of heat resistance and coating adhesion, it is ideally in the range of 5 to 75 parts by mass relative to 100 parts by mass of resin solids in the first resin layer 12, and more ideally in the range of 5 to 45 parts by mass.

[0111] The first resin layer 12 may contain only one maleimide compound (C), or it may contain two or more maleimide compounds (C). In the case of containing two or more, the total amount is ideally within the range described above.

[0112] <Other Resin Components>

[0113] Other resin components may include, for example, liquid crystal polyesters, epoxy compounds, cyanate compounds, phenolic compounds, benzoxazine compounds, organo-modified silicone compounds, and compounds having polymerizable unsaturated groups. The first resin layer 12 may also contain one or more of these components.

[0114] -Liquid Crystal Polyester-

[0115] Liquid crystal polyesters are aromatic polyesters that exhibit liquid crystal properties when melted. Conventional liquid crystal polyesters can be selected for use. Conventional liquid crystal polyesters may include, for example, aromatic polyesters described in Japanese Patent Application Publication No. 2001-11296. Specifically, aromatic polyesters containing 90 mol% or more of the structural units represented by the following formula (13) can be cited as examples.

[0116] [Chemistry 13]

[0117]

[0118] The aromatic polyesters containing the structural units represented by formula (13) described above, for example from the point of availability, can be polyoxybenzoic acid esters that are essentially homopolymers of the structural units represented by formula (13). The manufacturing method of this aromatic polyester can be a conventional method. Furthermore, the aromatic polyesters containing the structural units represented by formula (13) described above are mostly poorly soluble or insoluble in common solvents, and because they are difficult to melt or infusible, they do not exhibit liquid crystal properties. Therefore, the aromatic polyesters containing the structural units represented by formula (13) described above are ideally used as powders. These powders are obtained by pulverizing the resin or fibers of the aromatic polyester.

[0119] Although there are no specific limitations, the molecular weight of liquid crystal polyester is usually 1,000 to 100,000, and ideally 10,000 to 50,000.

[0120] Liquid crystal polyester can be selected from commercially available products, such as "Ekonol E101-F" manufactured by Sumitomo Chemical Industries, Ltd. In this embodiment, when liquid crystal polyester is used for the first resin layer 12, its content is not particularly limited. From the viewpoint of heat resistance and curability, it is ideally in the range of 10 to 90 parts by weight of resin solids per 100 parts by weight of the first resin layer 12, and particularly ideally in the range of 30 to 80 parts by weight.

[0121] - Epoxy compounds -

[0122] Epoxy compounds are not particularly limited as long as they have one or more epoxy groups per molecule (ideally 2 to 12, further ideally 2 to 6, even further ideally 2 to 4, even further ideally 2 or 3, and even further ideally 2). Any conventionally known epoxy compound can be used. From the viewpoint of further improving adhesion and flexibility, the epoxy equivalent of an epoxy compound is ideally 250 g / eq to 850 g / eq, and even more ideally 250 g / eq to 450 g / eq. The epoxy equivalent can be determined by conventional methods.

[0123] Specific examples of epoxy compounds include: compounds formed by epoxidation of the double bonds of polyoxynaphthyl-type epoxy resins, biphenyl aralkyl-type epoxy resins, naphthalene tetrafunctional epoxy resins, xylene-type epoxy resins, naphthol aralkyl-type epoxy resins, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol A phenolic epoxy resins, trifunctional phenol-type epoxy resins, tetrafunctional phenol-type epoxy resins, naphthalene-type epoxy resins, biphenyl-type epoxy resins, aralkylphenolic epoxy resins, alicyclic epoxy resins, polyol-type epoxy resins, epioxypropylamine-type epoxy resins, epioxypropyl ester-type epoxy resins, butadiene, etc.; and compounds obtained by reacting hydroxyl-containing silicone resins with epichlorohydrin. Among these, especially from the viewpoint of copper plating adhesion and flame retardancy, ideally are polyoxynaphthylene epoxy resins, biphenyl aralkyl epoxy resins, naphthalene tetrafunctional epoxy resins, xylene epoxy resins, and naphthol aralkyl epoxy resins. One of these epoxy compounds may be used, or a suitable mixture of two or more may be used.

[0124] In this embodiment, when the first resin layer 12 uses an epoxy compound, although its content is not particularly limited, from the viewpoint of heat resistance and curing properties, it is ideally in the range of 1 to 60 parts by mass relative to 100 parts by mass of resin solids in the first resin layer 12, and particularly ideally in the range of 1 to 30 parts by mass.

[0125] - Cyanate compounds -

[0126] Cyanate ester compounds have excellent chemical resistance and adhesion properties. Due to their excellent chemical resistance, they can form a uniform roughened surface, and therefore can be appropriately used as a component of the resin layer in this embodiment.

[0127] Cyanate ester compounds are not particularly limited as long as they contain one or more cyanate groups (ideally 2 to 12, more ideally 2 to 6, even more ideally 2 to 4, even more ideally 2 or 3, and even more ideally 2) within their molecules, and can be widely used in compounds commonly used in the field of printed circuit boards. Specific examples of cyanate ester compounds include, for example, at least one of the following groups: α-naphthol aralkyl cyanate esters represented by formula (14), phenolic phenolic cyanate esters represented by formula (15), biphenyl aralkyl cyanate esters represented by formula (16), naphthyl ether cyanate esters, xylene resin cyanate esters, triphenol methane cyanate esters, adamantane skeleton cyanate esters, bisphenol M cyanate esters, bisphenol A cyanate esters, and diallyl bisphenol A cyanate esters. From the viewpoint of further improving low water absorption, it is ideal to select at least one of the following groups: α-naphthol aralkyl cyanate compound represented by formula (14), phenolic phenolic cyanate compound represented by formula (15), biphenyl aralkyl cyanate compound represented by formula (16), naphthyl ether cyanate compound, xylene resin cyanate compound, bisphenol M cyanate compound, bisphenol A cyanate compound, and diallyl bisphenol A cyanate compound. These cyanate compounds can be prepared by conventional methods or commercially available products can be used.

[0128] Among these, the α-naphthol aralkyl cyanate compound represented by formula (14), the phenol phenolic cyanate compound represented by formula (15), and the biphenyl aralkyl cyanate compound represented by formula (16) are ideal because of their excellent flame retardancy, high hardening properties, and low coefficient of thermal expansion of the hardened product.

[0129] [Chemistry 14]

[0130]

[0131] In equation (14), R 1 The series represents a hydrogen atom or a methyl group, n 1 The series represents integers greater than or equal to 1. 1 Ideally, it should be an integer between 1 and 50.

[0132] [Chemistry 15]

[0133]

[0134] In equation (15), R 2 The series represents a hydrogen atom or a methyl group, n 2 The series represents integers greater than or equal to 1. 2 Ideally, it should be an integer between 1 and 50.

[0135] [Chemistry 16]

[0136]

[0137] In equation (16), R 3 The series represents a hydrogen atom or a methyl group, n 3 The series represents integers greater than or equal to 1. 3 Ideally, it should be an integer between 1 and 50.

[0138] In this embodiment, when the first resin layer 12 uses a cyanate ester compound, although its content is not particularly limited, from the viewpoint of heat resistance and adhesion to the copper foil, it is ideally in the range of 1 to 60 parts by mass relative to 100 parts by mass of resin solids in the first resin layer 12, and more ideally in the range of 1 to 30 parts by mass.

[0139] -Phenolic compounds-

[0140] Phenolic compounds are not particularly limited as long as they are phenolic compounds having one or more (ideally 2 to 12, further ideally 2 to 6, even further ideally 2 to 4, even further ideally 2 or 3, even further ideally 2) phenolic hydroxyl groups in one molecule, and any phenolic compound known in the past may be used. Specific examples of phenolic compounds include: bisphenol A type phenolic resins, bisphenol E type phenolic resins, bisphenol F type phenolic resins, bisphenol S type phenolic resins, phenol-formaldehyde resins, bisphenol A phenol-formaldehyde resins, glycidyl ester type phenolic resins, aralkyl phenol-formaldehyde resins, biphenyl aralkyl phenolic resins, cresol phenol-formaldehyde resins, polyfunctional phenolic resins, naphthol resins, naphthol phenol-formaldehyde resins, polyfunctional naphthol resins, anthracene type phenolic resins, naphthalene skeleton modified phenol-formaldehyde resins, phenol-aralkyl type phenolic resins, naphthol-aralkyl type phenolic resins, dicyclopentadiene type phenolic resins, biphenyl type phenolic resins, alicyclic phenolic resins, polyol type phenolic resins, phosphorus-containing phenolic resins, and hydroxyl-containing silicone resins, etc. These phenolic compounds can be used individually or in combination of two or more.

[0141] -Benzoxazine compounds-

[0142] Benzooxazine compounds are not particularly limited as long as they are compounds having two or more dihydrobenzooxazine rings in one molecule; generally, known compounds can be used. Specific examples of benzooxazine compounds include: bisphenol A type benzooxazine BA-BXZ (manufactured by Konishi Chemical, trade name), bisphenol F type benzooxazine BF-BXZ (manufactured by Konishi Chemical, trade name), bisphenol S type benzooxazine BS-BXZ (manufactured by Konishi Chemical, trade name), etc. These benzooxazine compounds can be used alone or in mixtures of two or more.

[0143] -Organic-based modified silicone compounds-

[0144] There are no particular limitations on the organo-modified silicone compounds, but specific examples include: di(methylamine)polydimethylsiloxane, di(ethylamine)polydimethylsiloxane, di(propylamine)polydimethylsiloxane, di(epoxypropyl)polydimethylsiloxane, and di(epoxybutyl)polydimethylsiloxane. One or more of these organo-modified silicone compounds may be used.

[0145] - Compounds with polymerizable unsaturated groups -

[0146] There are no particular limitations on the compounds having polymerizable unsaturated groups; generally, known compounds can be used. Specific examples of compounds having polymerizable unsaturated groups include: ethylene compounds such as ethylene, propylene, styrene, divinylbenzene, and divinylbiphenyl; monohydric or polyhydric alcohols such as methyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, neopentyl terephthalate tetra(meth)acrylate, and dinepentyl terephthalate hexa(meth)acrylate; epoxy (meth)acrylates such as bisphenol A type epoxy (meth)acrylate and bisphenol F type epoxy (meth)acrylate; and phenylcyclobutene resins, etc. These compounds having polymerizable unsaturated groups can be used individually or in combination of two or more.

[0147] <Inorganic filler>

[0148] The first resin layer 12 may or may not contain inorganic fillers. When it does contain inorganic fillers, the content is ideally 35% by volume or less, and more ideally 31% by volume or less. While adding inorganic fillers improves processability, excessive content can reduce flexibility and cause cracking, or reduce insulation. Furthermore, the content of inorganic fillers refers to the content of inorganic fillers relative to the first resin layer 12 (inorganic filler / first resin layer × 100).

[0149] From the viewpoints of low thermal expansion coefficient, formability, filling properties, and rigidity, spherical fillers can be used for inorganic fillers, and there are no particular limitations as long as they are spherical fillers used in the insulating layer of printed circuit boards. Examples of inorganic fillers include: magnesium hydroxide; magnesium oxide; natural silica, fused silica, amorphous silica, hollow silica, and other silica compounds; molybdenum compounds such as molybdenum disulfide, molybdenum oxide, and zinc molybdate; alumina; aluminum nitride; glass; talc; titanium compounds such as titanium oxide, barium titanate, and strontium titanate; and zirconium oxide. One or more of these can be used, or a mixture of two or more is suitable.

[0150] From the perspective of low thermal expansion, the ideal inorganic filler is silicon dioxide, specifically spherical fused silicon dioxide. Commercially available spherical fused silicon dioxide includes: SO-C1, SO-E1, YC100C, SC2500-SQ, and K180SQ-C1 manufactured by Admatechs Inc.; M273 manufactured by CIK NanoTek Inc.; and SFP-20M and SFP-130MC manufactured by Denka Co., Ltd., among others.

[0151] While there is no particular limitation on the particle size of inorganic fillers, ideally it is below 5 μm, further ideally below 3 μm, even further ideally below 2 μm, and still ideally below 1.0 μm. The particle size of inorganic fillers can be determined using laser diffraction scattering based on the Mie scattering theory. Ideally, the sample used for measurement should be a sample in which the inorganic filler is dispersed in water by ultrasonic waves. The laser diffraction scattering particle size distribution measuring device can be the "MT3000II" manufactured by MicrotracBEL Co., Ltd., etc.

[0152] In addition, inorganic fillers can also be surface-treated with silane coupling agents, etc. The silane coupling agents described later can be used.

[0153] [Other ingredients]

[0154] Other components, such as those for improving moisture absorption and heat resistance, may also contain silane coupling agents. There are no particular limitations on the type of silane coupling agent, as long as it is a silane coupling agent commonly used for the surface treatment of inorganic materials. Specific examples include: aminosilane-based silane coupling agents (e.g., γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane), epoxysilane-based silane coupling agents (e.g., γ-epoxypropoxypropyltrimethoxysilane), acryloylsilane-based silane coupling agents (e.g., γ-acryloyloxypropyltrimethoxysilane), vinylsilane-based silane coupling agents (e.g., γ-methacryloyloxypropyltrimethoxysilane), cationic silane-based silane coupling agents (e.g., N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride), phenylsilane-based silane coupling agents, etc. These silane coupling agents can be used in one or a suitable mixture of two or more.

[0155] In this embodiment, while the content of the silane coupling agent is not particularly limited, from the viewpoint of improving moisture absorption and heat resistance, it is ideally in the range of 0.05 to 5 parts by mass relative to 100 parts by mass of the inorganic filler, and more ideally in the range of 0.1 to 3 parts by mass. Furthermore, when two or more silane coupling agents are used together, the total amount is ideally within the aforementioned range.

[0156] Other ingredients, such as those for improving manufacturability, may also contain wetting and dispersing agents. There are no particular limitations on wetting and dispersing agents, as long as they are commonly used in coatings, etc. Specific examples include: Disperbyk (registered trademark)-110, Disperbyk-111, Disperbyk-118, Disperbyk-180, Disperbyk-161, BYK (registered trademark)-W996, BYK-W9010, BYK-W903, etc., manufactured by BYK Japan Co., Ltd. These wetting and dispersing agents can be used alone or in combination of two or more.

[0157] In this embodiment, while the content of the wetting and dispersing agent is not particularly limited, from the viewpoint of improving manufacturability, it is ideally in the range of 0.1 to 5 parts by mass relative to 100 parts by mass of the inorganic filler, and more ideally in the range of 0.5 to 3 parts by mass. Furthermore, when two or more wetting and dispersing agents are used together, the total amount should ideally satisfy the aforementioned range.

[0158] Other components, for example, for adjusting the curing speed, may also contain curing accelerators. While not particularly limited, curing accelerators may include: organometallic salts containing metals such as copper, zinc, cobalt, nickel, and manganese (e.g., lead naphthenate, lead stearate, zinc naphthenate, zinc octanoate, tin oleate, dibutyltin malate, manganese naphthenate, cobalt naphthenate, nickel octanoate, manganese octanoate, iron acetylacetone); compounds formed by dissolving these organometallic salts in hydroxyl-containing compounds such as phenols and bisphenols; organotin compounds (e.g., inorganic metal salts such as tin chloride, zinc chloride, and aluminum chloride; dioctyltin oxide, other alkyltin, and alkyltin oxide); imidazoles and their derivatives (e.g., 2-ethyl-4-methylimidazolium, 1-benzyl-2-benzylimidazole, 2,4,5-tribenzylimidazole); tertiary... Amines (e.g., triethylamine, N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, 2-N-ethylanilineethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, tetramethylbutyldiamine, N-methylpiperidine, etc.); organic peroxides (e.g., benzoyl peroxide, lauroyl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, di-tert-butyl-di-perphthalate); azo compounds (e.g., azobisnitrile); phenols (e.g., phenol, xylenol, cresol, resorcinol, catechol). These curing accelerators can be used alone or in combination of two or more.

[0159] In this embodiment, while the content of the curing accelerator is not particularly limited, from the viewpoint of obtaining a high glass transition temperature, it is ideally in the range of 0.001 to 5 parts by mass relative to 100 parts by mass of resin solids in the first resin layer 12, and more ideally in the range of 0.01 to 3 parts by mass. Furthermore, when two or more curing accelerators are used together, the total amount is ideally within the aforementioned range.

[0160] Other components may include various other polymers and / or flame-retardant compounds. There are no particular limitations on the polymers and flame-retardant compounds, as long as they are commonly used compounds.

[0161] Polymer compounds include various thermosetting resins and thermoplastic resins, as well as their oligomers and elastomers. Specifically, examples include: polyamide-imide resins, polystyrene, polyolefins, styrene-butadiene rubber (SBR), isoprene rubber (IR), polybutadiene rubber (BR), acrylonitrile-butadiene rubber (NBR), polyurethanes, polypropylene, (meth)acrylic acid oligomers, (meth)acrylic acid polymers, and silicone resins. From a compatibility perspective, acrylonitrile-butadiene rubber or styrene-butadiene rubber is ideal.

[0162] Specific examples of flame-retardant compounds include: phosphorus-containing compounds (e.g., phosphate esters, melamine phosphate, phosphorus-containing epoxy compounds); nitrogen-containing compounds (e.g., melamine, guanidine); compounds containing oxazine rings; silicone compounds, etc. These polymeric compounds and / or flame-retardant compounds may be used individually or in combination of two or more.

[0163] The first resin layer 12 may also contain various other additives for various purposes. Specific examples of additives include: ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, lubricants, defoamers, dispersants, leveling agents, and gloss agents. These additives may be used alone or in combination of two or more.

[0164] [Second resin layer]

[0165] The second resin layer 13 contains a thermosetting resin. While not particularly limited, examples of thermosetting resins include: epoxy compounds, cyanate ester compounds, maleimide compounds, phenolic compounds, polyphenylene ether compounds, benzoxazine compounds, organo-modified silicone compounds, and compounds having polymerizable unsaturated groups. These compounds can be the same as those exemplified in the first resin layer 12. One of these thermosetting resins can be used, or a suitable mixture of two or more of them can be used. Ideally, the presence of both epoxy and phenolic compounds provides excellent peel strength; further inclusion of maleimide compounds in addition to epoxy and phenolic compounds is even more desirable.

[0166] In this embodiment, when the second resin layer 13 uses an epoxy compound, although its content is not particularly limited, from the viewpoint of heat resistance and curing properties, it is ideally in the range of 10 to 80 parts by weight of resin solids relative to 100 parts by weight of the second resin layer 13, and particularly ideally in the range of 30 to 70 parts by weight.

[0167] In this embodiment, when the second resin layer 13 uses a phenolic compound, although its content is not particularly limited, from the viewpoint of heat resistance and adhesion to the copper foil, it is ideally in the range of 10 to 80 parts by weight of resin solids relative to 100 parts by weight of the second resin layer 13, and more ideally in the range of 20 to 60 parts by weight.

[0168] In this embodiment, when the second resin layer 13 uses a maleimide compound, although its content is not particularly limited, from the viewpoint of heat resistance and adhesion to the copper foil, it is ideally in the range of 10 to 80 parts by weight of resin solids relative to 100 parts by weight of the second resin layer 13, and more ideally in the range of 10 to 50 parts by weight.

[0169] While the thickness of the second resin layer 13 is not particularly limited, from a thin-film perspective, it is ideally 15 μm or less, and more ideally 10 μm or less. Furthermore, if insulation is also considered, the thickness of the second resin layer 13 is ideally 1 μm or more. Ideally, the second resin layer 13 is in a semi-cured state (B-Stage). The second resin layer 13 can be formed, for example, by conventional methods such as coating.

[0170] The second resin layer 13 may, as needed, contain at least one inorganic filler and other components. The inorganic filler and other components may be, for example, the same components described in the first resin layer 12. The second resin layer 13 may or may not contain inorganic fillers, ideally at a content of 35% by volume or less. While adding inorganic fillers improves processability, excessive content can reduce flexibility and increase the likelihood of cracking. Furthermore, the content of inorganic fillers refers to the content of inorganic fillers relative to the second resin layer 13 (inorganic filler / first resin layer × 100).

[0171] [Manufacturing method of copper foil with resin layer]

[0172] The method for manufacturing the copper foil 10 with the resin layer of this embodiment is not particularly limited. As a manufacturing method, for example, a solution (varnish) formed by dissolving or dispersing the composition of the first resin layer 12 in an organic solvent is first applied to the surface of the copper foil 11, followed by heating and / or drying under reduced pressure to remove the solvent and cure it, thereby forming the first resin layer 12. As described above, the first resin layer 12 can be in a semi-cured state or a fully cured state. Subsequently, ideally, a solution (varnish) formed by dissolving or dispersing the composition of the second resin layer 13 in an organic solvent is applied to the first resin layer 12, followed by heating and / or drying under reduced pressure to remove the solvent and cure it, thereby forming the second resin layer 13. At this time, the second resin layer 13 is ideally in a B-stage (semi-cured state). Furthermore, a protective layer such as a plastic film may also be provided on the second resin layer 13. This protective layer is suitably removed during the fabrication of the laminate described later.

[0173] While there are no particular limitations on drying conditions, to dry the first resin layer 12 or the second resin layer 13, the amount of organic solvent is typically less than 10 parts by weight per 100 parts by weight, ideally less than 5 parts by weight. The drying conditions also vary depending on the amount of organic solvent in the varnish. For example, if the varnish contains 30 to 60 parts by weight of organic solvent per 100 parts by weight, it can be dried at a temperature of 50°C to 200°C for approximately 3 to 10 minutes.

[0174] Organic solvents are not particularly limited as long as they can properly dissolve or disperse each component and achieve the effect of the first resin layer 12 or the second resin layer 13. Specific examples of organic solvents include: alcohols (e.g., methanol, ethanol, and propanol); ketones (e.g., acetone, methyl ethyl ketone, and methyl isobutyl ketone); amides (e.g., dimethylacetamide and dimethylformamide); aromatic hydrocarbons (e.g., toluene and xylene); N-methyl-2-pyrrolidone, or γ-butyrolactone, etc. One of these organic solvents may be used, or a mixture of two or more may be suitable.

[0175] There are no particular limitations on the coating method. Common coating methods such as bar coating, air knife coating, gravure coating, reverse gravure coating, micro-gravure coating, micro-reverse gravure coating machine coating, mold coating machine coating, dip coating, spin coating, and spray coating can be used.

[0176] [Laminated materials and their manufacturing methods]

[0177] The laminate of the copper foil 10 with resin layer of this embodiment (hereinafter referred to as "the laminate of this embodiment") can be used, for example, as an additive material for substrates for mounting printed circuit boards or semiconductor components, or for manufacturing coreless substrates.

[0178] The laminate of this embodiment can, for example, be configured as a laminate with added layers, wherein the added layers are formed by alternately laminating a conductor layer and an insulating layer formed using a copper foil 10 with a resin layer. Here, "the insulating layer formed using a copper foil 10 with a resin layer" means, for example, that can be laminated on a substrate on which the conductor layer is formed in a manner that is in contact with the second resin layer 13 of the copper foil 10 with a resin layer. Furthermore, when three or more copper foils 10 with resin layers are used to form the insulating layer, the copper foil 11 can be removed as needed, and the first resin layer 12 and the second resin layer 13 can be laminated to form the insulating layer. Furthermore, the aforementioned conductor layer can be formed by the copper foil 11 of the copper foil 10 with a resin layer, or by laminating other conductors (such as copper foil) such as copper foil from a copper-clad laminate. Figure 2 This is an example of the laminate 20 of this embodiment. The laminate 20 is formed by depositing a copper foil 10 with a resin layer on a substrate 22 on which a conductor layer 21 is formed, in a manner that is in contact with the second resin layer 13, and the insulating layer 23 is formed by the first resin layer 12 and the second resin layer 13.

[0179] When the laminate in this embodiment has an added layer, for example, the added layer has multiple conductor layers and insulating layers, and the conductor layers may be configured to be disposed between each insulating layer and on the surface of the outermost layer of the added layer. In this case, the number of insulating layers is not particularly limited, for example, it may be three or four layers.

[0180] Furthermore, the laminate of this embodiment can be used to fabricate a coreless substrate. Examples of such coreless substrates include those with two or more layers, and those with three layers. The structure of the coreless substrate will be described later.

[0181] Printed Circuit Board

[0182] The laminate system of this embodiment can be used as a printed circuit board. Here, compared to a metal-clad laminate where the insulating resin layer, referred to as the core substrate, has been fully cured, the printed circuit board can be obtained by using a laminate made by using the copper foil 10 with the resin layer of this embodiment as an additive material. If the copper foil 10 with the resin layer of this embodiment (laminate) is used, a thin printed circuit board can be manufactured, for example, without using a thick support substrate (carrier substrate).

[0183] On the surface of a metal-clad laminate, a conductor layer is formed by plating a conductor layer obtained by means of metal foil and / or metal foil peeling and then plating it. In addition, the substrate of the metal-clad laminate is not particularly limited, but is mainly glass epoxy board, metal substrate, polyester substrate, polyimide substrate, BT resin substrate and thermosetting polyphenylene ether substrate.

[0184] In this embodiment, the added layer refers to the first resin layer 12 of the copper foil 10, which is laminated with a resin layer onto the surface of the metal foil and / or conductor layer of the metal foil laminate, and the second resin layer 13, which is laminated as needed. When manufacturing a printed circuit board or a substrate for mounting semiconductor components, even if the copper foil 11 is etched and then plated, the plating adhesion is still improved because the first resin layer 12 has excellent plating adhesion.

[0185] In the manufacturing of printed circuit boards, through-holes and / or vias are often machined as needed to electrically connect the conductor layers. Hole machining is typically performed using methods such as mechanical drilling, CO2 lasers, UV lasers, and YAG lasers.

[0186] In cases where hole machining has already been performed, a roughening process, including the removal of adhesive residue, is subsequently carried out. The roughening process typically consists of a swelling step, a surface roughening and adhesive residue dissolution step, and a neutralization step. The swelling step is performed by using a swelling agent to swell the surface of the insulating resin layer. The swelling agent is not particularly limited as long as it can increase the wettability of the insulating resin layer surface, causing the surface to swell to a degree that promotes oxidative decomposition in the subsequent surface roughening and adhesive residue dissolution steps. Examples include alkaline solutions and surfactant solutions. The surface roughening and adhesive residue dissolution steps are performed using an oxidizing agent. Examples of oxidizing agents include, for example, alkaline permanganate solutions; ideal examples include aqueous solutions of potassium permanganate and sodium permanganate. This oxidant treatment is called wet degumming, but in addition to wet degumming, it can also be combined with dry degumming by plasma treatment or UV treatment, mechanical grinding by polishing machines, sandblasting, and other conventional roughening treatments. The neutralization step involves using a reducing agent to neutralize the oxidant used in the previous step. Examples of reducing agents include amine-based reducing agents; ideal examples include acidic aqueous solutions such as hydroxylamine sulfate, ethylenediaminetetraacetic acid, and azirmonotriacetic acid.

[0187] In this embodiment, it is ideal to perform metal plating after the vias and / or through-holes are formed, or after desmearing treatment is performed within the vias and / or through-holes, to electrically connect the conductor layers. The method of metal plating is not particularly limited, and conventional metal plating methods used in the manufacture of multilayer printed circuit boards can be used. The method of metal plating and the type of plating solution are not particularly limited, and conventional metal plating methods and solutions used in the manufacture of multilayer printed circuit boards can be used. The plating solution can also be commercially available. The metal plating method is not particularly limited, and examples include: treatment with a degreasing solution, treatment with a soft etching solution, pickling, treatment with a pre-immersion solution, treatment with a catalytic solution, treatment with a accelerator solution, treatment with a chemical copper solution, pickling, and treatment involving immersion in a copper sulfate solution with the application of an electric current.

[0188] Furthermore, when using a semi-cured copper foil 10 with a resin layer for layering, the semi-cured first resin layer 12 or second resin layer 13 is typically subjected to heat treatment or other methods to fully cure it, thereby obtaining a printed circuit board. In this embodiment, another copper foil 10 with a resin layer can also be further deposited on the obtained printed circuit board.

[0189] While there are no particular limitations on the lamination method in the build-up process, a vacuum pressure laminator can be appropriately used. In this case, the copper foil 10 with a resin layer can also be laminated using an elastomer such as rubber. The lamination conditions are not particularly limited as long as they are the conditions typically used in printed circuit board lamination, such as a temperature of 70°C to 140°C and a lamination density of 1 kgf / cm³. 2 ~11kgf / cm 2 The process is carried out under a range of contact pressures and an environmental pressure reduction of less than 20 hPa. After the lamination step, the laminated adhesive film can also be smoothed by hot pressing with a metal plate. The lamination and smoothing steps can be performed continuously using a commercially available vacuum pressure laminator. A heat curing step can also be performed after the lamination or smoothing step. By using the heat curing step, the first resin layer 12 and the second resin layer 13 can be completely cured. The heat curing conditions vary depending on the types of components contained in the first resin layer 12 and the second resin layer 13, and the curing temperature is usually 100°C to 300°C, and the pressure is 0.1 kgf / cm. 2 ~100kgf / cm 2 (Approximately 9.8 kPa to approximately 9.8 MPa), with a hardening time of 30 seconds to 5 hours.

[0190] Methods for forming circuit patterns on one or both sides of the copper foil of the printed circuit board of this embodiment can be listed as: semi-additive method, full additive method, subtractive method, etc. Among them, from the viewpoint of forming fine circuit patterns, the semi-additive method is ideal.

[0191] An example of a method for forming circuit patterns using a semi-additive process can be illustrated by selectively applying electroplating (pattern plating) using a plated photoresist, followed by stripping the plated photoresist and etching the entire pattern to form a circuit pattern. In circuit pattern formation using the semi-additive method, electroless plating and electroplating are performed in combination. Ideally, drying should be performed separately after electroless plating and after electroplating. While there are no particular limitations on drying after electroless plating, ideally it should be performed, for example, at 80°C to 180°C for 10 to 120 minutes; similarly, while there are no particular limitations on drying after electroplating, ideally it should be performed, for example, at 130°C to 220°C for 10 to 120 minutes. The plated material is ideally copper.

[0192] An example of a subtractive method for forming circuit patterns is the technique of selectively removing a conductor layer using an etched photoresist to form the circuit pattern. Specifically, this can be performed as follows: A dry film photoresist (RD-1225, manufactured by Hitachi Chemical) is laminated onto the entire surface of a copper foil at a temperature of 110±10°C and a pressure of 0.50±0.02 MPa. Next, the circuit pattern is exposed and shielded. Subsequently, the dry film photoresist is developed in a 1% sodium carbonate aqueous solution, and finally, it is stripped using an amine-based photoresist stripping solution. This forms a circuit pattern on the copper foil.

[0193] In this embodiment, an insulating resin layer and / or a conductor layer can be further deposited on the printed circuit board to obtain a multilayer printed circuit board. The inner layers of the multilayer printed circuit board may also include a circuit board. The copper foil 10 with the resin layer is one of the insulating resin layer and conductor layer constituting the multilayer printed circuit board.

[0194] There are no particular limitations on the lamination method; common lamination methods used for printed circuit boards can be used. Examples of lamination methods include: multi-stage presses, multi-stage vacuum presses, laminators, vacuum laminators, and autoclave forming machines. While there are no particular limitations on the lamination temperature, a range of 100℃ to 300℃ is suitable; similarly, there are no particular limitations on the pressure, but 0.1 kgf / cm² is acceptable. 2 ~100kgf / cm 2 The heating range (approximately 9.8 kPa to approximately 9.8 MPa) is suitable for selection; the heating time is not particularly limited, but for example, it is suitable to select a range of 30 seconds to 5 hours. In addition, post-hardening can also be carried out as needed, for example, in a temperature range of 150°C to 300°C, to adjust the degree of hardening.

[0195] [Substrate for mounting semiconductor components]

[0196] As described above, the multilayer system of this embodiment can be used as a substrate for mounting semiconductor components. The substrate for mounting semiconductor components is, for example, manufactured by depositing a resin-coated copper foil 10 onto a metal-clad laminate, and shielding and patterning the copper foil on one or both sides of the resulting multilayer. The shielding and patterning can utilize conventional shielding and patterning methods performed in the manufacture of printed circuit boards, and are not particularly limited, but ideally, the circuit pattern is formed using the aforementioned subtraction method. The circuit pattern can be formed only on one side of the multilayer or on both sides of the multilayer.

[0197] [Multilayer coreless substrate (multilayer printed circuit board)]

[0198] The laminate in this embodiment can be a coreless substrate as described above. An example of the aforementioned coreless substrate is a multilayer coreless substrate.

[0199] A multilayer coreless substrate, for example, may be configured as follows: having a plurality of insulating layers consisting of a first insulating layer and one or more second insulating layers deposited on one side of the first insulating layer, and a plurality of conductor layers consisting of a first conductor layer disposed between the plurality of insulating layers and a second conductor layer disposed on the outermost surface of the plurality of insulating layers, wherein the first insulating layer and the aforementioned second insulating layer each have a first resin layer 12 and a second resin layer 13 of a copper foil 10 with a resin layer attached, which are hardened. Figure 3 This will illustrate a specific example of a multilayer coreless substrate. Figure 3 This is a schematic diagram illustrating an example of a multilayer coreless substrate according to this embodiment. Figure 3 The multilayer coreless substrate 100 shown includes a first insulating layer 111 and two second insulating layers 112 deposited on one side (top direction in the diagram) of the first insulating layer 111. The first insulating layer 111 and the two second insulating layers 112 are each formed using a first resin layer 12 and a second resin layer 13 of a copper foil 10 with a resin layer attached. Furthermore, Figure 3 The multilayer coreless substrate 100 shown has multiple conductor layers, and the aforementioned multiple conductor layers are formed by a first conductor layer 113 disposed between each of the multiple insulating layers (first insulating layer 111 and second insulating layer 112) and a second conductor layer 114 disposed on the outermost layer of the multiple insulating layers (first insulating layer 111 and second insulating layer 112).

[0200] Thus, according to this embodiment, a copper foil with a resin layer that has excellent insulation, plating adhesion, and moisture absorption and heat resistance can be obtained, as well as a laminate using the same.

[0201] [Example]

[0202] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to these examples.

[0203] (Examples 1-7)

[0204] A composition for obtaining the first resin layer 12 is obtained by blending 15.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 49.9 parts by weight of a polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 34.9 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.), and 0.2 parts by weight of 2,4,5-tribenzamide (manufactured by Tokyo Chemical Industry Co., Ltd.). Next, the composition for obtaining the first resin layer 12 is diluted with N-methyl-2-pyrrolidone (hereinafter referred to as "NMP") to obtain varnish A. The obtained varnish A was applied to the matte side of a 12 μm thick copper foil 11 (product name: 3EC-M2S-VLP, manufactured by Mitsui Metals & Mining Co., Ltd.) using a bar coater. The matte side of the copper foil 11 was used as the surface, and the ten-point average surface roughness Rz was set to 1.7 μm in Examples 1-5, 0.3 μm in Example 6, and 4.5 μm in Example 7. Subsequently, the coated film was heated and dried at 180°C for 10 minutes, thereby forming a first resin layer 12 on the copper foil 11.

[0205] In addition, the composition comprising 35.8 parts by weight of biphenyl aralkyl phenolic resin (product name: KAYAHARD GPH-103, hydroxyl equivalent: 230 g / eq, manufactured by Nippon Kayaku Co., Ltd.), 17.9 parts by weight of bis(3-ethyl-5-methyl-4-maleimide diphenyl)methane (product name: BMI-70, manufactured by KI Kasei Co., Ltd.), 7.0 parts by weight of naphthyl aralkyl epoxy resin (product name: HP-9900-75M, epoxy equivalent: 274 g / eq., manufactured by DIC Co., Ltd.), 38.8 parts by weight of biphenyl aralkyl epoxy resin (product name: NC-3000-FH-75M, manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent: 320 g / eq.), and 0.5 parts by weight of 2,4,5-tribenzimidazole (manufactured by Tokyo Kasei Corporation) is obtained as the second resin layer 13. Next, the composition of the second resin layer 13 is diluted with methyl ethyl ketone to obtain varnish B. The obtained varnish B is then applied onto the first resin layer 12 obtained by the above method using a bar coater. Subsequently, the coated film is heated and dried at 150°C for 10 minutes to obtain a copper foil 10 with a resin layer having the first resin layer 12 and the second resin layer 13.

[0206] The thickness of the first resin layer 12 and the thickness of the second resin layer 13 vary in the various embodiments as follows. In Example 1, the thickness of the first resin layer 12 is 1.5 μm, and the thickness of the second resin layer 13 is 2.5 μm; in Example 2, the thickness of the first resin layer 12 is 2.5 μm, and the thickness of the second resin layer 13 is 2.5 μm; in Example 3, the thickness of the first resin layer 12 is 5.0 μm, and the thickness of the second resin layer 13 is 2.5 μm; in Example 4, the thickness of the first resin layer 12 is 2.5 μm, and the thickness of the second resin layer 13 is 1.5 μm; in Example 5, the thickness of the first resin layer 12 is 2.5 μm, and the thickness of the second resin layer 13 is 10 μm; in Example 6, the thickness of the first resin layer 12 is 2.5 μm, and the thickness of the second resin layer 13 is 2.5 μm; in Example 7, the thickness of the first resin layer 12 is 2.5 μm, and the thickness of the second resin layer 13 is 5.0 μm.

[0207] (Example 8)

[0208] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 18.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 49.9 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 31.9 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.), and 0.2 parts by weight of 2,4,5-tribenzamide (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0209] (Example 9)

[0210] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 10.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 51.9 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 37.9 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.), and 0.2 parts by weight of 2,4,5-tribenzamide (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0211] (Example 10)

[0212] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2, and the first resin layer 12 is formed on the surface of the copper foil 11. The composition of the first resin layer 12 is obtained by blending 15.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 49.9 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 34.9 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.), 0.2 parts by weight of 2,4,5-tribenzimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), and 79.8 parts by weight of silica (product name: K180SQ-C1, average particle size 0.18 μm, manufactured by Admatechs Co., Ltd.) as an inorganic filler. The content of inorganic filler in the first resin layer 12 (inorganic filler / first resin layer × 100) is 30.3% by volume.

[0213] In addition to changing the composition of the second resin layer 13, everything else is the same as in Example 2, with the second resin layer 13 formed on the first resin layer 12. The composition of the second resin layer 13 is a blended (mixed) biphenyl aryl phenolic resin (product name: KAYAHARD). The product was obtained by means of 35.8 parts by weight of GPH-103 (hydroxyl equivalent: 230 g / eq, manufactured by Nippon Kayaku Co., Ltd.), 17.9 parts by weight of bis(3-ethyl-5-methyl-4-maleimide diphenyl)methane (product name: BMI-70, manufactured by KI Kasei Co., Ltd.), 7.0 parts by weight of naphthyl alkyl epoxy resin (product name: HP-9900-75M, epoxy equivalent: 274 g / eq., manufactured by DIC Co., Ltd.), 38.8 parts by weight of biphenyl alkyl epoxy resin (product name: NC-3000-FH-75M, manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent: 320 g / eq.), 0.5 parts by weight of 2,4,5-tribenzimidazole (manufactured by Tokyo Kasei Kogyo Co., Ltd.), and 99.5 parts by weight of slurry silica as an inorganic filler (product name: M273, average particle size 0.1 μm, manufactured by CIKNanoTek Co., Ltd.). The content of inorganic filler in the second resin layer 13 (inorganic filler / second resin layer × 100) is 35.2% by volume.

[0214] (Example 11)

[0215] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 10.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 49.9 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 39.9 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.), and 0.2 parts by weight of 2,4,5-tribenzimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0216] (Example 12)

[0217] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 7.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 49.9 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 42.9 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.), and 0.2 parts by weight of 2,4,5-tribenzamide (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0218] (Example 13)

[0219] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 3.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 49.9 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 46.9 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.), and 0.2 parts by weight of 2,4,5-tribenzamide (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0220] (Comparative Example 1)

[0221] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 50.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends and 50.0 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.).

[0222] (Comparative Example 2)

[0223] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 30.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends and 70.0 parts by weight of a polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.).

[0224] (Comparative Example 3)

[0225] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 15.0 parts by weight of a polyphenylene ether compound (product name: OPE-2St2200, manufactured by Mitsubishi Gas Chemical Co., Ltd.) with styrene-terminated ends, 50.0 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.), and 35.0 parts by weight of an epoxy compound (product name: LCE-2615, manufactured by Nippon Kayaku Co., Ltd.).

[0226] (Comparative Example 4)

[0227] Except for changing the composition of the first resin layer 12, everything else is the same as in Example 2. The first resin layer 12 is formed on the surface of the copper foil 11, and the second resin layer 13 is formed on the first resin layer 12. The composition of the first resin layer 12 is obtained by blending 50.0 parts by weight of polyimide resin (product name: Neopulim (registered trademark) S100, manufactured by Mitsubishi Gas Chemical Co., Ltd.) and 50.0 parts by weight of 2,2-bis-(4-(4-maleimide phenoxy)phenyl)propane (product name: BMI-80, manufactured by KI Chemical Co., Ltd.).

[0228] (Comparative Example 5)

[0229] Except for the fact that the average roughness Rz of the ten points on the surface of the copper foil 11 is set to 10.5 μm, everything else is the same as in Example 7. A first resin layer 12 is formed on the surface of the copper foil 11, and a second resin layer 13 is formed on the first resin layer 12.

[0230] (Characteristic Evaluation)

[0231] The characteristics of each embodiment and each comparative example were determined using the following methods.

[0232] (Insulation evaluation)

[0233] The copper foil surfaces on both sides of the copper-clad laminate (HL832NS (trade name) T / T0.2mmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) are etched to a depth of approximately 0.5μm to 1μm (inner layer roughening treatment, CZ8101 (trade name), manufactured by MEC Corporation). Copper foil 10 with resin layers, as described in each embodiment and comparative example, is then disposed on both sides with the second resin layer 13 as the inner side, and subjected to a pressure of 30 kgf / cm². 2 A copper-clad laminate is obtained by performing a lamination process (thermosetting) at 220°C for 120 minutes. Next, an outer layer circuit for evaluating insulation is fabricated on the obtained copper-clad laminate using a subtractive method, thereby obtaining a substrate for insulation evaluation.

[0234] The resistance of the obtained insulation evaluation substrate was measured for 300 hours in a HAST test chamber (130°C, 85% RH, 5.0V), followed by measurement of the resistance after removal from the HAST test chamber. The results showed that when there was no short circuit in the HAST test chamber, the resistance after removal was 1 × 10⁻⁶. 8 When the value is Ω, the rating is 0 (good); otherwise, the rating is ×.

[0235] (Evaluation of coating adhesion)

[0236] For the copper foil 10 with resin layer obtained in each embodiment and comparative example, after etching the copper foil 10, electroless plating and electroplating of copper are performed to obtain a test piece with a plating layer of 20 μm thickness. The peel strength is measured using this test piece. Peel strength is determined by fixing the lower layer of the test piece to a board or similar material, stretching the edge of the plating layer perpendicular to the direction of the fixed board, and using the load required for peeling as the adhesion strength of the interface between the upper and lower layers. A peel strength of 0.5 kN / m or higher is considered good.

[0237] (Evaluation of moisture absorption and heat resistance)

[0238] The copper foil surfaces on both sides of the copper-clad laminate (HL832NS (trade name) T / T0.2mmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) are etched to a depth of approximately 0.5μm to 1μm (inner layer roughening treatment, CZ8101 (trade name), manufactured by MEC Corporation). Copper foil 10 with resin layers, as described in each embodiment and comparative example, is then disposed on both sides with the second resin layer 13 as the inner side, and subjected to a pressure of 30 kgf / cm². 2 A copper-clad laminate was obtained by lamination (thermosetting) at 220°C for 120 minutes. The obtained copper-clad laminate was then cut into 50mm×50mm pieces to obtain test pieces for testing. As a pretreatment, the heat resistance was evaluated by placing the obtained test pieces in a constant temperature bath at 120°C for 3 hours and then immersing them in a solder bath at 260°C for 30 seconds. After 30 seconds, it was confirmed whether delamination occurred between the following layers: (1) the copper foil on the surface of the copper-clad laminate and the layer containing the hardened material of the first resin layer 12 and the second resin layer 13, and (2) the layer containing the hardened material of the first resin layer 12 and the second resin layer 13 and the layer containing the hardened material of the resin composition in the copper-clad laminate (HL832NS (trade name) T / T0.2mmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.). For (1) and (2), if no delamination occurs, the rating is 0; if at least one of them delamination occurs, the rating is ×. The conditions and evaluation results of each embodiment and each comparative example are shown in Table 1 and Table 2.

[0239] [Table 1]

[0240]

[0241] [Table 2]

[0242]

[0243] As shown in Tables 1 and 2, good results were obtained in insulation, plating adhesion, and moisture absorption and heat resistance according to Examples 1 to 13. In contrast, no good results were obtained in Comparative Examples 1 to 5. That is, it can be seen that if the first resin layer 12 contains polyphenylene ether compound (A), polyimide resin (B), and maleimide compound (C), and the ten-point average roughness Rz of the copper foil 11 is set to 0.3 μm or more and 10 μm or less, excellent insulation, plating adhesion, and moisture absorption and heat resistance will be obtained.

[0244] [Symbol Explanation]

[0245] 10: Copper foil with resin layer

[0246] 11: Copper Foil

[0247] 12: First resin layer

[0248] 13: Second resin layer

[0249] 20: Laminated body

[0250] 21: Conductor layer

[0251] 22:Substrate

[0252] 23: Insulation layer

[0253] 100: Multilayer coreless substrate

[0254] 111: First insulating layer

[0255] 112: Second insulating layer

[0256] 113: First conductor layer

[0257] 114: Second conductor layer

Claims

1. A copper foil with a resin layer, comprising a copper foil and a first resin layer deposited on the surface of the copper foil; characterized in that... The first resin layer contains: polyphenylene ether compound (A), polyimide resin (B), and maleimide compound (C); The surface roughness Rz of the copper foil at ten points is between 0.3 μm and 10 μm. Relative to 100 parts by weight of resin solids, the proportion of polyphenylene ether compound (A) in the first resin layer is 3 parts by weight or more and less than 20 parts by weight, the proportion of polyimide resin (B) is 10 parts by weight or more and less than 80 parts by weight, and the proportion of maleimide compound (C) is 5 parts by weight or more and less than 75 parts by weight. The first resin layer is provided with a second resin layer containing a thermosetting resin. The second resin layer contains at least one compound selected from the group consisting of epoxy compounds, cyanate compounds, maleimide compounds, phenolic compounds, polyphenylene ether compounds, benzoxazine compounds, and organo-modified silicone compounds. The second resin layer differs from the first resin layer in at least one of its constituent components and physical properties.

2. The copper foil with a resin layer as described in claim 1, wherein, The first resin layer contains no inorganic filler, or contains inorganic filler in a volume percentage of less than 35%.

3. The copper foil with a resin layer as described in claim 2, wherein, The inorganic filler in the first resin layer contains at least one selected from magnesium hydroxide, magnesium oxide, silicon dioxide, molybdenum compounds, aluminum oxide, aluminum nitride, glass, talc, titanium compounds, and zirconium oxide.

4. The copper foil with a resin layer as described in claim 1, wherein, The thickness of the first resin layer is between 1.5 μm and 5 μm.

5. The copper foil with a resin layer as described in claim 1, wherein, The second resin layer contains no inorganic filler, or contains inorganic filler in a content of less than 36% by volume.

6. The copper foil with a resin layer as described in claim 5, wherein, The inorganic filler in the second resin layer contains at least one selected from magnesium hydroxide, magnesium oxide, silicon dioxide, molybdenum compounds, aluminum oxide, aluminum nitride, glass, talc, titanium compounds, and zirconium oxide.

7. The copper foil with a resin layer as described in claim 1, wherein, The thickness of the second resin layer is between 1 μm and 15 μm.

8. A laminate, characterized in that, It has a conductor layer and an extension layer formed using a copper foil with a resin layer as described in claim 1.

Citation Information

Patent Citations

  • Thermosetting resin composition, insulation material for build-up construction method, and build-up printed- wiring board

    JP2001011296A

  • Method for producing solvent-soluble polyimide

    JP2005015629A

  • Insulation resin sheet

    JP2017050561A

  • Metallic foil with resin, laminated plate, printed wiring board and multilayer printed wiring board

    JP2018001632A

  • Copper foil with resin

    WO2010073952A1