A ternary positive electrode material and preparation method thereof
Through the mixing method of alternate rotation processing in the mixing container, the crack problem caused by the mixing method in the preparation of high-nickel ternary positive electrode materials is solved, and the uniform doping and high discharge capacity of the material are achieved, which improves the cycle stability and Structural integrity.
Patent Information
- Application Number
- CN202310015753.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-01-04
AI Technical Summary
In the existing high-nickel ternary cathode material preparation methods, the mixing method can easily lead to cracks or crushing of the material, affecting the cycle stability and discharge capacity.
The ternary precursor particles and lithium source are rotated simultaneously in the mixing container in a vertical and horizontal direction, and combined with the alternating mixing method of clockwise and counterclockwise rotation to avoid the huge force generated by mechanical stirring and achieve uniformity. Mixing and doping to prevent electrolyte from being injected into the inside of the material.
It realizes uniform mixing and doping of ternary positive electrode materials, improves the cyclic stability and discharge capacity of the material, avoids material fragmentation and side reactions, and is suitable for large-scale mass production.
Smart Images

Figure CN116102082B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of positive electrode materials, and in particular, relates to a ternary positive electrode material and a preparation method thereof. Background Art
[0002] The discharge capacity and first efficiency of high-nickel ternary positive electrode materials are closely related to the uniformity of the raw material mixing, especially the uniform mixing between the lithium source and the high-nickel ternary precursor to obtain a higher discharge capacity and the first discharge to charge capacity ratio. In addition, in order to obtain good cycle stability, high-nickel ternary positive electrode materials also need element doping and surface coating. In order for the doping elements and surface coating to play a good effect, the precursor or positive electrode material powder needs to be evenly mixed with the dopant and coating agent. If uniform doping cannot be achieved, it is difficult to inhibit oxygen evolution and stabilize the TM-O bond, and if the material cannot be uniformly coated, the exposed part will still react with the electrolyte in the fully charged state, and the electrolyte will also be injected into the material from the through-cracks, causing rapid failure.
[0003] At present, the raw material mixing in the process of high-nickel ternary positive electrode materials mainly relies on high-speed mixers or mechanical stirrers. Under the action of high-speed rotating stirring paddles, the materials move from the bottom of the mixer to the side wall, climb to a certain height, and then fall under the action of gravity to mix. However, it is difficult to mix the lithium source and the high-nickel ternary precursor powder under low-speed stirring of mechanical paddles. Although the mixing is relatively uniform under high-speed stirring, the bonding force between the high-nickel ternary precursor particles is weak and the impact resistance is poor. After high-speed mechanical stirring, it is easy to crack or even break. In addition, when using a ball mill to add balls to mix, a large amount of precursors will also crack or even crush due to the fierce collision between the grinding balls and between the grinding balls and the particles. The cracks generated by the precursor can easily cause the electrolyte to be injected from the cracks into the interior of the positive electrode material, resulting in serious side reactions, causing the material to fail quickly and affect the positive electrode cycle stability. Summary of the invention
[0004] The purpose of the present application is to provide a ternary positive electrode material and a preparation method thereof, aiming to solve the problem that the mixing method adopted in the existing preparation method of the ternary positive electrode material easily causes the material to crack or even break.
[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0006] In a first aspect, the present application provides a method for preparing a ternary positive electrode material, comprising:
[0007] Provide ternary precursor particles and lithium source;
[0008] The ternary precursor particles and the lithium source are added to a mixing container for a first mixing process to obtain a first mixture; the first mixing process includes the following first cycle process: the mixing container is first rotated in a vertical direction and in a horizontal direction at the same time, and then the mixing container is rotated in a vertical direction and in a horizontal direction at the same time; the first rotation process in the vertical direction is opposite to the second rotation process in the vertical direction, and the first rotation process in the horizontal direction is opposite to the second rotation process in the horizontal direction;
[0009] The first mixture is subjected to a first sintering treatment to obtain a first ternary positive electrode material.
[0010] In a second aspect, the present application provides a ternary positive electrode material, including a ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in the present application.
[0011] Compared with the prior art, this application has the following beneficial effects:
[0012] The first aspect of the present application provides a method for preparing a ternary positive electrode material, which comprises rotating a mixing container containing ternary precursor particles and a lithium source in a first vertical direction and a first horizontal direction at the same time, and then rotating the mixing container in a second vertical direction and a second horizontal direction at the same time, and making the first rotation in the vertical direction opposite to the second rotation in the vertical direction, and the first rotation in the horizontal direction and the second rotation in the horizontal direction opposite to each other. By repeating the above-mentioned first cycle process many times, the ternary precursor particles and the lithium source can be uniformly mixed. Therefore, by rotating the mixing container containing ternary precursor particles and a lithium source in a horizontal direction and a vertical direction at the same time, and combining clockwise rotation and counterclockwise rotation alternately, not only can the ternary precursor particles and the lithium source be fully mixed, but also the huge force generated by the mechanical stirring paddle can be avoided to cause the ternary precursor particles to break, thereby effectively preventing the electrolyte from being directly injected into the interior of the positive electrode material from the cracks. Therefore, the ternary positive electrode material prepared by the preparation method of the present application has good cycle stability and high discharge capacity. In addition, the preparation method has simple steps, is easy to implement, and is suitable for large-scale mass production.
[0013] The ternary positive electrode material provided in the second aspect of the present application is prepared by the preparation method of the ternary positive electrode material provided in the present application, so it has good structural integrity and can effectively prevent the electrolyte from being directly injected into the interior of the positive electrode material from the cracks, thereby having the advantages of good cycle stability and high discharge capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0015] Figure 1 is a process flow chart of a method for preparing a ternary positive electrode material provided in an embodiment of the present application;
[0016] Figure 2 It is a diagram of the mixing process in the method for preparing the ternary positive electrode material provided in the embodiment of the present application;
[0017] Figure 3 This is a physical picture of the first mixture obtained by the method for preparing the ternary positive electrode material provided in Example 1 of the present application;
[0018] Figure 4 is a SEM image of the first mixture obtained by the method for preparing the ternary positive electrode material provided in Example 1 of the present application;
[0019] Figure 5 This is a SEM image of the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Example 1 of the present application;
[0020] Figure 6 is a SEM image of the first mixture prepared by the method for preparing the ternary positive electrode material provided in Example 2 of the present application;
[0021] Figure 7 This is a SEM image of the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Example 2 of the present application;
[0022] Figure 8 This is a SEM image of the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Example 3 of the present application;
[0023] Fig. 9 This is a SEM image of the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Comparative Example 1 of the present application;
[0024] Fig.10 This is a SEM image of the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Comparative Example 2 of the present application;
[0025] Fig.11 This is a physical picture of the first mixture obtained by the method for preparing the ternary positive electrode material provided in Comparative Example 3 of the present application;
[0026] Fig.12This is a SEM image of the first mixture prepared by the method for preparing the ternary positive electrode material provided in Comparative Example 3 of the present application;
[0027] Fig.13 This is a SEM image of a ternary positive electrode material obtained by the preparation method of a ternary positive electrode material provided in Comparative Example 3 of the present application;
[0028] Fig.14 This is a SEM image of the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Comparative Example 4 of the present application;
[0029] Fig.15 It is the charge and discharge curve of the button battery assembled with the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Example 1 of the present application;
[0030] Fig.16 It is the charge and discharge curve of the button battery assembled with the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Example 2 of the present application;
[0031] Fig.17 It is the charge and discharge curve of the button battery assembled with the ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Example 3 of the present application;
[0032] Fig.18 is a cycle stability curve of a button cell assembled with a ternary positive electrode material prepared by the method for preparing a ternary positive electrode material provided in Example 3 of the present application;
[0033] Fig.19 This is a cycle stability curve of a button cell assembled with a ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Comparative Example 2 of the present application;
[0034] Fig. 20 This is the charge and discharge curve of a button cell assembled with a ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in Comparative Example 3 of the present application. DETAILED DESCRIPTION
[0035] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0036] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0037] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0038] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0039] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0040] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0041] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0042] The first aspect of the present application provides a method for preparing a ternary positive electrode material, such as Figure 1 As shown, including:
[0043] S01: Provide ternary precursor particles and lithium source;
[0044] S02: adding the ternary precursor particles and the lithium source into a mixing container for a first mixing process to obtain a first mixture; the first mixing process includes the following first cycle process: the mixing container is first rotated in a vertical direction and in a horizontal direction at the same time, and then the mixing container is rotated in a vertical direction and in a horizontal direction at the same time; the first rotation process in the vertical direction is opposite to the second rotation process in the vertical direction, and the first rotation process in the horizontal direction is opposite to the second rotation process in the horizontal direction;
[0045] S03: performing a first sintering process on the first mixture to obtain a first ternary positive electrode material.
[0046] The preparation method of the ternary positive electrode material provided in the embodiment of the present application is as follows: the mixing container containing the ternary precursor particles and the lithium source is first rotated in the vertical direction and in the horizontal direction at the same time, and then the mixing container is rotated in the vertical direction and in the horizontal direction at the same time, and the first rotation in the vertical direction is opposite to the second rotation in the vertical direction, and the first rotation in the horizontal direction is opposite to the second rotation in the horizontal direction. By repeating the above-mentioned first cycle process many times, the ternary precursor particles and the lithium source can be uniformly mixed. Therefore, by rotating the mixing container containing the ternary precursor particles and the lithium source in the horizontal direction and in the vertical direction at the same time, and combining the clockwise rotation and the counterclockwise rotation alternately, not only can the ternary precursor particles and the lithium source be fully mixed, but also the huge force generated by the mechanical stirring paddle can be avoided to cause the ternary precursor particles to break, thereby effectively preventing the electrolyte from being directly injected into the interior of the positive electrode material from the cracks. Therefore, the ternary positive electrode material prepared by the preparation method of the present application has good cycle stability and high discharge capacity. In addition, the preparation method has simple steps, is easy to implement, and is suitable for large-scale mass production.
[0047] In the above step S01, the general formula of the ternary precursor is Ni x Co y Mn z (OH)2, x+y+z=1, 0.9≤x≤1, 0≤y≤0.1, 0≤z≤0.1; for example, the ternary precursor can be Ni 0.9 Co 0.06 Mn 0.04 (OH)2、Ni 0.92 Co 0.06 Mn 0.02 (OH)2、Ni 0.95 Co 0.03 Mn 0.02(OH)2. The lithium source may be lithium hydroxide monohydrate. In the embodiment, the molar ratio of the ternary precursor to the lithium source is 1:(1-1.1), such as 1:1, 1:1.05, 1:1.1, etc., and appropriate amounts of the ternary precursor and the lithium source may be weighed according to the molar ratio.
[0048] In the above step S02, the mixing container is first rotated in the vertical direction and in the horizontal direction at the same time for the first time, and then the mixing container is rotated in the vertical direction and in the horizontal direction for the second time, which may include the following four situations: the mixing container is first rotated in the vertical direction clockwise and in the horizontal direction clockwise at the same time, and then the mixing container is rotated in the vertical direction counterclockwise and in the horizontal direction counterclockwise at the same time. Alternatively, the mixing container is first rotated in the vertical direction counterclockwise and in the horizontal direction counterclockwise at the same time, and then the mixing container is rotated in the vertical direction clockwise and in the horizontal direction clockwise at the same time. Alternatively, the mixing container is first rotated in the vertical direction clockwise and in the horizontal direction counterclockwise at the same time, and then the mixing container is rotated in the vertical direction clockwise and in the horizontal direction clockwise at the same time. Alternatively, the mixing container is first rotated in the vertical direction clockwise and in the horizontal direction counterclockwise at the same time, and then the mixing container is rotated in the vertical direction counterclockwise and in the horizontal direction clockwise at the same time. Alternatively, the mixing container is first rotated counterclockwise in the vertical direction and clockwise in the horizontal direction simultaneously, and then the mixing container is rotated clockwise in the vertical direction and counterclockwise in the horizontal direction simultaneously.
[0049] Figure 2 Although three materials are shown as mixed, it should be noted that two materials and three materials can be used Figure 2 Example description. In the embodiment, Figure 2As shown, the specific steps of adding the ternary precursor particles and the lithium source into the mixing container for the first mixing treatment may include: adding the ternary precursor particles and the lithium source into the mixing container, and rotating the mixing container counterclockwise in the vertical direction and counterclockwise in the horizontal direction at the same time, and then rotating the mixing container clockwise in the vertical direction and clockwise in the horizontal direction at the same time, and obtaining the first mixture by alternating the clockwise rotation treatment and the counterclockwise rotation treatment N times, where N may be an integer greater than 1. The alternating clockwise rotation treatment and the counterclockwise rotation treatment can be understood as clockwise rotation treatment, counterclockwise rotation treatment, clockwise rotation treatment, counterclockwise rotation treatment, clockwise rotation treatment, counterclockwise rotation treatment..., and so on. The clockwise rotation treatment of the mixing container in the vertical direction and the counterclockwise rotation treatment in the vertical direction can be understood as the revolution treatment of the mixing container, and the clockwise rotation treatment of the mixing container in the horizontal direction and the counterclockwise rotation treatment in the horizontal direction can be understood as the rotation treatment of the mixing container. Alternatively, rotating the mixing container clockwise in the vertical direction and rotating it counterclockwise in the vertical direction can be understood as the rotation of the mixing container, and rotating the mixing container clockwise in the horizontal direction and rotating it counterclockwise in the horizontal direction can be understood as the revolution of the mixing container. In the embodiment of the present application, by rotating the mixing container containing the ternary precursor particles and the lithium source in the horizontal direction and in the vertical direction at the same time, and combining the mixing method of alternating clockwise rotation and counterclockwise rotation, the ternary precursor particles and the lithium source can be fully mixed, without the need for mechanical stirring paddle stirring, and the fragmentation of the ternary precursor particles caused by the huge force generated by stirring can be avoided, so that the obtained ternary positive electrode material has good structural integrity.
[0050] In an embodiment, adding the ternary precursor particles and the lithium source to the mixing container for the first mixing treatment includes: adding the dopant, the ternary precursor particles and the lithium source to the mixing container for the first mixing treatment. It can be understood that the ternary precursor particles, the lithium source and the dopant are added to the mixing container, the mixing container is first rotated in the vertical direction and in the horizontal direction at the same time, and then the mixing container is rotated in the vertical direction and in the horizontal direction at the same time; and the first rotation in the vertical direction is opposite to the second rotation in the vertical direction, and the first rotation in the horizontal direction is opposite to the second rotation in the horizontal direction. After repeating the above first cycle process for many times, the dopant, the ternary precursor particles and the lithium source can be fully mixed to obtain a mixture, and the mixture is subjected to a first sintering treatment to obtain a doped ternary positive electrode material. Therefore, by rotating the mixing container containing the dopant, the ternary precursor particles and the lithium source in the horizontal direction and in the vertical direction at the same time, and combining the mixing method of alternating clockwise rotation and counterclockwise rotation, that is, the mixing method of alternating forward rotation and reverse rotation, the dopant, the ternary precursor particles and the lithium source can be fully and uniformly mixed, and the uniform doping of the ternary positive electrode material is achieved without using a mechanical stirring paddle, thereby avoiding the breakage of the ternary precursor particles caused by the huge force generated by the stirring, thereby achieving the purpose of inhibiting oxygen evolution and stabilizing the TM-O bond.
[0051] In an embodiment, the molar ratio of the total molar amount of nickel, cobalt and manganese of the ternary precursor to the doping element of the dopant is 1:(0.001-0.03), for example, 1:0.001, 1:0.005, 1:0.01, 1:0.02, 1:0.03. It can be understood that if the doping element is too little, it is not conducive to improving the stability of the material structure. If the doping element is too much, it is easy to cause the capacity to decay and the conductivity to decrease. Therefore, within the scope of the embodiment of the present application, it is conducive to improving the stability of the material structure and improving the cycle stability of the material, so that the material has the best comprehensive performance. The dopant may include at least one of NaOH, Al2O3, Al(OH)3, MgO, Mg(OH)2, B2O3, H3BO3, TiO2, HF, LiF, and NH4F.
[0052] In an embodiment, the number of cycles of the first cycle process is 2 to 30 times, for example, 2 times, 5 times, 10 times, 15 times, 20 times, 25 times, 30 times, etc. After completing the number of cycles of the first cycle process, the ternary precursor particles and the lithium source in the mixing container can be fully and evenly mixed.
[0053] In the embodiment, the speed of the first rotation process in the vertical direction, the first rotation process in the horizontal direction, the second rotation process in the vertical direction and the second rotation process in the horizontal direction are independently 100-500 r / min, and the time is 1-30 min. For example, the speed is 100 r / min, 200 r / min, 300 r / min, 400 r / min, 500 r / min, etc., and the time is 1 min, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min.
[0054] In the above step S03, the first sintering treatment includes: keeping at 490-600°C for 1-3 hours in an oxygen atmosphere, and then sintering at 650-750°C for 8-20 hours. In an oxygen atmosphere, first keep at 490-600°C for 1-3 hours to pre-lithiate the lithium source and remove the crystal water, and then sinter at 650-750°C for 8-20 hours to react the lithium source with the ternary precursor to form a ternary positive electrode material. In application, the sintering furnace may include but is not limited to a tubular furnace, a box furnace, a roller kiln, etc.
[0055] After the first sintering treatment is performed in the above step S03, step S04 is also included: adding the coating agent and the first ternary positive electrode material to the mixing container for a second mixing treatment to obtain a second mixture; the second mixing treatment includes the following second cycle process: the mixing container is first rotated in the vertical direction for the third time and in the horizontal direction for the third time at the same time, and then the mixing container is rotated in the vertical direction for the fourth time and in the horizontal direction for the fourth time at the same time; the third rotation treatment in the vertical direction is opposite to the fourth rotation treatment in the vertical direction, and the third rotation treatment in the horizontal direction is opposite to the fourth rotation treatment in the horizontal direction. The second mixture is subjected to a second sintering treatment to obtain a second ternary positive electrode material.
[0056] In step S04, the mixing container is first subjected to the third rotation process in the vertical direction and the third rotation process in the horizontal direction at the same time, and then the mixing container is subjected to the fourth rotation process in the vertical direction and the fourth rotation process in the horizontal direction at the same time, which may include the following four situations: the mixing container is first subjected to the clockwise rotation process in the vertical direction and the clockwise rotation process in the horizontal direction at the same time, and then the mixing container is subjected to the counterclockwise rotation process in the vertical direction and the counterclockwise rotation process in the horizontal direction at the same time. Alternatively, the mixing container is first subjected to the counterclockwise rotation process in the vertical direction and the counterclockwise rotation process in the horizontal direction at the same time, and then the mixing container is subjected to the clockwise rotation process in the vertical direction and the clockwise rotation process in the horizontal direction at the same time. Alternatively, the mixing container is first subjected to the clockwise rotation process in the vertical direction and the counterclockwise rotation process in the horizontal direction at the same time, and then the mixing container is subjected to the counterclockwise rotation process in the vertical direction and the clockwise rotation process in the horizontal direction at the same time. Alternatively, the mixing container is first rotated counterclockwise in the vertical direction and clockwise in the horizontal direction simultaneously, and then the mixing container is rotated clockwise in the vertical direction and counterclockwise in the horizontal direction simultaneously.
[0057] In an embodiment, Figure 2 As shown, the specific steps of adding the coating agent and the first ternary positive electrode material to the mixing container for the second mixing treatment may include: adding the coating agent and the first ternary positive electrode material to the mixing container, and rotating the mixing container counterclockwise in the vertical direction and counterclockwise in the horizontal direction at the same time, and then rotating the mixing container clockwise in the vertical direction and clockwise in the horizontal direction at the same time, and performing the clockwise rotation treatment and the counterclockwise rotation treatment alternately N times to obtain the first mixture, where N may be an integer greater than 1. The alternating clockwise rotation treatment and the counterclockwise rotation treatment may be understood as clockwise rotation treatment, counterclockwise rotation treatment, clockwise rotation treatment, counterclockwise rotation treatment, clockwise rotation treatment, counterclockwise rotation treatment, etc., and so on. In this embodiment, the coating agent can be uniformly coated on the surface of the first ternary positive electrode material by rotating the mixing container containing the coating agent and the first ternary positive electrode material in the horizontal direction and in the vertical direction at the same time, and by combining the mixing method of rotating clockwise and counterclockwise alternately, so as to prevent the exposed part of the ternary positive electrode material from having a side reaction with the electrolyte. In addition, there is no need to stir with a mechanical stirring paddle, so the fragmentation of the ternary precursor particles caused by the huge force generated by stirring can be avoided, and therefore, the electrolyte can be prevented from being injected from the through cracks to cause rapid failure inside the material.
[0058] In an embodiment, the number of cycles of the second cycle process is 2 to 100 times, such as 2 times, 5 times, 10 times, 20 times, 40 times, 60 times, 80 times, 100 times, etc. After completing the number of cycles of the second cycle process, the coating agent in the mixing container can be uniformly coated on the surface of the first ternary positive electrode material. The coating agent includes at least one of ZrO2, Nb2O5, MoO3, TaO2, CeO2, and SiO2.
[0059] In the embodiment, the rotation speeds of the third rotation process in the vertical direction, the third rotation process in the horizontal direction, the fourth rotation process in the vertical direction, and the fourth rotation process in the horizontal direction are independently 100-600 r / min, and the time is 1-30 min. For example, the rotation speed is 100 r / min, 200 r / min, 300 r / min, 400 r / min, 500 r / min, 600 r / min, etc., and the time is 1 min, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min.
[0060] In an embodiment, the conditions of the second sintering treatment include: an oxygen atmosphere, a temperature of 300-750° C., and a time of 0.5-20 hours. In applications, the sintering furnace may include but is not limited to a tube furnace, a box furnace, a roller kiln, and the like.
[0061] A second aspect of an embodiment of the present application provides a ternary positive electrode material, including a ternary positive electrode material prepared by the preparation method of the ternary positive electrode material provided in the present application.
[0062] The ternary positive electrode material provided in the embodiment of the present application is prepared by the preparation method of the ternary positive electrode material provided in the present application, so it has good structural integrity and can effectively prevent the electrolyte from being directly injected into the interior of the positive electrode material from the cracks, thereby having the advantages of good cycle stability and high discharge capacity.
[0063] The following describes the invention in conjunction with specific embodiments.
[0064] Example 1
[0065] This embodiment provides a method for preparing a ternary positive electrode material, comprising the following steps:
[0066] S11: According to the molar ratio of 1:1.04, weigh an appropriate amount of ternary precursor particles (Ni 0.90 Co 0.06 Mn 0.04 (OH)2) and lithium hydroxide monohydrate particles;
[0067] S12: adding ternary precursor particles and lithium hydroxide monohydrate particles into a mixing kettle, and rotating the mixing kettle vertically at a speed of 350 r / min clockwise for 1 min and horizontally at a speed of 350 r / min clockwise for 1 min, and then rotating the mixing kettle vertically at a speed of 350 r / min counterclockwise for 1 min and horizontally at a speed of 350 r / min counterclockwise for 1 min, and repeating the above process 30 times to obtain a first mixture;
[0068] S13: The first mixture is placed in a tube furnace and oxygen is introduced at a flow rate of 300 sccm. The temperature is first increased to 500°C at a heating rate of 5°C / min and kept at this temperature for 1 hour. The temperature is then increased to 735°C at a heating rate of 2°C / min and kept at this temperature for 16 hours. After natural cooling, the mixture is successively refined, washed with water and vacuum dried. Finally, the mixture is placed in a tube furnace in an oxygen atmosphere and heated to 720°C at a heating rate of 3°C / min and kept at this temperature for 6 hours. After natural cooling, the mixture is refined and sieved to obtain a ternary positive electrode material (LiNi 0.90 Co 0.06 Mn 0.04 O2).
[0069] Example 2
[0070] This embodiment provides a method for preparing a ternary positive electrode material, comprising the following steps:
[0071] S21: According to the molar ratio of 1:1.02, weigh an appropriate amount of ternary precursor particles (Ni 0.95 Co 0.03 Mn 0.02 (OH)2) and lithium hydroxide monohydrate particles;
[0072] S22: adding the ternary precursor particles and the lithium hydroxide monohydrate particles into a mixing kettle, and rotating the mixing kettle clockwise at a speed of 100 r / min in the vertical direction for 15 min and in the horizontal direction for 15 min at a speed of 100 r / min, and then rotating the mixing kettle counterclockwise at a speed of 100 r / min in the vertical direction for 15 min and in the horizontal direction for 15 min at a speed of 100 r / min, and repeating the above process twice to obtain a first mixture;
[0073] S23: The first mixture is placed in a tubular furnace and oxygen is introduced at a flow rate of 400 sccm, and the temperature is first increased to 500°C at a heating rate of 5°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 700°C at a heating rate of 3°C / min, and the temperature is kept for 18 hours. After natural cooling, the mixture is refined, washed with water, and vacuum dried in sequence. Finally, the mixture is placed in a tubular furnace in an oxygen atmosphere and the temperature is increased to 720°C at a heating rate of 3°C / min, and the temperature is kept for 6 hours. After natural cooling, the mixture is refined and sieved to obtain a ternary positive electrode material (LiNi 0.95 Co 0.03 Mn 0.02 O2).
[0074] Example 3
[0075] This embodiment provides a method for preparing a ternary positive electrode material, comprising the following steps:
[0076] S31: According to the molar ratio of the ternary precursor to lithium hydroxide being 1:1.04, the molar ratio of the total molar amount of Ni, Co, and Mn elements in the ternary precursor to the Al element in aluminum hydroxide being 0.997:0.003, weigh an appropriate amount of ternary precursor particles (Ni 0.90 Co 0.06 Mn 0.04 (OH)2), lithium hydroxide monohydrate particles and aluminum hydroxide;
[0077] S32: adding ternary precursor particles, lithium hydroxide monohydrate particles and aluminum hydroxide into a mixing kettle, and rotating the mixing kettle clockwise at a speed of 500 r / min for 2 min in the vertical direction and clockwise at a speed of 500 r / min for 2 min in the horizontal direction, and then rotating the mixing kettle counterclockwise at a speed of 500 r / min for 2 min in the vertical direction and counterclockwise at a speed of 500 r / min for 2 min in the horizontal direction, and repeating the above process 15 times to obtain a first mixture;
[0078] S33: The first mixture is placed in a tubular furnace and oxygen is introduced at a flow rate of 300 sccm, and the temperature is first increased to 500°C at a heating rate of 5°C / min, and the temperature is kept for 1 hour, and then the temperature is increased to 735°C at a heating rate of 2°C / min, and the temperature is kept for 12 hours. After natural cooling, the mixture is refined, washed with water, and vacuum dried in sequence. Finally, the mixture is placed in a tubular furnace in an oxygen atmosphere and the temperature is increased to 720°C at a heating rate of 3°C / min, and the temperature is kept for 6 hours. After natural cooling, the mixture is refined and sieved to obtain a ternary positive electrode material (Li(Ni 0.90 Co 0.06 Mn 0.04 ) 0.997 Al 0.003 O2);
[0079] S34: According to the molar ratio of 1:0.002:0.001, weigh an appropriate amount of Li(Ni 0.90 Co 0.06 Mn 0.04 ) 0.997 Al 0.003 O2, ZrO2 nanoparticles and B2O3 particles are added to the mixing kettle, and the mixing kettle is first rotated clockwise at a speed of 380 r / min in the vertical direction for 1 min and in the horizontal direction for 1 min at a speed of 380 r / min, and then the mixing kettle is rotated counterclockwise at a speed of 380 r / min in the vertical direction for 1 min and in the horizontal direction for 1 min at a speed of 380 r / min, and the above process is repeated 15 times to obtain a second mixture;
[0080] S35: placing the second mixture in a tubular furnace in an oxygen atmosphere, heating it to 720°C at a heating rate of 3°C / min, keeping it warm for 6 hours, and then refining and sieving to obtain a coated ternary positive electrode material.
[0081] Comparative Example 1
[0082] This comparative example provides a method for preparing a ternary positive electrode material, comprising the following steps:
[0083] S1: According to the molar ratio of 1:1.04, weigh an appropriate amount of ternary precursor particles (Ni 0.90 Co 0.06 Mn 0.04 (OH)2) and lithium hydroxide monohydrate particles;
[0084] S2: adding the ternary precursor particles and the lithium hydroxide monohydrate particles into a ball mill (100 mL), and then adding two zirconium oxide balls (with particle sizes of 7 mm and 3 mm, respectively), and rotating the ball mill clockwise and counterclockwise for 2 min at a speed of 300 r / min for a total of 20 min to obtain a first mixture;
[0085] S3: The first mixture was placed in a tube furnace and oxygen was introduced at a flow rate of 300 sccm. The temperature was first increased to 500°C at a heating rate of 5°C / min and kept at that temperature for 1 hour. The temperature was then increased to 735°C at a heating rate of 2°C / min and kept at that temperature for 16 hours. After natural cooling, the mixture was refined, washed with water and vacuum dried in sequence. Finally, the mixture was placed in a tube furnace in an oxygen atmosphere and heated to 720°C at a heating rate of 3°C / min and kept at that temperature for 6 hours. After natural cooling, the mixture was refined and sieved to obtain a ternary positive electrode material (LiNi 0.90 Co 0.06 Mn 0.04 O2).
[0086] Comparative Example 2
[0087] This comparative example provides a method for preparing a ternary positive electrode material, including steps S1 to S5; wherein steps S1 to S3 and S5 are the same as steps S31 to S33 and S35 of Example 3;
[0088] The difference from Example 3 is that in step S4 of this comparative example, an appropriate amount of Li(Ni 0.90 Co 0.06 Mn 0.04 ) 0.997 Al 0.003 O2, ZrO2 nanoparticles and B2O3 particles were added to the ball mill, and then two zirconium oxide balls (particle sizes were 7 mm and 3 mm, respectively) were added. The ball mill was rotated clockwise for 2 min and counterclockwise for 2 min alternately at a speed of 280 r / min for a total of 60 min to obtain a second mixture.
[0089] Comparative Example 3
[0090] This comparative example provides a method for preparing a ternary positive electrode material, comprising the following steps:
[0091] S1: According to the molar ratio of the ternary precursor to lithium hydroxide being 1:1.04, the molar ratio of the total molar amount of Ni, Co, and Mn elements in the ternary precursor to the Al element in aluminum hydroxide being 0.997:0.003, weigh an appropriate amount of ternary precursor particles (Ni 0.92 Co 0.06 Mn 0.02 (OH)2), lithium hydroxide monohydrate particles and aluminum hydroxide;
[0092] S2: adding ternary precursor particles, lithium hydroxide monohydrate particles and aluminum hydroxide into a conical cavity (2L) of a high-speed mixer, and rotating at a speed of 300 r / min for 2 h to obtain a first mixture;
[0093] S3: The first mixture is placed in a tube furnace and oxygen is introduced at a flow rate of 300 sccm. The temperature is first increased to 500°C at a heating rate of 5°C / min and kept at this temperature for 1 hour. The temperature is then increased to 735°C at a heating rate of 2°C / min and kept at this temperature for 16 hours. After natural cooling, the mixture is refined, washed with water and vacuum dried in sequence. Finally, the mixture is placed in a tube furnace in an oxygen atmosphere and heated to 720°C at a heating rate of 3°C / min and kept at this temperature for 6 hours. After natural cooling, the mixture is refined and sieved to obtain a ternary positive electrode material (Li(Ni 0.90 Co 0.06 Mn 0.04 ) 0.997 Al 0.003 O2).
[0094] Comparative Example 4
[0095] This comparative example provides a method for preparing a ternary positive electrode material, comprising the following steps:
[0096] S1: According to the molar ratio of 1:1.02, weigh an appropriate amount of ternary precursor particles (Ni 0.95 Co 0.03 Mn 0.02 (OH)2) and lithium hydroxide monohydrate particles;
[0097] S2: adding the ternary precursor particles and the lithium hydroxide monohydrate particles into a ball mill (100 mL), and then adding two zirconium oxide balls (with particle sizes of 7 mm and 3 mm, respectively), and rotating the ball mill clockwise and counterclockwise for 2 min at a speed of 250 r / min for 10 min to obtain a first mixture;
[0098] S3: The first mixture was placed in a tubular furnace and oxygen was introduced at a flow rate of 400 sccm. The temperature was first increased to 500°C at a heating rate of 5°C / min and kept for 1 hour. The temperature was then increased to 700°C at a heating rate of 2°C / min and kept for 16 hours. After natural cooling, the mixture was refined, washed with water and vacuum dried in sequence. Finally, the mixture was placed in a tubular furnace in an oxygen atmosphere and heated to 720°C at a heating rate of 3°C / min and kept for 6 hours. After natural cooling, the mixture was refined and sieved to obtain a ternary positive electrode material (LiNi 0.95 Co 0.03 Mn 0.02 O2)
[0099] Related performance test analysis:
[0100] 1. The uniformity of the materials after mixing and the microscopic morphology of the prepared ternary positive electrode materials of Examples 1 to 3 and Comparative Examples 1 to 4 were observed using a scanning electron microscope (SEM). The test results are as follows: Figures 3 to 12 .
[0101] 2. According to the mass ratio of 90:5:5, the ternary positive electrode materials, conductive agents and binders prepared in Examples 1 to 3 and Comparative Examples 2 to 3 were respectively made into positive electrode sheets, and then assembled into button batteries, and electrochemical performance tests were performed. The test conditions were: the assembled batteries were charged and discharged at room temperature at 0.1C constant current and constant voltage, the charge and discharge voltage was 2.7-4.3V, and the cut-off charge current was 0.005C; the charge and discharge cycle test was performed at 45°C at 0.5C constant current and constant voltage, the charge and discharge voltage was 2.7-4.3V, and the cut-off charge current was 0.005C. The test results are shown in Table 1 below:
[0102] Table 1
[0103]
[0104] Figure 3 This is a physical picture of the first mixture obtained in Example 1; Figure 4 is a SEM image of the first mixture obtained in Example 1; Figure 5 This is a SEM image of the ternary cathode material prepared in Example 1; Figure 6 is a SEM image of the first mixture obtained in Example 2; Figure 7 This is a SEM image of the ternary cathode material prepared in Example 2; Figure 8 This is a SEM image of the ternary cathode material prepared in Example 3; Fig. 9 This is a SEM image of the ternary positive electrode material prepared in Comparative Example 1; Fig.10 This is a SEM image of the ternary positive electrode material prepared in Comparative Example 2; Fig.11 This is a physical picture of the first mixture obtained in Comparative Example 3; Fig.12 is a SEM image of the first mixture prepared in Comparative Example 3; Fig.13 This is a SEM image of the ternary positive electrode material prepared in Comparative Example 3; Fig.14 This is a SEM image of the ternary positive electrode material prepared in Comparative Example 4. Figure 3 It can be seen that the mixture of Example 1 (the first mixture) is uniform and no white powder is present. Figure 4 It can be seen that the ternary precursor particles and lithium hydroxide monohydrate are evenly dispersed after mixing, and the ternary precursor particles remain intact without obvious surface cracks and fragments. Figure 5 It can be seen that the ternary cathode material prepared in Example 1 is uniformly lithiated after sintering without obvious cracks and fragments. Figure 6 It can be seen that after mixing in Example 2, the ternary precursor particles and lithium hydroxide monohydrate are evenly mixed, and the ternary precursor particles remain intact without obvious surface cracks and fragments. Figure 7 It can be seen that the ternary cathode material prepared in Example 2 is uniformly lithiated after sintering, but since the Ni95 ternary precursor itself is relatively fragile, a small amount of cracks exist after high-temperature calcination; Figure 8 It can be seen that the ternary cathode material prepared in Example 3 is evenly lithiated after sintering, has no obvious cracks and fragments, and has a uniform coating layer formed on the surface. Fig. 9 It can be seen that the ternary positive electrode material prepared in Comparative Example 1 has obvious crushing phenomenon; Fig.10 It can be seen that the ternary cathode material prepared in Comparative Example 2 has a large number of cracks and fragments; Fig.11 It can be seen that the mixing of Comparative Example 3 is very uneven, and there is a large amount of white powder (lithium hydroxide monohydrate). Fig.12It can be seen that the ternary precursor particles and lithium hydroxide monohydrate are unevenly dispersed after mixing, and many fragments appear. Fig.13 It can be seen that there are many fragments in the ternary positive electrode material prepared in Comparative Example 3; Fig.14 It can be seen that the ternary cathode material prepared in Comparative Example 4 has a large amount of crushing phenomenon; this indicates that Comparative Example 1 uses a two-ball milling method to mix the ternary precursor particles with lithium hydroxide monohydrate. Although the mixture is uniform, the ternary precursor particles are easily broken due to the mechanical impact of the grinding balls. Comparative Example 2 uses a two-ball milling method to mix the ternary cathode material with the coating agent. The mechanical impact of the grinding balls easily causes the ternary cathode material to break. Therefore, from Figures 3 to 14 It is shown that the embodiment of the present application can fully mix the ternary precursor particles and the lithium source, and fully mix the ternary positive electrode material and the coating agent by rotating the mixing container containing the ternary precursor particles and the lithium source in the horizontal direction and in the vertical direction at the same time, and combining clockwise rotation and counterclockwise rotation alternately, without the need for mechanical stirring paddle stirring, which can avoid the breakage of the ternary precursor particles or the ternary positive electrode material caused by the huge force generated by stirring.
[0105] Fig.15 The charge and discharge curves of button cells assembled with the ternary cathode material prepared in Example 1, wherein battery #1 and battery #2 are two parallel experiments conducted with the same ternary cathode material; Fig.16 The charge and discharge curves of button cells assembled with the ternary cathode material prepared in Example 2, wherein battery #1 and battery #2 are two parallel experiments conducted with the same ternary cathode material; Fig.17 The charge and discharge curve of the button cell assembled with the ternary cathode material prepared in Example 3; Fig.18 The cycle stability curve of the button cell assembled with the ternary cathode material prepared in Example 3; Fig.19 The cycle stability curve of the button cell assembled with the ternary cathode material prepared in Comparative Example 2; Fig. 20 The charge and discharge curves of button cells assembled with ternary cathode materials prepared in Comparative Example 3, where battery #1 and battery #2 are two parallel experiments conducted with the same ternary cathode material. Figures 15-20As can be seen from Table 1, the first discharge specific capacity and the first coulombic efficiency of the batteries corresponding to the ternary positive electrode materials prepared in Examples 1 to 3 are significantly higher than the first discharge specific capacity and the first coulombic efficiency of the batteries corresponding to the ternary positive electrode materials prepared in Comparative Example 3, and the capacity retention rate of the batteries corresponding to the ternary positive electrode materials prepared in Example 3 after 50 cycles is significantly higher than the capacity retention rate of the batteries corresponding to the ternary positive electrode materials prepared in Comparative Example 2 after 50 cycles, which further illustrates that the embodiments of the present application utilize a mixing container containing ternary precursor particles and a lithium source to rotate horizontally and vertically at the same time, and to combine clockwise rotation and counterclockwise rotation alternately, which can not only fully mix the ternary precursor particles and the lithium source, and fully mix the ternary positive electrode material and the coating agent, but also maintain the structural integrity of the ternary positive electrode material, and can effectively prevent the electrolyte from being directly injected into the interior of the positive electrode material from the cracks, thereby achieving better cycle stability and higher discharge capacity.
[0106] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a ternary positive electrode material, characterized in that: include: Provide ternary precursor particles and lithium source; The ternary precursor particles and the lithium source are added to a mixing container for a first mixing process to obtain a first mixture; the first mixing process includes the following first cycle process: the mixing container is first rotated in a vertical direction and in a horizontal direction at the same time, and then the mixing container is rotated in a vertical direction and in a horizontal direction at the same time; The first rotation process in the vertical direction is opposite to the second rotation process in the vertical direction, and the first rotation process in the horizontal direction is opposite to the second rotation process in the horizontal direction; The first mixture is subjected to a first sintering treatment to obtain a first ternary positive electrode material.
2. The preparation method according to claim 1, characterized in that Adding the ternary precursor particles and the lithium source into a mixing container for a first mixing process includes: adding a dopant, the ternary precursor particles and the lithium source into a mixing container for the first mixing process.
3. The preparation method according to claim 2, characterized in that: After the step of performing the first sintering treatment, the method further includes adding the coating agent and the first ternary positive electrode material into a mixing container for a second mixing treatment to obtain a second mixture; the second mixing treatment includes the following second cycle process: the mixing container is first subjected to a third rotation treatment in the vertical direction and a third rotation treatment in the horizontal direction at the same time, and then the mixing container is subjected to a fourth rotation treatment in the vertical direction and a fourth rotation treatment in the horizontal direction at the same time; the third rotation treatment in the vertical direction is opposite to the fourth rotation treatment in the vertical direction, and the third rotation treatment in the horizontal direction is opposite to the fourth rotation treatment in the horizontal direction; The second mixture is subjected to a second sintering treatment to obtain a second ternary positive electrode material.
4. The preparation method according to claim 3, characterized in that: The number of cycles of the second cycle process is 2 to 100; and / or The rotation speeds of the third rotation process in the vertical direction, the third rotation process in the horizontal direction, the fourth rotation process in the vertical direction, and the fourth rotation process in the horizontal direction are independently 100 to 600 r / min, and the time is 1 to 30 min.
5. The preparation method according to claim 3, characterized in that: The conditions of the second sintering treatment include: an oxygen atmosphere, a temperature of 300 to 750° C., and a time of 0.5 to 20 hours.
6. The preparation method according to claim 3, characterized in that: At least one of the following conditions is met: The molar ratio of the ternary precursor to the lithium source is 1:(1-1.1); The molar ratio of the total molar amount of nickel, cobalt and manganese of the ternary precursor to the doping element of the dopant is 1:(0.001-0.03); The dopant includes at least one of NaOH, Al2O3, Al(OH)3, MgO, Mg(OH)2, B2O3, H3BO3, TiO2, HF, LiF, and NH4F; The coating agent includes at least one of ZrO2, Nb2O5, MoO3, TaO2, CeO2, and SiO2.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The number of cycles of the first cycle process is 2 to 30; and / or The rotation speeds of the first rotation process in the vertical direction, the first rotation process in the horizontal direction, the second rotation process in the vertical direction and the second rotation process in the horizontal direction are independently 100 to 500 r / min, and the time is 1 to 30 min.
8. The preparation method according to claim 7, characterized in that: The first sintering treatment includes: keeping the temperature at 490-600° C. for 1-3 hours in an oxygen atmosphere, and then sintering at 650-750° C. for 8-20 hours.