A method for treating medical waste slag and building material prepared by the method

By pretreatment, granulation, mixing, pressing and heat treatment of medical waste slag, high-performance building materials are prepared, which solves the problems of low utilization rate of medical waste slag and environmental pollution, and provides a new direction for diversified solid waste treatment.

CN116102280BActive Publication Date: 2024-10-18SHANGHAI SOLID WASTE DISPOSAL CENT
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310097009.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-08
Publication Date
2024-10-18
Estimated Expiration
2043-02-08

AI Technical Summary

Technical Problem

The existing methods for treating waste slag from traditional Chinese medicine have problems of low utilization rate and environmental pollution. Moreover, the technical level of solid waste treatment is limited at this stage, making it difficult to prepare building materials with good performance.

Method used

By preprocessing, granulating, mixing with inorganic fibers and burning aids, pressing and heat treatment of medical waste slag, building materials with high strength and good water resistance, acid and alkali resistance are prepared.

Benefits of technology

It effectively improves the utilization rate of medical waste slag, solves the problem of environmental pollution, and provides a new direction for the diversified treatment of solid waste. The prepared building materials have high strength and good water resistance, acid and alkali resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116102280B_ABST
    Figure CN116102280B_ABST
Patent Text Reader

Abstract

The present invention provides a method for treating medical waste slag and a building material prepared by the method, and specifically relates to the field of solid waste resource utilization. The treatment method comprises pre-treating medical waste slag to obtain slag powder; granulating the slag powder to obtain granulated powder; uniformly mixing the granulated powder with inorganic fiber and a sintering aid to obtain a mixed powder; pressing the mixed powder into a shape to obtain a green body; heat-treating the green body, and cooling it to obtain a building material. The method for treating medical waste slag of the present invention effectively turns medical waste slag into treasure, which not only solves the environmental pollution problem caused by medical waste slag, but also provides a direction for the diversified treatment of solid waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to a method for treating medical waste slag and a building material prepared by the method. Background Art

[0002] Medical waste slag is the solid waste left after the incineration of medical waste. At present, the main treatment method for medical waste slag is landfill, which requires more land and has a greater impact on the environment. The resource utilization of solid waste is the development direction of solid waste treatment. Many solid wastes can be used as environmentally friendly materials or building materials after treatment. However, due to the limitations of the current technical level, my country's solid waste treatment has the disadvantages of low utilization rate and low product quality.

[0003] Therefore, it is necessary to develop a new solid waste treatment process to improve the utilization rate of solid waste and prepare products with better performance, so as to increase the enthusiasm of all sectors of society for solid waste treatment and solve the current serious problem of medical waste slag accumulation. Summary of the invention

[0004] In view of the above shortcomings of the prior art, the present invention provides a method for treating medical waste slag and a building material prepared by the method, which improves the utilization rate of medical waste slag and improves the land occupation and environmental pollution problems of medical waste slag.

[0005] To achieve the above-mentioned purpose and other related purposes, the present invention provides a method for treating medical waste slag, comprising pretreating the medical waste slag to obtain slag powder; granulating the slag powder to obtain granulated powder; uniformly mixing the granulated powder with inorganic fiber and a sintering aid to obtain a mixed powder; pressing the mixed powder into a shape to obtain a green body; heat treating the green body and cooling it to obtain a building material.

[0006] In one example of the present invention, the medical waste slag contains SiO 2 30~40wt%;Al 2 O 3 5~15wt%; CaO20~30wt%; Fe 2 O 3 5~15wt%;Na 2 O 0~5wt%.

[0007] In one example of the present invention, pre-treatment of medical waste slag includes: placing the medical waste slag in a drying oven and drying it at a temperature of 100 to 200° C. for 2 to 6 hours; placing the dried medical waste slag in a ball mill for crushing, wherein the crushing time is 6 to 12 hours; and screening the crushed medical waste slag with a 40 to 80 mesh sieve to obtain medical waste slag powder with uniform particle size.

[0008] In one example of the present invention, the grinding balls of the ball mill are one or more of alumina, zirconia, and stainless steel grinding balls, the diameter of the grinding balls is 3 cm to 20 cm, and the ball-to-material mass ratio is (1 to 2):1.

[0009] In one example of the present invention, the amount of granulation binder used in the step of granulating the slag powder is 0.5wt% to 10wt% of the mass of the slag powder, and the granulation binder is a polyvinyl alcohol (PVA) aqueous solution, and the concentration of the polyvinyl alcohol aqueous solution is 3wt% to 15wt%.

[0010] In one example of the present invention, the granulated powder is evenly mixed with inorganic fibers and a sintering aid, including placing the granulated powder in a mixer, adding inorganic fibers and a sintering aid, and mixing in the mixer for 2 to 6 hours to obtain a uniformly mixed mixed powder, wherein the mass of the inorganic fibers is 10wt% to 60wt% of the mass of the slag powder, and the mass of the sintering aid is 5wt% to 20wt% of the mass of the slag powder.

[0011] In an example of the present invention, the inorganic fiber includes one or more of glass fiber, alumina fiber, and mullite fiber; the sintering aid includes one or two of glass powder and sodium silicate.

[0012] In one example of the present invention, the mixed powder is pressed into shape, comprising: placing the mixed material in a pressing mold for pressing, wherein the pressing pressure is 3 to 10 MPa and the holding time is 10 to 30 seconds.

[0013] In one example of the present invention, the green body is heat treated, including: placing the green body in a kiln at a temperature of 700 to 1000° C. for 1 to 6 hours.

[0014] The present invention also provides a building material, wherein the building material is prepared using medical waste slag as a main raw material and the medical waste slag treatment method of the present invention.

[0015] The method for treating medical waste slag of the present invention prepares building materials by pretreating the medical waste slag, granulating, mixing with inorganic fibers and sintering aids, pressing and forming, and heat treating the medical waste slag, and the building materials have high strength and good water resistance, acid and alkali resistance. The method for treating medical waste slag of the present invention effectively turns the medical waste slag into treasure, which not only solves the environmental pollution problem caused by the medical waste slag, but also provides a direction for the diversified treatment of solid waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 This is a flow chart of the method for treating medical waste slag of the present invention;

[0018] Figure 2 The present invention is a flow chart of pretreatment in the method for treating medical waste slag. DETAILED DESCRIPTION

[0019] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.

[0020] In the present application, "%" and "wt%" represent mass percentage unless otherwise specified.

[0021] See also Figure 1 to Figure 2 The present invention provides a method for treating medical waste slag and a building material prepared by the method. The building material is prepared by using medical waste slag as the main raw material, which not only solves the environmental problems caused by medical waste slag, but also provides a direction for the diversified treatment of solid waste.

[0022] See also Figure 1 The method for treating medical waste slag of the present invention comprises at least the following steps:

[0023] S1. Pre-treating medical waste slag to obtain slag powder;

[0024] S2, granulating the slag powder to obtain granulated powder;

[0025] S3, mixing the granulated powder with inorganic fiber and sintering aid to obtain a mixed powder;

[0026] S4, pressing the mixed powder into a shape to obtain a green body;

[0027] S5, heat-treating the green body and cooling it to obtain a building material.

[0028] Specifically, the main components of the medical waste slag in step S1 include SiO 2 (Silicon dioxide), Al 2 O 3 (aluminum oxide), CaO (calcium oxide), Fe 2 O 3 (Iron Oxide) and Na 2 O (sodium oxide), and of course some other impurities. The contents of various components in medical waste slag are shown in Table 1.

[0029]

[0030] See also Figure 1 and Figure 2 In step S1, pre-treating the medical waste slag includes:

[0031] S11, placing the medical waste slag in a drying oven and drying it at 100-200°C for 2-6 hours;

[0032] S12, placing the dried medical waste slag in a ball mill for crushing, wherein the crushing time is 6 to 12 hours;

[0033] S13, using a 40-80 mesh sieve to sieve the crushed medical waste slag to obtain medical waste slag powder with uniform particle size.

[0034] Among them, the drying box in step S11 can be, for example, a blast drying box, and the medical waste slag is placed in the blast drying box for drying to remove the moisture in the medical waste slag. The drying temperature can be, for example, 100°C, 150°C or 200°C, and the drying time can be, for example, 2h, 4h or 6h. The drying temperature and drying time are not limited here, and can be set according to actual conditions to achieve the purpose of drying the medical waste slag. For example, if the selected drying temperature is low and the water evaporates slowly, the drying time can be set longer; if the selected drying temperature is high and the water evaporates quickly, the drying time can be set shorter.

[0035] Medical waste slag is solid waste left after the incineration of medical waste. It contains large particles, which is not conducive to the mixing of various components. Therefore, after drying, it needs to be crushed in step S12 to crush it into powder. The crushing method of the present invention is ball milling, which can obtain uniform and continuous powder raw materials with good particle morphology.

[0036] In step S12, the dried medical waste slag is placed in a ball mill for crushing for 6 to 12 hours, such as 6 hours, 8 hours, 10 hours or 12 hours. The crushing time is determined according to the actual crushing situation and is not limited here. Among them, the grinding balls used in the ball mill include one or more of aluminum oxide, zirconium oxide, and stainless steel grinding balls, that is, the grinding balls can be single-material grinding balls, such as aluminum oxide grinding balls or zirconium oxide grinding balls or stainless steel grinding balls; any two or three combinations can also be used, such as aluminum oxide and zirconium oxide combined grinding balls, stainless steel and aluminum oxide combined grinding balls, zirconium oxide and stainless steel combined grinding balls, or aluminum oxide, zirconium oxide, stainless steel three grinding balls. When a combination of grinding balls is used, there is no restriction on the ratio between the components in the combination, and they can be mixed in any proportion. Preferably, aluminum oxide grinding balls and stainless steel grinding balls are used. The diameter of the grinding balls is 3 cm to 20 cm, such as 3 cm, 8 cm, 12 cm, 16 cm or 20 cm. In order to make the crushing result more uniform, the ball-to-material mass ratio in the ball mill (the mass ratio of grinding balls to medical waste slag) is (1-2):1, and the ball-to-material mass ratio is, for example, 1:1, 1.5:1 or 2:1.

[0037] Since ball milling can only crush brittle inorganic slag, but cannot crush large pieces of metal and other difficult-to-crush slag, the material needs to be screened after the crushing process, and the difficult-to-crush slag can be removed by screening. In addition, the gradation of the raw material powder can be adjusted by screening, making subsequent granulation mixing, heat treatment and other processes easier to control. Step S13 of the present invention uses a 40-80 mesh sieve to screen the slag to remove large particles of slag. The mesh sieve can be selected as 40 mesh, 60 mesh or 80 mesh, for example.

[0038] Please continue reading Figure 1 , step S2 granulates the slag powder obtained in step S1. Granulation is to bond multiple particles together to form a larger and rounder particle aggregate, so as to have stronger fluidity. The slag powder and the granulation binder are placed in a granulator, and granulation is performed according to a conventional granulation process to obtain granulated powder. Wherein, the amount of the granulation binder is 0.5wt% to 10wt% of the mass of the slag powder, for example, 0.5wt%, 3wt%, 7wt% or 10wt%, etc. Preferably, the amount of the granulation binder is 1wt% to 5wt% of the mass of the slag powder, for example, 1wt%, 2wt%, 4wt% or 5wt%, etc. In one embodiment, the granulation binder is a PVA aqueous solution, and its concentration (the mass of PVA as a percentage of the total mass of the PVA aqueous solution) is 3wt% to 15wt%, for example, the concentration of the PVA aqueous solution is 3wt%, 6wt%, 9wt%, 12wt% or 15wt%; preferably, the concentration of the PVA aqueous solution is 5wt% to 10wt%, for example, 5wt%, 8wt% or 10wt%.

[0039] Step S3 mixing specifically includes: mixing the granulation powder, inorganic fiber and sintering aid in a mixer in a certain proportion. The mixer can be a three-dimensional mixer. The mixing cylinder of the three-dimensional mixer moves in multiple directions, which can promote the material to make a three-way composite movement along the cylinder in the circumferential, radial and axial directions, so as to achieve the mutual flow, diffusion, accumulation and doping of the materials, so as to achieve the purpose of uniform mixing and better mixing effect. The mixing time of the granulation powder, inorganic fiber and sintering aid in the mixer is 2 to 6 hours, such as 2 hours, 4 hours or 6 hours, for the purpose of uniform mixing.

[0040] The addition of inorganic fiber in step S3 can not only improve the strength of the material, but also improve the thermal stability of the material. The inorganic fiber includes one or more of glass fiber, alumina fiber, and mullite fiber, that is, the inorganic fiber can be any one of the listed types, such as glass fiber or alumina fiber or mullite fiber; it can also be any two or three combinations of the listed types, such as a combination of glass fiber and alumina fiber, a combination of alumina and mullite fiber, a combination of glass fiber and mullite fiber, or a combination of glass fiber, alumina fiber and mullite fiber. When the inorganic fiber composition is used, there is no restriction on the proportion of each component in the composition, and it can be mixed in any proportion. Of course, the inorganic fiber can also be selected from other unlisted components. The amount of inorganic fiber added is 10wt% to 60wt% of the mass of the slag powder, for example, 10wt%, 30wt%, 50wt% or 60wt%, etc.

[0041] The sintering aid includes any one or two of glass powder and sodium silicate, for example, the sintering aid is glass powder, sodium silicate or a combination of glass powder and sodium silicate. When the sintering aid is a combination of glass powder and sodium silicate, there is no restriction on the ratio between the components in the composition, and they can be mixed in any proportion. Glass powder and sodium silicate have a low melting temperature, and after melting, the particles can be effectively bonded together, which can not only effectively reduce the sintering temperature, but also obtain a finished product with higher strength. Preferably, the sintering aid uses glass powder, which can be processed from glass waste, and a new product is processed from the two wastes, which will effectively improve the utilization rate of solid waste. The melting point of glass powder is 500-900°C, and the specification is 100-200 mesh. The amount of sintering aid added is 5wt%-20wt% of the mass of the slag powder, for example, 5wt%, 12wt% or 20wt%.

[0042] In step S4, the mixed powder is placed in a pressing mold for pressing, and the pressure during pressing is 3-10 MPa, preferably 5-10 MPa, such as 5 MPa, 8 MPa or 10 MPa; the holding time is 10-30 s, such as 10 s, 20 s or 30 s, etc. After pressing, a green body with a certain strength is obtained.

[0043] Step S5 is to heat treat the green body, specifically, placing the green body in a kiln and keeping it at 700-1000° C. for 1-6 hours. The heat treatment temperature is, for example, 700° C., 800° C., 900° C. or 1000° C., and the holding time is, for example, 1 hour, 3 hours, 5 hours or 6 hours.

[0044] The building material of the present invention uses medical waste slag as the main raw material and is prepared by the method for treating medical waste slag of the present invention. It has high strength: the compressive strength is as high as 40MPa, which is higher than the general building materials on the market, and it also has good water resistance and acid and alkali resistance.

[0045] The present application is described in detail below through some specific embodiments.

[0046] Example 1

[0047] Step 1, pretreatment: put 1000g of medical waste slag into a blast dryer and dry it at 200℃ for 3h; put the dried slag into a ball mill for crushing, the crushing time is 6h, the grinding balls used are alumina grinding balls, the ball diameter is 8cm, and the ball-to-material mass ratio is 2:1; use a 60-mesh sieve to screen the crushed slag, collect the remaining part, re-ball mill and screen it to obtain slag powder;

[0048] Step 2, granulation: granulating the screened slag powder to obtain granulated powder; wherein the granulation binder is a PVA aqueous solution with a concentration of 3wt%, and the amount of the granulation binder is 3wt% of the mass of the slag powder;

[0049] Step 3, mixing: the granulated powder, the inorganic fiber and the sintering aid are mixed in a three-dimensional mixer for 6 hours. The inorganic fiber used in this embodiment is glass fiber, and the mass of the glass fiber is 10wt% of the mass of the slag; the sintering aid is sodium silicate, and the mass of the sodium silicate is 5wt% of the mass of the slag;

[0050] Step 4: Pressing: placing the mixed powder in a pressing mold for pressing to obtain a green body. In this embodiment, the pressure during pressing is 5 MPa and the holding time is 30 seconds.

[0051] Step 5: Place the pressed green body in a kiln for heat treatment at a final firing temperature of 1000°C and a holding time of 2 hours. After the heat treatment is completed, high-performance building materials are obtained after cooling.

[0052] Example 2

[0053] Step 1, pretreatment: put 1000g of medical waste slag into a blast dryer and dry it at 100℃ for 6h; put the dried slag into a ball mill for crushing, the crushing time is 12h, the grinding balls used are a mixture of stainless steel grinding balls and alumina grinding balls, the ball diameter is 20cm, and the ball-to-material mass ratio is 1:1; use an 80-mesh sieve to screen the crushed slag, collect the remaining part, re-ball mill and screen it to obtain slag powder;

[0054] Step 2, granulation: granulating the screened slag powder to obtain granulated powder; wherein the granulation binder is a PVA aqueous solution with a concentration of 10wt%, and the amount of the granulation binder is 10wt% of the mass of the slag powder;

[0055] Step 3, mixing: the granulated powder, the inorganic fiber and the sintering aid are mixed in a three-dimensional mixer for 4 hours. The inorganic fiber used in this embodiment is alumina fiber, and the mass of the alumina fiber is 40wt% of the mass of the slag; the sintering aid is glass powder, and the mass of the glass powder is 12wt% of the mass of the slag;

[0056] Step 4: Pressing: placing the mixed powder in a pressing mold for pressing to obtain a green body. In this embodiment, the pressure during pressing is 10 MPa and the holding time is 10 seconds.

[0057] Step 5: Place the pressed green body in a kiln for heat treatment at a final firing temperature of 700°C and a holding time of 6 hours. After the heat treatment is completed, high-performance building materials are obtained after cooling.

[0058] Example 3

[0059] Step 1, pretreatment: put 1000g of medical waste slag into a blast dryer and dry it at 150℃ for 4h; put the dried slag into a ball mill for crushing, the crushing time is 9h, the grinding balls used are zirconium oxide grinding balls, the ball diameter is 15cm, and the ball-to-material mass ratio is 1.5:1; use a 40-mesh sieve to screen the crushed slag, collect the remaining part, re-ball mill and screen it to obtain slag powder;

[0060] Step 2, granulation: granulating the screened slag powder to obtain granulated powder; wherein the granulation binder is a PVA aqueous solution with a concentration of 15wt% and an amount of the granulation binder of 7wt% of the mass of the slag powder;

[0061] Step 3, mixing: the granulated powder, the inorganic fiber and the sintering aid are mixed in a three-dimensional mixer for 6 hours. The inorganic fiber used in this embodiment is a combination of glass fiber and mullite fiber, and the total mass of the two fibers is 60wt% of the mass of the slag; the sintering aid is sodium silicate, and the mass of the sodium silicate is 20wt% of the mass of the slag;

[0062] Step 4: Pressing: placing the mixed powder in a pressing mold for pressing to obtain a green body. In this embodiment, the pressure during pressing is 8 MPa and the holding time is 20 seconds.

[0063] Step 5: Place the pressed green body in a kiln for heat treatment at a final firing temperature of 900°C and a holding time of 4 hours. After the heat treatment is completed, high-performance building materials are obtained after cooling.

[0064] The present invention prepares building materials by pre-treating medical waste slag, granulating, mixing with inorganic fiber and sintering aid, pressing and heat treating, and the prepared building materials have high strength and good water resistance, acid and alkali resistance. The method for treating medical waste slag of the present invention effectively turns medical waste slag into treasure, which not only solves the environmental pollution problem caused by medical waste slag, but also provides a direction for the diversified treatment of solid waste. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.

[0065] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for treating medical waste slag, characterized in that: include: Pre-treating medical waste slag to obtain slag powder; granulating the slag powder to obtain granulated powder; The granulated powder is uniformly mixed with inorganic fibers and a sintering aid to obtain a mixed powder; Pressing the mixed powder into a shape to obtain a green compact; Heat treating the green body and cooling it to obtain a building material; The mass of the inorganic fiber is 10wt% to 60wt% of the mass of the slag powder, and the mass of the sintering aid is 5wt% to 20wt% of the mass of the slag powder; the inorganic fiber includes one or more of glass fiber, alumina fiber, and mullite fiber; Pretreatment of medical waste slag includes: The medical waste slag is placed in a drying oven and dried at 100-200° C. for 2-6 h; The dried medical waste slag is placed in a ball mill for crushing, wherein the crushing time is 6 to 12 hours; The crushed medical waste slag is sieved with a 40-80 mesh sieve to obtain medical waste slag powder with uniform particle size; The green body is heat treated, comprising: placing the green body in a kiln, keeping the temperature at 700-1000° C. for 1-6 hours.

2. The method for treating medical waste slag according to claim 1, characterized in that: The medical waste slag contains SiO2 30-40wt%; Al2O 35-15wt%; CaO 20-30wt%; Fe2O 35-15wt%; and Na2O 0-5wt%.

3. The method for treating medical waste slag according to claim 1, characterized in that: The grinding balls of the ball mill are one or more of alumina, zirconia, and stainless steel grinding balls. The diameter of the grinding balls is 3 cm to 20 cm, and the ball-to-material mass ratio is (1 to 2):

1.

4. The method for treating medical waste slag according to claim 1, characterized in that: In the step of granulating the slag powder, the amount of the granulation binder used is 0.5wt%~10wt% of the mass of the slag powder, and the granulation binder is a polyvinyl alcohol aqueous solution, and the concentration of the polyvinyl alcohol aqueous solution is 3wt%~15wt%.

5. The method for treating medical waste slag according to claim 1, characterized in that: The granulated powder is mixed evenly with the inorganic fiber and the sintering aid, comprising placing the granulated powder in a mixer, adding the inorganic fiber and the sintering aid, and mixing in the mixer for 2 to 6 hours to obtain a uniformly mixed powder.

6. The method for treating medical waste slag according to claim 5, characterized in that: The sintering aid includes one or both of glass powder and sodium silicate.

7. The method for treating medical waste slag according to claim 1, characterized in that: The mixed powder is pressed into shape, comprising: placing the mixed powder in a pressing mold and pressing into shape, wherein the pressure during pressing and molding is 3-10 MPa, and the holding time is 10-30 seconds.

8. A building material, characterized in that: The medical waste slag is used as raw material and is prepared by the medical waste slag treatment method described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of rich-pore high-water-absorption ceramsite based on sludge